A method for selecting iron from red mud
By combining microwave and ultrasonic pretreatment with hydrocyclone grading and differentiated magnetic separation, the problem of fine particle size and low degree of individual dissociation of iron minerals in red mud was solved, and the efficient recovery of iron minerals in red mud was achieved.
Patent Information
- Application Number
- CN202611383105.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-24
AI Technical Summary
In existing red mud magnetic separation processes, the iron minerals in red mud are finely embedded with low degree of individual dissociation, resulting in severe particle size interference and low recovery rate of fine-grained iron minerals.
Microwave and ultrasonic treatments were used to pretreat red mud, which was then combined with hydrocyclone grading and differentiated magnetic separation to enhance flocculation and perform cross-selection, thereby improving the degree of liberation and recovery rate of iron minerals.
Microwave pretreatment and ultrasonic treatment improved the individual dissociation degree of iron minerals in red mud, solved the particle size interference problem, improved the recovery rate of fine-grained iron minerals, and achieved efficient recovery of iron resources in red mud.
Smart Images

Figure CN123149229A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of mineral processing engineering technology, specifically to a method for iron beneficiation from red mud. Background Technology
[0002] Red mud is a highly alkaline solid waste generated during alumina production, producing approximately 1.0 to 2.0 tons of red mud for every ton of alumina produced. Red mud contains a large amount of iron, with a TFe content typically between 20% and 50%, making it highly valuable for recycling. Currently, the main method for recovering iron from red mud is magnetic separation, with a typical process including: slag screening, pre-selection using a cylindrical magnetic separator, high-intensity magnetic roughing, and high-intensity magnetic cleaning / sweeping.
[0003] However, existing red mud magnetic separation processes have the following technical shortcomings:
[0004] Firstly, the iron minerals in red mud are extremely fine-grained, with a large number of iron minerals closely coexisting with gangue minerals in the form of fine particles, resulting in low degree of individual liberation. Conventional ball milling cannot achieve effective liberation without excessive pulverization, leading to a large amount of iron minerals being difficult to capture during magnetic separation and being lost in the tailings.
[0005] Secondly, the magnetic separation behavior of iron minerals of different particle sizes in red mud varies significantly. Traditional processes treat the mixture of coarse and fine materials as a whole, resulting in severe particle size interference between different particle sizes. Coarse and fine particles restrict each other, making it difficult to optimize the separation index simultaneously.
[0006] Third, for fine-grained iron minerals, conventional high-gradient strong magnetic separation has extremely low collection efficiency, and a large amount of fine-grained iron minerals are lost with the tailings. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention provides a method for iron beneficiation from red mud, which solves the problems of fine-grained iron minerals in red mud, difficulty in monomer dissociation, severe particle size interference, and low recovery rate of fine-grained iron minerals.
[0008] To achieve the above objectives, the present invention provides the following technical solution:
[0009] A method for iron ore beneficiation from red mud includes the following steps:
[0010] S10. Pretreatment: The high-iron red mud sent from the bottom of the alumina production settling tank is subjected to microwave and ultrasonic treatment to obtain pretreated material.
[0011] S20. Impurity removal: The pretreated material is diluted with water and fed into a cylindrical screen for slag removal and impurity removal to obtain undersize material.
[0012] S30. Grading process: The screened material is fed into a hydrocyclone for grading, and is divided into three grades according to particle size: coarse slurry, medium slurry and fine slurry.
[0013] S40. Enhanced flocculation: Add dispersant to fine-grained slurry and stir, then add ultrafine magnetite powder and stir, and finally add selective flocculant and stir to obtain fine-grained flocculent slurry.
[0014] S50, Differentiated magnetic separation, feeds coarse-grained slurry, medium-grained slurry and fine-grained flocculent slurry into magnetic separators with corresponding magnetic field strength and corresponding separation structure for differentiated magnetic separation, and obtains coarse-grained tailings, coarse-grained concentrate, medium-grained concentrate and fine-grained concentrate;
[0015] S60, cross-selection: The coarse-grained tailings are fed into the fine-grained magnetic separator for cross-selection to obtain fine-grained concentrate mixed in with the coarse-grained tailings.
[0016] S70, Concentrate Dewatering: All coarse, medium, and fine-grained concentrates are combined, classified by a hydrocyclone, and the underflow is sent to a filter press for dewatering to obtain iron concentrate product. The overflow enters the medium-grade system.
[0017] Optionally, in step S10, pretreatment, the red mud is first fed into a microwave reactor and irradiated for 10 to 30 minutes at a microwave frequency of 2.45 GHz, a power of 1.0 to 1.4 kW, and a temperature of 500°C to 1000°C. After cooling, it is ball-milled into a slurry. Then, the slurry is fed into an ultrasonic treatment tank and ultrasonically treated for 2 to 10 minutes at a frequency of 20 to 50 kHz and a power density of 0.1 to 0.5 W / mL.
[0018] Optionally, in step S10, the pretreatment, the microwave irradiation treatment is carried out in a weakly reducing atmosphere, which is a nitrogen mixture with a CO volume fraction of 5% to 15%.
[0019] Optionally, in step S10, the pretreatment, the moisture content of the high-iron red mud is adjusted to 3.0%~5.0% before microwave irradiation, and a heat preservation and static treatment is performed between microwave irradiation and ultrasonic treatment.
[0020] Optionally, in step S30, the grading process, the coarse-grained slurry has a particle size greater than 0.15 mm, the medium-grained slurry has a particle size of 0.074–0.15 mm, and the fine-grained slurry has a particle size less than 0.074 mm.
[0021] Optionally, in step S40, enhanced flocculation, the dispersant is NSF or sodium hexametaphosphate, with a dosage of 50~200g / t, and the selective flocculant is a polyacrylamide type A flocculant, with a dosage of 10~50g / t.
[0022] Optionally, in step S40, enhanced flocculation, the particle size of the ultrafine magnetite powder is less than or equal to 5μm, and its addition amount is 1~6kg / t based on the solid mass in the slurry.
[0023] Optionally, in step S50, differentiated magnetic separation, coarse-grained slurry is separated using a high-gradient low-speed magnetic separator with a magnetic field strength of 1.2~1.8T, medium-grained slurry is separated using a conventional gradient medium-speed magnetic separator with a magnetic field strength of 0.8~1.2T, and fine-grained slurry is separated using a high-gradient high-speed magnetic separator or a flat-plate high-gradient magnetic separator with a magnetic field strength of 1.5~2.0T.
[0024] Optionally, in step S60, before the coarse-grained tailings are fed into the fine-grained magnetic separator for cross-selection, some of the coarse gangue is removed by a gravity separation device, and the gravity concentrate is then fed into the fine-grained magnetic separator for magnetic separation.
[0025] Optionally, it also includes:
[0026] S80, tailings disposal, combines the tailings from each magnetic separation section and sends them into the tailings settling tank, and the settling underflow is sent to the red mud filter press for disposal.
[0027] Compared with the prior art, the beneficial effects of the present invention are:
[0028] Microwave irradiation combined with a weakly reducing atmosphere in the pretreatment stage transforms some of the hematite in the red mud into magnetite. At the same time, microwave thermal stress and ultrasonic cavitation effects can significantly improve the degree of individual dissociation of iron minerals, thereby avoiding the problem of fine-grained iron minerals and difficult individual dissociation in red mud.
[0029] In the grading and magnetic separation stages, the slurry is divided into three grades based on two key particle size nodes: 0.15 mm and 0.074 mm. Each grade then undergoes differentiated separation in an optimized magnetic separation environment, thus avoiding particle size interference. Magnetic seed-enhanced flocculation causes fine-grained iron minerals to form strongly magnetic flocs, solving the problem of low recovery rates of fine-grained iron minerals in conventional magnetic separation. Cross-concentration further recovers fine-grained iron minerals entrained in the roughing tailings, achieving efficient recovery of valuable minerals. Attached Figure Description
[0030] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0031] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0032] In the following description, only certain exemplary embodiments are briefly described. As those skilled in the art will recognize, the described embodiments can be modified in various ways without departing from the spirit or scope of the invention. Therefore, the drawings and description are considered to be exemplary in nature and not restrictive.
[0033] The following disclosure provides many different embodiments or examples for implementing various structures of the invention. To simplify the disclosure, specific examples of components and arrangements are described below. These are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different examples; such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed. In addition, the various specific examples of processes and materials provided in this invention are examples of applications of other processes and / or the use of other materials that will be apparent to those skilled in the art.
[0034] The embodiments of the present invention / invention are described in detail below with reference to the accompanying drawings.
[0035] Example 1:
[0036] See Figure 1 This embodiment provides a method for iron ore beneficiation from red mud, which includes, in sequence, pretreatment, impurity removal, classification, enhanced flocculation, differentiated magnetic separation, cross-concentration, concentrate dewatering, and tailings disposal. Specifically:
[0037] S10, Pretreatment:
[0038] First, the moisture content of the high-speed iron red mud is adjusted to the range of 3.0% to 5.0%. Appropriate moisture helps the microwave energy to be evenly transferred inside the red mud particles, avoids excessive energy consumption in the water vaporization process due to excessive moisture, and also prevents excessive sintering between red mud particles when the moisture is too low.
[0039] The red mud was then continuously fed into a microwave reactor for irradiation treatment. The operating frequency of the microwave reactor was set to 2.45 GHz, which is the standard frequency for industrial microwave heating, achieving a good balance between penetration depth and heating efficiency. The microwave output power was between 1.0 and 1.4 kW, the internal temperature of the reactor was maintained in the range of 500℃ to 1000℃, and the irradiation treatment duration was 10 to 30 minutes.
[0040] It is worth noting that the microwave irradiation treatment is carried out in a weakly reducing atmosphere, which is a nitrogen mixture with a carbon monoxide volume fraction of 5% to 15%. Under microwave selective heating conditions, the iron minerals inside the red mud particles preferentially absorb microwave energy and heat up. Under the action of the weakly reducing atmosphere, some hematite is reduced to magnetite, thereby enhancing the magnetic response of the iron minerals. At the same time, due to the difference in dielectric constant, the iron minerals and gangue minerals (mainly aluminosilicate minerals) undergo differentiated thermal expansion in the microwave field, resulting in thermal stress microcracks at the interface between the two.
[0041] After microwave irradiation, the microwave-treated red mud sintered blocks were naturally cooled to room temperature and then fed into a ball mill for ball milling and pulping. The liquid-to-solid ratio during pulping was controlled at 200-500 mL / g. After ball milling and pulping, the resulting slurry was fed into an ultrasonic treatment tank for ultrasonic treatment. The ultrasonic treatment tank operated at a frequency of 20-50 kHz, a power density of 0.1-0.5 W / mL, and the ultrasonic treatment time was 2-10 min.
[0042] The cavitation effect generated when ultrasound propagates in the slurry can produce local high temperature and pressure and strong micro-jet impact, which further expands the microcracks and promotes the complete separation of the dissociated iron mineral particles from the gangue particles.
[0043] Microwave pretreatment and ultrasonic treatment can achieve the effects of thermal stress cracking and ultrasonic mechanical ablation, creating better selection conditions for subsequent magnetic separation.
[0044] In a preferred embodiment of step S10, after microwave irradiation treatment and before ball milling, a heat preservation and static setting stage is added, that is, holding at a temperature of 500℃~700℃ for 5~15 minutes, so that the microcracks formed during microwave irradiation have sufficient time to expand and extend, and at the same time, the reduction reaction between the weakly reducing atmosphere and the iron mineral is carried out more fully, thereby further improving the conversion rate of magnetite.
[0045] In step S10, thermal stress microcracks are formed at the interface between iron minerals and gangue by selective microwave heating. At the same time, a weakly reducing atmosphere is used to reduce some of the hematite to magnetite, which enhances the magnetic response of the red mud raw material. Subsequent ultrasonic treatment utilizes the cavitation effect to achieve efficient mineral liberation along the microcracks, resulting in a significant increase in the degree of liberation of iron minerals in the red mud compared to the untreated material. The iron grade of the magnetic separation concentrate can reach 57%~63%, providing high-quality feed material for subsequent magnetic separation.
[0046] S20, Impurity Removal:
[0047] After diluting the pretreated material obtained in step S10 with water to a suitable concentration, it is pumped into a cylindrical screen for slag and impurity removal. Under the rotation of the cylindrical screen, coarse particles larger than the screen openings (such as incompletely dissolved coarse diaspores in bauxite, metal fragments worn off by the crusher, and other large impurities mixed in the process) are trapped on the screen surface and move along the inner wall of the screen cylinder towards the discharge end, eventually being discharged into the ditch as oversize. Meanwhile, qualified slurry with particles smaller than the screen openings passes through the screen openings to become undersize material, which enters the next step.
[0048] In step S20, coarse impurities in the red mud slurry are effectively removed to avoid wear or blockage of subsequent precision equipment such as hydrocyclones and magnetic separators, thus ensuring the stable operation of the entire process.
[0049] S30, Graded processing:
[0050] The undersize slurry obtained in step S20 is introduced into a hydrocyclone assembly for classification. The hydrocyclone utilizes the principle of centrifugal sedimentation to separate the slurry into three grades: coarse, medium, and fine particles. The three grades of slurry are then fed into the next processing stage via their respective pipelines. The coarse and medium particles directly enter the differential magnetic separation process, while the fine particle slurry undergoes pretreatment via enhanced flocculation before magnetic separation.
[0051] In this step, precise particle size classification is achieved by connecting multiple hydrocyclones in series or parallel and controlling the feed pressure, underflow diameter, and overflow pipe insertion depth of each hydrocyclone. For example, coarse-grained slurry has a particle size greater than 0.15 mm. This grade of material is mainly composed of coarse intergrowths, with high density and fast settling velocity. Medium-grained slurry has a particle size of 0.074~0.15 mm. This grade of material has a high degree of liberation of individual particles and is the optimal feed size for conventional magnetic separation. Fine-grained slurry has a particle size less than 0.074 mm. This grade of material has a fine particle size, large specific surface area, and surface force dominates. Under conventional magnetic separation conditions, it is easily lost with water flow.
[0052] In this step, the red mud slurry is precisely classified according to particle size, allowing materials of different particle sizes to enter their respective optimal separation conditions, thereby solving the particle size interference problem between coarse and fine particles in traditional mixed magnetic separation. Coarse particles no longer cause blockage and entrainment interference in the magnetic separation process of fine particles, and fine particles can also be effectively recovered under specially optimized low flow rate and high gradient conditions.
[0053] S40, Enhanced Flocculation:
[0054] The fine-grained slurry obtained from step S30 is fed into a mixing tank for magnetic seed-enhanced flocculation treatment. Before the magnetic seed-enhanced flocculation treatment, the solid content of the fine-grained slurry is controlled within the range of 15% to 30% to ensure effective collision and contact between the flocculant and the mineral particles.
[0055] During operation, a dispersant is first added to the fine-grained slurry in the mixing tank. The dispersant can be either NSF or sodium hexametaphosphate, with a dosage of 50-200 g / t based on the solid mass of the slurry. After adding the dispersant, it is thoroughly dispersed for 5-10 minutes under stirring conditions, with the stirring speed controlled at 300-500 rpm. The dispersant works by adsorbing onto the surface of mineral particles, altering the charge distribution on the particle surface, and increasing the electrostatic repulsion or steric hindrance between particles. This allows the fine particles to achieve a uniform dispersion in the slurry, preventing reduced flocculation selectivity due to heterogeneous agglomeration.
[0056] After dispersion treatment, ultrafine magnetite powder is added to the mixing tank as a magnetic seed. The particle size of this ultrafine magnetite powder is no greater than 5μm, and its addition amount is 1~6kg / t based on the solid mass of the slurry. After adding the magnetic seed, stirring is continued for 3~5 minutes to ensure that the magnetic seed particles are fully contacted and mixed with the fine iron mineral particles. As a magnetic seed, the ultrafine magnetite powder can provide core magnetism to the fine iron mineral particles, allowing the originally weakly magnetic fine hematite particles to adhere to the surface of the magnetic seed or form agglomerates with the magnetic seed, thereby increasing the magnetization of the agglomerates.
[0057] After the magnetic seeds are added and stirred evenly, a selective flocculant is finally added to the mixing tank. The selective flocculant used is a polyacrylamide type A flocculant, with a dosage of 10-50 g / t based on the solid mass of the slurry. After adding the flocculant, the mixture is stirred continuously at a speed of 200-400 rpm for 5-15 minutes. During continuous stirring, the flocculant molecules adsorbed on the surface of the iron mineral particles connect multiple fine iron mineral particles and magnetic seed particles together, forming large, strongly magnetic flocs. The slurry containing these magnetic flocs is a fine-grained flocculent slurry.
[0058] In this step, the fine particles are uniformly dispersed by a dispersant, the flocs are given strong magnetism by a magnetic seed, and selective flocs are formed by a selective flocculant, thereby increasing the particle size of the fine iron minerals and improving the magnetic susceptibility of the flocs.
[0059] S50, Differentiated Magnetic Separation:
[0060] The coarse-grained slurry and medium-grained slurry obtained from the grading in step S30, and the fine-grained flocculent slurry obtained after the flocculation treatment in step S40, are respectively fed into magnetic separators with corresponding magnetic field strengths and corresponding separation structures for differentiated magnetic separation.
[0061] The coarse-grained slurry is separated using a high-gradient, low-speed magnetic separator. The separator's separation chamber contains rod-type or toothed plate media with a spacing of 3-8 mm to ensure smooth passage of coarse particles. The magnetic field strength is set to 1.2-1.8 T to ensure effective capture of coarse, weakly magnetic iron minerals. Low-speed operation allows sufficient residence time for coarse particles to contact the magnetic media within the separation zone, increasing the capture probability. During magnetic separation, the magnetic material captured by the magnetic media becomes the coarse-grained concentrate, while the uncaptured non-magnetic material is discharged as coarse-grained tailings.
[0062] Medium-grained slurry was separated using a conventional gradient medium-speed magnetic separator with a magnetic field strength set at 0.8~1.2T. This particle size exhibits high degree of monomer liberation and relatively uniform magnetic characteristics, allowing for good separation results using conventional magnetic separation parameters. The magnetic separation yielded medium-grained concentrate and medium-grained tailings.
[0063] Fine-grained flocculent slurry is separated using a high-gradient, high-speed magnetic separator or a flat-plate high-gradient magnetic separator, with the magnetic field strength set at 1.5~2.0T. The separating media in the fine-grained magnetic separator is fine steel wool or a mesh medium with a spacing of 0.5~2mm. The dense media gaps generate a high magnetic field gradient, producing a strong magnetic capture force on the fine-grained flocculent slurry. The high speed causes the separating media to frequently alternate entering and exiting the separating zone, which facilitates the timely unloading of captured magnetic flocs and avoids media blockage. After magnetic separation, fine-grained concentrate and fine-grained tailings are obtained.
[0064] In a preferred embodiment of step S50, the magnetic separation process for each particle size includes a roughing stage and a cleaning stage. Taking coarse particle magnetic separation as an example, the coarse particle slurry first enters a roughing magnetic separator for roughing, and the roughing concentrate then enters a cleaning magnetic separator for cleaning. The cleaned concentrate is output as the final coarse particle concentrate, and the cleaning tailings are returned to the roughing operation, thereby improving the concentrate grade and recovery rate.
[0065] S60, Cross-selection:
[0066] The coarse-grained tailings discharged from the coarse-grained magnetic separation in step S50 are transported through a pipeline to a fine-grained magnetic separator for cross-concentration. Although the coarse-grained tailings are mainly composed of non-magnetic coarse gangue, they also contain a certain amount of fine-grained iron minerals that have been liberated. During the coarse-grained magnetic separation process, the fine-grained iron minerals are washed into the tailings due to the strong impact force of the water flow. The coarse-grained tailings are then fed into the fine-grained magnetic separator, where the slow-flow, high-gradient separation conditions effectively recover the fine-grained iron minerals entrained in the coarse-grained tailings, obtaining additional fine-grained concentrate.
[0067] In a preferred embodiment of step S60, the coarse-grained tailings are first fed into a gravity separator to remove some of the coarse gangue before being fed into the fine-grained magnetic separator for cross-concentration. The gravity separator utilizes the density difference between coarse gangue and fine-grained iron minerals to remove most of the coarse, lightweight gangue under the influence of gravity and hydrodynamics. The concentrate obtained from the gravity separator is then fed into the fine-grained magnetic separator for further magnetic separation, thereby further improving the feed grade and separation efficiency of the cross-concentration.
[0068] S70, Concentrate Dehydration:
[0069] All coarse, medium, and fine-grained concentrates obtained in steps S50 and S60 are combined to form a mixed concentrate slurry. The mixed concentrate slurry is pumped into a concentrate hydrocyclone assembly for classification. After the underflow solids content reaches 65%–75%, it is sent to a high-grade filter press for dewatering. The filter press operation is carried out at a feed pressure of 0.6–1.0 MPa, and the moisture content of the iron concentrate after filter pressing is controlled below 12%. The dewatered iron concentrate is then conveyed by a belt conveyor to a finished iron ore bin for storage, awaiting loading and sale. The hydrocyclone overflow enters the medium-grade system and is combined with the medium-grade concentrate for further processing.
[0070] Through two-stage solid-liquid separation using hydrocyclone classification and pressure filtration dewatering, the moisture content of the concentrate is reduced from 60%~70% to below 12%, enabling the iron concentrate product to meet the standards for transportation and sales. At the same time, the removed water is returned to the process for recycling through the filtrate recovery system.
[0071] S80, Tailings Disposal:
[0072] The tailings from each magnetic separation stage generated in steps S50 and S60 are combined and piped into a tailings settling tank for natural settling and concentration. After a certain period of settling in the settling tank, the upper clear liquid is discharged as overflow, part of which is returned to the production process as dilution water and rinsing water, and most of it enters the turbid water tank for production makeup water; the lower underflow is pumped to the red mud filter press station and filtered and stored together with the red mud generated by the alumina production system.
[0073] In this embodiment, microwave irradiation in the pretreatment stage, combined with a weakly reducing atmosphere, transforms some of the hematite in the red mud into magnetite. At the same time, microwave thermal stress and ultrasonic cavitation effects can significantly improve the degree of individual dissociation of iron minerals, thereby avoiding the problem of fine-grained iron minerals and difficult individual dissociation in red mud.
[0074] In the grading and magnetic separation stages, the slurry is divided into three grades based on two key particle size nodes: 0.15 mm and 0.074 mm. Each grade then undergoes differentiated separation in an optimized magnetic separation environment, thus avoiding particle size interference. Magnetic seed-enhanced flocculation causes fine-grained iron minerals to form strongly magnetic flocs, solving the problem of low recovery rates of fine-grained iron minerals in conventional magnetic separation. Cross-concentration further recovers fine-grained iron minerals entrained in the roughing tailings, achieving efficient recovery of valuable minerals.
[0075] This embodiment can increase the iron recovery rate of the entire red mud iron beneficiation process to over 50%, and the iron concentrate grade can be stably maintained at over 55%. Simultaneously, the entire process employs physical beneficiation methods, and the resulting tailings are safely stored as red mud, which is environmentally friendly.
[0076] Example 2:
[0077] This embodiment provides a method for iron beneficiation from red mud. The difference from Embodiment 1 is that in step S10, the microwave irradiation temperature is controlled between 700℃ and 850℃, and the irradiation time is 15 to 20 minutes. Within this temperature range, the reduction rate of hematite in the red mud is moderate in a weakly reducing atmosphere, resulting in the highest magnetite formation rate. This avoids mineral sintering caused by excessively high temperatures and the over-reduction of magnetite into weakly magnetic aragonite. The remaining operating steps and process parameters are the same as in Embodiment 1.
[0078] Example 3:
[0079] This embodiment provides a method for iron beneficiation from red mud. The difference from Embodiment 1 is that in step S40, NSF is used as the dispersant at a dosage of 80-120 g / t, an anionic polyacrylamide flocculant is used as the selective flocculant at a dosage of 20-35 g / t, and the amount of ultrafine magnetite powder added is 2-4 kg / t. This results in optimal selective flocculation between the fine iron mineral particles and the magnetic seed, with concentrated floc size distribution and moderate floc strength, making them less prone to breakage during subsequent pumping and magnetic separation. The remaining operating steps and process parameters are the same as in Embodiment 1.
[0080] Example 4:
[0081] This embodiment provides a method for iron ore beneficiation from red mud. The difference from Embodiment 1 is that in step S60, the coarse-grained tailings are first subjected to gravity separation via a spiral sluice to remove some of the coarse gangue. The feed concentration of the spiral sluice is controlled at 20%~30%, and the pitch and cross-sectional shape of the spiral sluice are adjusted according to the properties of the raw material. The concentrate obtained from gravity separation is then fed into a fine-grained plate high-gradient magnetic separator for magnetic separation.
[0082] This embodiment reduces the content of coarse gangue in the material entering the fine-particle magnetic separator by 40% to 60%, which can mitigate the risk of contamination and clogging of the separation medium by coarse gangue, while simultaneously improving the feed grade of the fine-particle magnetic separator. All other operating steps and process parameters are the same as in Embodiment 1.
[0083] Example 5:
[0084] This embodiment provides a method for iron ore separation from red mud. The difference from Embodiment 1 is that in step S50, the media gap of the coarse-grained magnetic separator is set to 5mm, and the media gap of the fine-grained magnetic separator is set to 1mm; the magnetic field strength for coarse-grained magnetic separation is set to 1.5T, for medium-grained magnetic separation to 1.0T, and for fine-grained magnetic separation to 1.8T. Under this preferred combination of magnetic separation parameters, the overall separation efficiency of each particle size reaches an optimal balance. The remaining operating steps and process parameters are the same as in Embodiment 1.
[0085] Example 6:
[0086] This embodiment provides a method for iron beneficiation from red mud. The difference from Embodiment 1 lies in the use of a two-stage pressure filtration dewatering process in step S70: the first stage is high-pressure filtration using a diaphragm filter press with a feed pressure of 1.0~1.2 MPa; the second stage is auxiliary dewatering using a vacuum filter press, further reducing concentrate transportation costs and improving product quality. Both the pressure filtration filtrate and the vacuum filtration filtrate are returned to the production water replenishment system for recycling. All other operating steps and process parameters are the same as in Embodiment 1.
[0087] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the technical solutions of the present invention. Any technical solution that can be implemented based on the above embodiments without creative effort should be considered to fall within the scope of protection of the patent of the present invention.
Claims
1. A method of iron recovery from red mud, characterised in that, Includes the following steps: S10. Pretreatment: The high-iron red mud sent from the bottom of the alumina production settling tank is subjected to microwave and ultrasonic treatment to obtain pretreated material. S20. Impurity removal: The pretreated material is diluted with water and fed into a cylindrical screen for slag removal and impurity removal to obtain undersize material. S30. Grading process: The screened material is fed into a hydrocyclone for grading, and is divided into three grades according to particle size: coarse slurry, medium slurry and fine slurry. S40. Enhanced flocculation: Add dispersant to fine-grained slurry and stir, then add ultrafine magnetite powder and stir, and finally add selective flocculant and stir to obtain fine-grained flocculent slurry. S50, Differentiated magnetic separation, feeds coarse-grained slurry, medium-grained slurry and fine-grained flocculent slurry into magnetic separators with corresponding magnetic field strength and corresponding separation structure for differentiated magnetic separation, and obtains coarse-grained tailings, coarse-grained concentrate, medium-grained concentrate and fine-grained concentrate; S60, cross-selection: The coarse-grained tailings are fed into the fine-grained magnetic separator for cross-selection to obtain fine-grained concentrate mixed in with the coarse-grained tailings. S70, Concentrate Dewatering: All coarse, medium, and fine-grained concentrates are combined, classified by a hydrocyclone, and the underflow is sent to a filter press for dewatering to obtain iron concentrate product. The overflow enters the medium-grade system.
2. The red mud iron recovery process of claim 1, characterised in that, In step S10, pretreatment, the red mud is first fed into a microwave reactor and irradiated for 10 to 30 minutes at a microwave frequency of 2.45 GHz, a power of 1.0 to 1.4 kW, and a temperature of 500°C to 1000°C. After cooling, it is ball-milled into a slurry. Then, the slurry is fed into an ultrasonic treatment tank and ultrasonically treated for 2 to 10 minutes at a frequency of 20 to 50 kHz and a power density of 0.1 to 0.5 W / mL.
3. The red mud iron recovery process of claim 2, characterised in that, In step S10, the pretreatment, the microwave irradiation treatment is carried out in a weakly reducing atmosphere, which is a nitrogen mixture with a CO volume fraction of 5% to 15%.
4. The red mud iron recovery process of claim 2, characterised in that, In step S10, pretreatment, the moisture content of the high-iron red mud is adjusted to 3.0%~5.0% before microwave irradiation, and it is kept at a constant temperature between microwave irradiation and ultrasonic treatment.
5. The red mud iron recovery process as claimed in claim 1, wherein, In step S30, the grading process, the coarse-grained slurry has a particle size greater than 0.15 mm, the medium-grained slurry has a particle size of 0.074–0.15 mm, and the fine-grained slurry has a particle size less than 0.074 mm.
6. The red mud iron recovery process of claim 1, characterised in that, In step S40, enhanced flocculation, the dispersant is NSF or sodium hexametaphosphate, with a dosage of 50~200g / t, and the selective flocculant is a polyacrylamide type A flocculant, with a dosage of 10~50g / t.
7. The red mud iron recovery process as claimed in claim 1, wherein, In step S40, enhanced flocculation, the particle size of the ultrafine magnetite powder is less than or equal to 5μm, and its addition amount is 1~6kg / t based on the solid mass in the slurry.
8. The red mud iron recovery process of claim 1, characterised in that, In step S50, differentiated magnetic separation, coarse-grained slurry is separated using a high-gradient low-speed magnetic separator with a magnetic field strength of 1.2~1.8T, medium-grained slurry is separated using a conventional gradient medium-speed magnetic separator with a magnetic field strength of 0.8~1.2T, and fine-grained slurry is separated using a high-gradient high-speed magnetic separator or a flat-plate high-gradient magnetic separator with a magnetic field strength of 1.5~2.0T.
9. The red mud iron recovery process as claimed in claim 1, wherein, In step S60, before the coarse-grained tailings are sent to the fine-grained magnetic separator for cross-selection, some of the coarse gangue is removed by the gravity separation equipment, and the gravity concentrate is then sent to the fine-grained magnetic separator for magnetic separation.
10. The red mud iron recovery process according to any one of claims 1 to 9, characterised in that, Also includes: S80, tailings disposal, combines the tailings from each magnetic separation section and sends them into the tailings settling tank, and the settling underflow is sent to the red mud filter press for disposal.