High-efficiency rust removal process for strip steel edge

By adding an edge treatment device to the stainless steel strip production line, independent and continuous processing of the strip edge is achieved, solving the problems of black edge phenomenon and insufficient oxide scale removal rate in the existing technology, improving product quality and pass rate, and applicable to edge treatment of 200 series, 300 series and 400 series stainless steel strips.

CN123149200APending Publication Date: 2026-11-24GUANGDONG GUANGQING METAL ROLLING CO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611422122.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing stainless steel strip production lines cannot effectively handle the left and right edges of the strip, resulting in black edges on the finished steel coils. The oxide scale removal rate on the edges is insufficient, making them prone to rust and cracking. Furthermore, the product qualification rate is low, failing to meet the appearance and performance requirements of high-end products.

Method used

Edge treatment devices are added to key processes such as shot blasting, brushing, pickling and cleaning. These devices include side shot blasters, re-brushing equipment, side spray pickling and high-pressure water washing, etc., to achieve independent and continuous treatment of the strip steel edges. Through the synergistic effect of multiple processes, oxide scale and impurities are removed, ensuring that the edge treatment effect is consistent with that of the upper and lower surfaces.

Benefits of technology

It achieves full-process coverage treatment of the steel strip edges, with an oxide scale removal rate of over 99%, eliminating black edge defects, improving the product's appearance quality and corrosion resistance, reducing labor costs and operational difficulty, and meeting the quality requirements of high-end products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149200A_ABST
    Figure CN123149200A_ABST
Patent Text Reader

Abstract

This invention discloses a high-efficiency strip steel edge rust removal process, relating to the field of metallurgical technology. The high-efficiency strip steel edge rust removal process includes the following steps: first, shot blasting the left and right edges of the strip steel using a side shot blaster; then, rotating and brushing the strip steel edges using a brush roller; next, spraying pickling solution onto the strip steel edges using a side spray nozzle; then, removing pickling residue using a brush roller; finally, spraying high-pressure cleaning water onto the strip steel edges using a high-pressure nozzle; and finally, drying. This invention, by adding an edge treatment device to the shot blasting, brushing, pickling, and cleaning processes, achieves full-process coverage treatment of the strip steel edges, improving the edge oxide scale removal rate and product qualification rate, and eliminating black edge defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallurgical technology, specifically to a high-efficiency rust removal process for the edges of steel strips. Background Technology

[0002] Stainless steel strip is widely used in construction decoration, chemical equipment, food machinery, automobile manufacturing and other fields due to its excellent corrosion resistance and good processing performance. In the production process of stainless steel strip, hot annealing and pickling are key processes. Their purpose is to remove the oxide scale formed on the surface of the strip during hot rolling and annealing, and to form a dense passivation film on the surface of the strip, thereby improving the surface quality and corrosion resistance of the strip.

[0003] Currently, stainless steel strip production lines generally employ conventional processes such as descaling, shot blasting for rust removal, and brushing, pickling, and passivation. Existing shot blasting, brushing, pickling, and cleaning equipment can only treat the top and bottom surfaces of the strip, failing to effectively treat the left and right edges. This results in 100% black edges on the finished steel coils, insufficient removal of oxide scale, and susceptibility to rust and cracking during subsequent processing. This necessitates additional manual grinding, leading to a low product qualification rate, increased labor costs, and compromised edge precision after grinding, failing to meet the appearance and performance requirements of high-end stainless steel products.

[0004] To address the shortcomings of the existing technology, this invention provides a highly efficient strip steel edge rust removal process. By adding an edge treatment device to key processes such as shot blasting, brushing, pickling, and cleaning, the process enables independent and continuous treatment of the strip steel edges, ensuring consistent edge treatment with the upper and lower surfaces, eliminating black edge phenomena, and improving overall product quality. Summary of the Invention

[0005] The purpose of this invention is to provide an efficient rust removal process for the edges of steel strips to solve the problems mentioned in the background art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a high-efficiency strip edge rust removal process, comprising the following steps: S1: Edge shot blasting, which involves shot blasting the left and right edges of the strip to remove the oxide scale from the surface of the edges. S2: Edge re-brushing: The edges of the strip steel treated in step S1 are re-brushed before pickling to remove residual rust, oil, and shot blasting residue. S3: Side pickling: The edge of the strip steel after step S2 is pickled to dissolve the residual oxide scale on the edge. S4: Secondary brushing of the edge: The edge of the strip steel after the treatment in step S3 is pickled and then brushed again to remove the residue generated during the pickling process. S5: High-pressure water washing of the edge: The edge of the strip steel after the treatment in step S4 is subjected to high-pressure water washing to wash away the residual acid and salt on the edge. S6: The strip steel processed in step S5 is dried to obtain finished strip steel without black edge defects.

[0007] Preferably, the shot blasting parameters of the side shot blasting device in the edge shot blasting treatment include: a shot blasting angle of 45° to 60° with the side edge of the strip, a shot blasting speed of 70m / s to 120m / s, and a shot blasting rate of 80kg / h to 120kg / h per group; the side shot blasting device is provided in two groups, symmetrically arranged on the left and right sides of the strip, with the shot blasting center of each group of side shot blasting devices aligned with the center line of the corresponding side edge of the strip, and the distance between the side shot blasting device and the edge of the strip is 150mm to 200mm; the side shot blasting device uses high-chromium cast steel shot as the shot blasting medium, the diameter of the high-chromium cast steel shot is 0.8mm to 1.2mm, and the hardness is HRC58 to HRC62.

[0008] Preferably, the brush roller used in the pre-pickling edge re-brushing treatment is a wear-resistant abrasive brush, the brush bristles of the brush roller are made of silicon carbide, and the bristles are arranged in bundles of 3, with each bundle having a diameter of 0.8 mm; the brush roller used in the post-pickling edge re-brushing treatment is an abrasive brush, the brush roller is made of diamond, and the bristles are arranged in bundles of 1, with each bundle having a diameter of 1.8 mm.

[0009] Preferably, in both the pre-pickling edge re-brushing treatment and the post-pickling edge secondary re-brushing treatment, a lateral drive mechanism is used to drive the brush roller to move along the width direction of the strip, so that the brush roller automatically aligns with and fits against the left and right edges of the strip; the lateral drive mechanism includes a servo motor and a ball screw driven by the servo motor, the brush roller is mounted on a sliding base, the sliding base is fixedly connected to the nut seat of the ball screw, the bottom of the sliding base is provided with a linear guide rail, and the servo motor drives the sliding base to reciprocate along the linear guide rail through the ball screw; the lateral drive mechanism also includes a proximity switch for detecting the lateral position of the sliding base.

[0010] Preferably, in the edge pickling process, the side spray nozzles are arranged on both sides of the squeeze roller in the pickling tank, with two fan-shaped side spray nozzles on each side; the side spray nozzles are installed on the tank wall of the pickling tank through a flange connection structure, the flange connection structure including: a PPH flange short pipe fixed to the tank wall, the side spray nozzles are inserted into the PPH flange short pipe and connected by a flange, and a PTFE gasket is provided between the connecting surfaces of the flange; a one-way valve for preventing acid backflow is provided behind the side spray nozzles.

[0011] Preferably, in the edge pickling treatment, the spraying parameters of the side spray nozzle include: a spraying pressure of 0.4 MPa to 0.6 MPa, and an acid temperature of 30°C to 45°C; the pickling solution is a mixed aqueous solution of nitric acid and hydrofluoric acid, wherein, for 200 series stainless steel, the mass concentration of nitric acid is 8% to 10%, and the mass concentration of hydrofluoric acid is 1.5% to 2.0%; for 300 series stainless steel, the mass concentration of nitric acid is 10% to 12%, and the mass concentration of hydrofluoric acid is 2.0% to 2.5%; for 400 series stainless steel, the mass concentration of nitric acid is 12% to 15%, and the mass concentration of hydrofluoric acid is 2.5% to 3.0%.

[0012] Preferably, in the edge high-pressure water washing treatment, the high-pressure nozzles are located on both sides of the strip steel in the final cleaning tank, with two sets of columnar high-pressure nozzles on each side. The distance between the high-pressure nozzles and the edge of the strip steel is 100mm to 150mm. The high-pressure cleaning water is deionized water with a conductivity ≤10μS / cm, a rinsing pressure of 5MPa to 20MPa, and a water temperature of 40℃ to 50℃. The water temperature is obtained by heating the waste heat of the drying box through a heat exchanger. The heat exchanger is installed in the exhaust pipe section at the top of the drying box, and the heat source medium of the heat exchanger is the hot flue gas discharged from the drying box. The heated medium of the heat exchanger is the high-pressure cleaning water.

[0013] Preferably, the method further includes a process parameter linkage control step: acquiring the running speed signal and thickness signal of the strip; calculating and outputting the process parameter setting values ​​of each edge processing unit according to the running speed of the strip and a preset mapping function, wherein the process parameters include side shot blasting amount, side spray pickling pressure, high-pressure flushing pressure and brush roller speed; compensating and correcting the process parameter setting values ​​according to the thickness and / or steel grade of the strip to obtain the final process parameter control value; and outputting the final process parameter control value to the corresponding actuator to control the operation of each edge processing unit.

[0014] Preferably, the mapping function is: The side shot blasting rate Q = 2.4 × V + 30, where Q is in kg / min and V is the strip running speed in m / min; The side-spray pickling pressure P1 = 0.008 × V + 0.1, where the unit of P1 is MPa; The high-pressure flushing pressure P2 = 0.16 × V + 2.0, where the unit of P2 is MPa; The brush roller rotation speed N = 5 × V + 100, where N is in r / min; In the compensation correction step, the correction is performed according to the following compensation coefficient: Steel grade compensation coefficient K sThe value is 0.90 for the 200 series, 1.00 for the 300 series, and 1.15 for the 400 series. Thickness compensation coefficient K t The rate is 0.85 for strip thicknesses of 0.3mm to 1.0mm, 1.00 for 1.0mm to 3.0mm, 1.20 for 3.0mm to 8.0mm, and 1.40 for 8.0mm to 16.0mm. The final process parameter control value = basic mapping value × K s ×K t .

[0015] Preferably, the strip is a 200 series, 300 series, or 400 series stainless steel strip, the thickness of the strip is 0.3 mm to 16.0 mm, and the width is 800 mm to 2500 mm; the process enables the oxide scale removal rate of the strip edge to be ≥99%, the edge surface roughness Ra≤1.8 μm, and the edge color to be consistent with the upper and lower surfaces as silver-white, without black edge defects.

[0016] The technical effects and advantages of this invention are as follows: 1. This efficient strip steel edge rust removal process achieves independent and continuous treatment of the strip steel edges. By adding targeted edge treatment devices in key processes such as shot blasting, brushing, pickling, and cleaning, it achieves full-process coverage treatment of the strip steel edges from shot blasting to final cleaning, resulting in uniform and consistent treatment effects on the edges and the upper and lower surfaces.

[0017] 2. This high-efficiency strip edge rust removal process effectively eliminates the black edge phenomenon. Through the efficient shot blasting and peeling by the side shot blasting machine, the cleaning and opening of the re-brushing equipment, the full dissolution by the side spray pickling, the removal of residue by the secondary re-brushing equipment, and the thorough rinsing by high-pressure water washing, the five processes work together to achieve an edge oxide scale removal rate of over 99%, which can eliminate black edge defects and significantly improve the appearance quality and corrosion resistance of the product.

[0018] 3. This highly efficient strip edge rust removal process is highly integrated. All edge treatment devices are added to or modified from existing production lines, without affecting the rhythm and efficiency of the original production lines. It does not require large-scale reconstruction of existing production lines and is easy to implement and promote.

[0019] 4. This efficient strip edge rust removal process boasts low modification costs and significant benefits. The side shot blasting machine, side spray nozzles, and brush rollers are all localized improvements or additions to existing equipment, keeping modification costs under control. After processing with this invention, the product qualification rate is significantly improved, eliminating the need for subsequent manual grinding and avoiding damage to edge precision caused by grinding, thus meeting the quality requirements of high-end stainless steel products.

[0020] 5. This efficient strip edge rust removal process achieves automatic matching of process parameters with strip speed, thickness, and steel type through a PLC linkage control system, ensuring stable processing results throughout the entire process, avoiding quality fluctuations caused by local parameter mismatches, and reducing operational difficulty and reliance on manual experience. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 This is a process flow diagram of the present invention; Figure 2 This is a structural block diagram of the edge shot blasting system of the present invention; Figure 3 This is a structural block diagram of the edge repainting device of the present invention; Figure 4 This is a structural block diagram of the acid spraying system on the side of the pickling tank according to the present invention; Figure 5 This is a structural block diagram of the pickling tank re-brushing equipment of the present invention; Figure 6 This is a structural block diagram of the final cleaning tank edge high-pressure rinsing system of the present invention; Figure 7 This is a block diagram of the PLC linkage control system of the present invention; Figure 8 This is a table of stainless steel edge treatment parameters for the present invention; Figure 9 This is a table showing the acid solution ratio and reaction time of this invention. Detailed Implementation

[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] This invention discloses an efficient rust removal process for the edges of steel strips, according to the attached... Figures 1 to 9 As shown, the process includes the following steps: S1: edge shot blasting, S2: edge re-brushing, S3: edge side spray pickling, S4: edge secondary re-brushing, S5: edge high-pressure water washing, and S6: drying treatment.

[0025] Further, S1: Edge shot blasting, which involves shot blasting the left and right edges of the strip to remove the oxide scale from the surface of the edges. Specifically, at least one set of side shot blasters is added to each of the left and right sides of the strip inside the shot blasting machine. The shot blasting direction of the side shot blasters is aimed at the edge of the strip, and the shot blasting medium is propelled at high speed onto the edge of the strip through the side shot blasters, causing the oxide scale on the edge to be impacted and peeled off. The shot blasting parameters of the side shot blasters in the edge shot blasting process include: a shot angle of 45° to 60° with the side of the strip, a shot velocity of 70m / s to 120m / s, and a shot blasting rate of 80kg / h to 120kg / h per set. There are two sets of side shot blasters, symmetrically arranged on the left and right sides of the strip. The shot center of each set of side shot blasters is aligned with the center line of the corresponding side edge of the strip, and the distance between the side shot blasters and the edge of the strip is 150mm to 200mm. The side shot blasting machine uses high-chromium cast steel shot as the blasting medium. The high-chromium cast steel shot has a diameter of 0.8 mm to 1.2 mm and a hardness of HRC58 to HRC62. The blasting speed of the side shot blasting machine is 5 m / s to 10 m / s higher than that of the upper and lower shot blasting machines to meet the requirements for removing dense oxide scale on the edges.

[0026] Further, S2: Edge re-brushing. The edges of the strip steel treated in step S1 are re-brushed before pickling to remove residual rust, oil, and shot blasting residue. Specifically, a set of brush rollers symmetrically arranged on the left and right sides of the strip steel are installed before the pickling tank inlet. The brush rollers are driven to rotate and adhere to the left and right edges of the strip steel, and the edges are rotated and brushed to mechanically remove residual rust, oil, and shot blasting residue, resulting in a clean edge surface. The brush rollers are wear-resistant abrasive brushes with silicon carbide bristles, in bundles of three bristles each, with a bristle diameter of 0.8 mm and a bristle density of 500 to 800 bristles / cm². A pressure regulating device is provided, with a contact pressure of 0.2 MPa to 0.3 MPa and a brush roller rotation speed of 300 to 800 r / min. The cleanliness level can reach Sa2.5, ensuring sufficient contact between the acid and the substrate.

[0027] The brush roller is equipped with a lateral drive mechanism for moving the brush roller along the width direction of the strip steel, so that the brush roller automatically aligns with and conforms to the left and right edges of the strip steel. The lateral drive mechanism includes a servo motor and a ball screw driven by the servo motor. The brush roller is mounted on a sliding base, and the sliding base is fixedly connected to the nut seat of the ball screw. A linear guide rail is provided at the bottom of the sliding base. The servo motor drives the sliding base to reciprocate along the linear guide rail through the ball screw. The lateral drive mechanism also includes a proximity switch for detecting the lateral position of the sliding base.

[0028] Further, S3: Edge pickling, the edges of the strip treated in step S2 are pickled to dissolve the residual oxide scale. Specifically, at least one side spray nozzle is installed on each of the left and right sides of the strip in the pickling tank. The spray direction of the side spray nozzles is aimed at the edge of the strip, and pickling liquid is sprayed onto the edge through the side spray nozzles, so that the pickling liquid adheres to the edge surface and reacts chemically with the oxide scale, dissolving and removing the oxide scale. The side spray nozzles are located on both sides of the squeeze roller in the pickling tank. At this position, the strip will not fluctuate, ensuring that the acid is accurately sprayed onto the edge of the strip. There are two fan-shaped side spray nozzles on each side. The nozzle distance from the strip edge is 80mm to 120mm, the spray angle is 60° to 90°, the side spray pressure is 0.4MPa to 0.6MPa, which is 0.2MPa to 0.3MPa higher than the main tank spray pressure, and the acid temperature is 30° to 45°, which is synchronously controlled with the main tank temperature. Under these parameters, the thickness of the acid film at the edge can reach 50μm to 80μm, the reaction time is extended to 15s to 20s, and the oxide scale is fully dissolved.

[0029] The pickling solution is a mixed aqueous solution of nitric acid and hydrofluoric acid. For 200 series stainless steel, the mass concentration of nitric acid is 8% to 10%, the mass concentration of hydrofluoric acid is 1.5% to 2.0%, and the reaction time is 15 to 18 seconds; for 300 series stainless steel, the mass concentration of nitric acid is 10% to 12%, the mass concentration of hydrofluoric acid is 2.0% to 2.5%, and the reaction time is 18 to 22 seconds; for 400 series stainless steel, the mass concentration of nitric acid is 12% to 15%, the mass concentration of hydrofluoric acid is 2.5% to 3.0%, and the reaction time is 20 to 25 seconds. 0.3% to 0.5% of Lan-826 corrosion inhibitor may also be added to the pickling solution to inhibit excessive corrosion of the substrate by the acid.

[0030] The side spray nozzle is mounted on the wall of the pickling tank via a flange connection structure. The flange connection structure includes a PPH flange short pipe fixed to the tank wall. The side spray nozzle is inserted into the PPH flange short pipe and connected via a flange. A PTFE gasket is provided between the connecting surfaces of the flange to ensure a leak-proof seal. A one-way valve for preventing acid backflow is located behind the side spray nozzle. The one-way valve is made of a clamp-on PPH material.

[0031] Further, S4: Secondary brushing of the edges. After the S3 step, the edges of the strip are pickled and then brushed again to remove residue generated during the pickling process. Specifically, a set of brush rollers symmetrically arranged on the left and right sides of the strip are placed between the main spray zone and the squeeze rollers in the pickling tank. The brush rollers are driven to rotate and adhere to the left and right edges of the strip, rotating and brushing the edges to mechanically remove the metal oxide residue generated after pickling. The brush rollers are abrasive brushes with diamond bristles, one bristle per bundle, each bundle having a diameter of 1.8 mm. The brush roller speed is 200 r / min to 800 r / min, and the contact pressure is 0.1 MPa to 0.2 MPa, half the contact pressure of the primary brushing. The hardness of the secondary brush bristles is HRC25 to HRC30, lower than that of the primary brush bristles, to avoid scratching the edges. The service life of the secondary brushing is 2 months.

[0032] The secondary brush roller also has a lateral drive mechanism for driving the brush roller to move along the width direction of the strip, so that the brush roller automatically aligns with and fits against the left and right edges of the strip. Its specific structure is the same as the lateral drive mechanism described in step S2.

[0033] Specifically disclosed is S5: High-pressure water washing of the edge. This involves high-pressure water washing of the strip edge after step S4 to remove residual acid and salt. Specifically, at least one high-pressure nozzle is installed on each of the left and right sides of the strip within the final cleaning tank. The nozzles are aimed at the edge of the strip, spraying high-pressure cleaning water onto the edge. The impact force of the high-pressure water flow washes away residual acid and salt adhering to the edge surface. The high-pressure nozzles are located on both sides of the strip within the final cleaning tank, with two sets of columnar high-pressure nozzles on each side. The distance between the high-pressure nozzles and the edge of the strip is 100mm to 150mm. The high-pressure cleaning water is deionized water with a conductivity ≤10μS / cm, a rinsing pressure of 5MPa to 20MPa, and a water temperature of 40℃ to 50℃. Under these parameters, the pH value of the edge can be stabilized at 6.5 to 7.5, with no acid or salt residue remaining.

[0034] The water temperature is obtained by heating the waste heat from the drying chamber via a heat exchanger, thus saving energy and reducing consumption. The heat exchanger is installed in the exhaust duct section at the top of the drying chamber. The heat source medium for the heat exchanger is the hot flue gas emitted from the drying chamber, and the heated medium is the high-pressure cleaning water. The heat exchanger is a plate heat exchanger, model BR-0.5, made of 316L stainless steel plates and nitrile rubber gaskets, with a design pressure of 20.0 MPa and a heat exchange area of ​​3.5 m². It is connected to the flue via a flange. The high-pressure flushing system uses a variable displacement plunger pump with a power of 22 kW, 4 stages, 1450 rpm, a flow rate of 70 L / min, a pressure of 20 MPa, and frequency conversion control. An 80-mesh basket filter is installed at the inlet to prevent brushing residue from entering the heat exchanger and clogging the plate gaps. The system is also equipped with an electric regulating valve, which is a proportional integral valve DN50. It receives a 4-20mA signal from the PLC and automatically adjusts the opening based on the water temperature of the cleaning tank PT100 to control the hot water return flow and maintain a water temperature of 45±2℃.

[0035] Specifically disclosed is S6: Drying treatment, which involves drying the strip steel after step S5. Specifically, the strip steel that has been washed with high pressure is sent into a drying oven and dried at a temperature of 120°C to 150°C for 30 to 60 seconds to obtain a finished strip steel with no black edge defects.

[0036] Furthermore, the process described in this invention also includes a process parameter linkage control step: acquiring the running speed signal and thickness signal of the strip steel. Specifically, the strip speed signal is acquired using an incremental encoder with a resolution of 1024P / R, installed between the uncoiler and the straightener; the strip thickness signal is acquired using a laser thickness gauge with an accuracy of ±1μm, installed at the inlet of the descaling machine; the steel grade selection signal is manually input via an HMI touchscreen or issued by the MES system; the temperature signal is acquired via the pickling tank PT100, the cleaning tank PT100, and the drying oven PT100; and the pressure signal is acquired via a side-spray acid pressure transmitter, a high-pressure flushing pressure transmitter, and a squeeze roll air pressure sensor.

[0037] Specifically disclosed, based on the running speed of the strip steel, the process parameter settings of each edge processing unit are calculated and output according to a preset mapping function. The process parameters include the side shot blasting amount, the side spray pickling pressure, the high-pressure flushing pressure, and the brush roller speed.

[0038] The mapping function is: The side shot blasting rate Q = 2.4 × V + 30, where Q is in kg / min and V is the strip running speed in m / min; The speed range of 30-50 m / min corresponds to 120 kg / min, the speed range of 50-80 m / min corresponds to 180 kg / min, and the speed range of 80-100 m / min corresponds to 240 kg / min.

[0039] The side-spray pickling pressure P1 = 0.008 × V + 0.1, where the unit of P1 is MPa; The corresponding pressure is 0.35 MPa in the low-speed range, 0.5 MPa in the medium-speed range, and 0.65 MPa in the high-speed range.

[0040] The high-pressure flushing pressure P2 = 0.16 × V + 2.0, where the unit of P2 is MPa; The low-speed range corresponds to 6 MPa, the medium-speed range corresponds to 10 MPa, and the high-speed range corresponds to 14 MPa.

[0041] The brush roller rotation speed N = 5 × V + 100, where N is in r / min; The low-speed range corresponds to 300 r / min, the medium-speed range corresponds to 400 r / min, and the high-speed range corresponds to 500 r / min.

[0042] It is particularly important to emphasize that the process parameter setpoints are compensated and corrected based on the strip thickness and / or steel grade to obtain the final process parameter control values. The compensation and correction coefficients are as follows: Steel grade compensation coefficient K s The value is 0.90 for the 200 series, 1.00 for the 300 series, and 1.15 for the 400 series.

[0043] Thickness compensation coefficient K t The value is 0.85 for strip thickness of 0.3mm to 1.0mm, as thin plates are prone to deformation and their strength is reduced; 1.00 for 1.0mm to 3.0mm, which is the baseline value; 1.20 for 3.0mm to 8.0mm, as the oxide scale thickens and increases strength; and 1.40 for 8.0mm to 16.0mm, which is for extra-thick plates and requires strengthening treatment.

[0044] The final process parameter control value = basic mapping value × K s ×K t The PLC control system refreshes its calculations every 100ms to ensure that parameters transition smoothly and continuously with speed, without any abrupt changes.

[0045] It is particularly important to emphasize that the final process parameter control values ​​are output to the corresponding actuators to control the operation of each side processing unit. The actuators include: a side shot blasting machine frequency converter for adjusting the shot blasting motor speed and controlling the shot blasting volume; a side acid spray pump frequency converter for adjusting the acid spray pressure; a high-pressure rinsing pump frequency converter for adjusting the side rinsing water pressure; a heavy brush / secondary heavy brush servo driver for precisely controlling the brush roller speed; a squeeze roller proportional valve for adjusting the pressing pressure; a drying oven temperature control module for adjusting the electric heating power; and a heat exchanger electric regulating valve for adjusting the hot water flow rate.

[0046] It is particularly important to emphasize that the process described in this invention is applicable to the edge treatment of various stainless steel strips, including 200, 300, and 400 series, with strip thicknesses ranging from 0.3mm to 16.0mm and widths from 800mm to 2500mm. Strips treated by this process exhibit an edge oxide scale removal rate ≥99%, an edge surface roughness Ra ≤1.8μm, and an edge color consistent with the upper and lower surfaces (silver-white), with no black edge defects. The product qualification rate can be increased to over 98%.

[0047] Working principle: This invention, through a design concept of targeted processing and process coordination, breaks through the coverage blind zone of upper and lower shot blasting by optimizing the angle and speed of the side shot blaster during the shot blasting stage, thereby achieving the initial removal of the oxide scale on the edge. During the pretreatment stage, impurities on the edges are removed by a re-brushing device to avoid ineffective reactions where the acid cannot contact the substrate, thus paving the way for acid washing. During the pickling stage, the high-pressure design of the side spray nozzles increases the amount of acid adhering and the reaction time, ensuring that the oxide scale is fully dissolved; During the slag removal stage, the dissolved residue is removed by a secondary brushing device to prevent secondary pollution from affecting the passivation effect; During the cleaning stage, high-pressure edge rinsing combined with deionized water and residual heat heating is used to ensure that acid residue is completely removed and there are no black edges after drying; By using PLC linkage control to synchronize equipment parameters with strip speed, stable processing results are ensured throughout the entire process. This invention can be widely applied to the edge processing of 200, 300, and 400 series stainless steel strips with thicknesses ranging from 0.3mm to 16.0mm and widths from 800mm to 2500mm, and has good industrial application prospects and economic benefits.

[0048] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0049] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.

Claims

1. A high-efficiency strip steel edge rust removal process, characterized in that, Includes the following steps: S1: Edge shot blasting, which involves shot blasting the left and right edges of the strip to remove the oxide scale from the surface of the edges. S2: Edge re-brushing: The edges of the strip steel treated in step S1 are re-brushed before pickling to remove residual rust, oil, and shot blasting residue. S3: Side pickling: The edge of the strip steel after step S2 is pickled to dissolve the residual oxide scale on the edge. S4: Secondary brushing of the edge: The edge of the strip steel after the treatment in step S3 is pickled and then brushed again to remove the residue generated during the pickling process. S5: High-pressure water washing of the edge: The edge of the strip steel after the treatment in step S4 is subjected to high-pressure water washing to wash away the residual acid and salt on the edge. S6: Drying treatment. The strip steel after step S5 is dried to obtain finished strip steel without black edge defects.

2. The efficient strip edge rust removal process according to claim 1, characterized in that, The shot blasting parameters of the side shot blasting machine in the edge shot blasting treatment include: a shot angle of 45° to 60° with the side edge of the strip, a shot speed of 70m / s to 120m / s, and a shot blasting rate of 80kg / h to 120kg / h per group; there are two groups of side shot blasting machines, symmetrically arranged on the left and right sides of the strip, with the shot center of each group of side shot blasting machines aligned with the center line of the corresponding side edge of the strip, and the distance between the side shot blasting machine and the edge of the strip is 150mm to 200mm; the side shot blasting machine uses high-chromium cast steel shot as the shot blasting medium, with a diameter of 0.8mm to 1.2mm and a hardness of HRC58 to HRC62.

3. The efficient strip edge rust removal process according to claim 1, characterized in that, The brush roller used in the pre-pickling edge re-brushing treatment is a wear-resistant abrasive brush, the brush bristles of which are made of silicon carbide, and the bristles are arranged in bundles of 3, with each bundle having a diameter of 0.8 mm; the brush roller used in the post-pickling edge re-brushing treatment is an abrasive brush, the brush roller is made of diamond, and the bristles are arranged in bundles of 1, with each bundle having a diameter of 1.8 mm.

4. The efficient strip edge rust removal process according to claim 1, characterized in that, In both the pre-pickling edge re-brushing treatment and the post-pickling edge secondary re-brushing treatment, a lateral drive mechanism is used to drive the brush roller to move along the width direction of the strip steel, so that the brush roller automatically aligns with and fits against the left and right edges of the strip steel. The lateral drive mechanism includes a servo motor and a ball screw driven by the servo motor. The brush roller is mounted on a sliding base, and the sliding base is fixedly connected to the nut seat of the ball screw. A linear guide rail is provided at the bottom of the sliding base. The servo motor drives the sliding base to reciprocate along the linear guide rail through the ball screw. The lateral drive mechanism also includes a proximity switch for detecting the lateral position of the sliding base.

5. The efficient strip edge rust removal process according to claim 1, characterized in that, In the edge pickling process, the side spray nozzles are arranged on both sides of the squeezing roller in the pickling tank, with two fan-shaped side spray nozzles on each side; the side spray nozzles are installed on the tank wall of the pickling tank through a flange connection structure, the flange connection structure including: a PPH flange short pipe fixed to the tank wall, the side spray nozzles are inserted into the PPH flange short pipe and connected by a flange, and a PTFE gasket is provided between the connecting surfaces of the flange; a one-way valve for preventing acid backflow is provided behind the side spray nozzles.

6. The efficient strip edge rust removal process according to claim 1, characterized in that, In the edge pickling treatment, the spraying parameters of the side spray nozzles include: a spraying pressure of 0.4 MPa to 0.6 MPa and an acid temperature of 30°C to 45°C; the pickling solution is a mixed aqueous solution of nitric acid and hydrofluoric acid, wherein, for 200 series stainless steel, the mass concentration of nitric acid is 8% to 10% and the mass concentration of hydrofluoric acid is 1.5% to 2.0%; for 300 series stainless steel, the mass concentration of nitric acid is 10% to 12% and the mass concentration of hydrofluoric acid is 2.0% to 2.5%; and for 400 series stainless steel, the mass concentration of nitric acid is 12% to 15% and the mass concentration of hydrofluoric acid is 2.5% to 3.0%.

7. The efficient strip edge rust removal process according to claim 1, characterized in that, In the high-pressure water washing process, the high-pressure nozzles are located on both sides of the strip steel in the final cleaning tank, with two sets of columnar high-pressure nozzles on each side. The distance between the high-pressure nozzles and the edge of the strip steel is 100mm to 150mm. The high-pressure cleaning water is deionized water with a conductivity ≤10μS / cm, a rinsing pressure of 5MPa to 20MPa, and a water temperature of 40℃ to 50℃. The water temperature is obtained by heating the waste heat from the drying oven through a heat exchanger. The heat exchanger is installed in the exhaust pipe section at the top of the drying oven. The heat source medium of the heat exchanger is the hot flue gas discharged from the drying oven, and the heated medium of the heat exchanger is the high-pressure cleaning water.

8. The efficient strip edge rust removal process according to claim 1, characterized in that, It also includes a process parameter linkage control step: acquiring the running speed signal and thickness signal of the strip steel; calculating and outputting the process parameter setting values ​​of each edge processing unit according to the running speed of the strip steel and a preset mapping function, wherein the process parameters include side shot blasting amount, side spray pickling pressure, high-pressure flushing pressure and brush roller speed; and compensating and correcting the process parameter setting values ​​according to the thickness and / or steel grade of the strip steel to obtain the final process parameter control values. The final process parameter control values ​​are output to the corresponding actuators to control the operation of each side processing unit.

9. The efficient strip edge rust removal process according to claim 8, characterized in that, The mapping function is: The side shot blasting rate Q = 2.4 × V + 30, where Q is in kg / min and V is the strip running speed in m / min; The side-spray pickling pressure P1 = 0.008 × V + 0.1, where the unit of P1 is MPa; The high-pressure flushing pressure P2 = 0.16 × V + 2.0, where the unit of P2 is MPa; The brush roller rotation speed N = 5 × V + 100, where N is in r / min; In the compensation correction step, the correction is performed according to the following compensation coefficient: Steel grade compensation coefficient K s The value is 0.90 for the 200 series, 1.00 for the 300 series, and 1.15 for the 400 series. Thickness compensation coefficient K t The rate is 0.85 for strip thicknesses of 0.3mm to 1.0mm, 1.00 for 1.0mm to 3.0mm, 1.20 for 3.0mm to 8.0mm, and 1.40 for 8.0mm to 16.0mm. The final process parameter control value = basic mapping value × K s ×K t .

10. The efficient strip edge rust removal process according to claim 1, characterized in that, The strip is a 200 series, 300 series, or 400 series stainless steel strip, with a thickness of 0.3 mm to 16.0 mm and a width of 800 mm to 2500 mm. The process enables the removal rate of oxide scale on the edge of the strip to be ≥99%, the surface roughness Ra of the edge to be ≤1.8 μm, and the edge color to be consistent with the upper and lower surfaces as silver-white, without black edge defects.