A recycling method of waste printed circuit board
Through pretreatment, two-stage crushing, ball milling and screening processes, and ball milling under a water vapor atmosphere using composite additives, the problem of secondary pollution in the treatment of non-metallic components of waste printed circuit boards has been solved, and efficient resource utilization and the preparation of flame-retardant composite materials have been achieved.
Patent Information
- Application Number
- CN202611285453.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-24
AI Technical Summary
There is a lack of effective treatment methods for the non-metallic components of waste printed circuit boards in the current technology, which leads to serious secondary pollution caused by landfill or incineration.
By pretreatment to remove electronic components and detinning, combined with two-stage crushing, ball milling and screening processes, and ball milling under a water vapor atmosphere using composite additives, flame-retardant composite materials are prepared by achieving efficient separation and utilization of non-metallic components.
It achieves full and high-value utilization of non-metallic components, avoids secondary pollution, improves resource utilization rate, reduces production costs, and prepares high-efficiency flame-retardant composite materials.
Smart Images

Figure CN123149231A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of circuit board recycling technology, and specifically to a method for recycling and processing waste printed circuit boards. Background Technology
[0002] As a significant component of electronic waste, discarded printed circuit boards (PCBs) contain various heavy metals and hazardous substances such as lead, cadmium, polyvinyl chloride (PVC) plastics, and brominated flame retardants, posing potential environmental pollution risks. However, they also contain common and rare metals like copper, gold, and silver, giving them high recycling value. With the accelerating pace of electronic product upgrades, the amount of discarded PCBs generated is increasing year by year, making their resource recycling a pressing issue in global environmental protection and resource recycling.
[0003] Currently, the main recycling technologies for waste printed circuit boards (PCBs) include physical-mechanical methods, pyrolysis, hydrometallurgical methods, and supercritical fluid treatment. Physical-mechanical methods separate metallic and non-metallic components through crushing and sorting processes, resulting in a relatively simple process. However, this method can only recover metals. The non-metallic components (mainly a mixture of epoxy resin and glass fiber), which account for approximately 60%–70% of the total PCB mass, are typically disposed of as waste through landfill or incineration. Incineration of the non-metallic components leads to the formation of highly toxic polybrominated dibenzodioxins and polybrominated dibenzofurans, while landfilling them causes serious secondary pollution due to the seepage of heavy metals and brominated flame retardants into groundwater. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a method for recycling and processing waste printed circuit boards, which solves the problem that existing recycling technologies only focus on metal recovery, while the non-metallic components, which account for 60% to 70% of the total, lack effective treatment methods, and landfilling or incineration both cause serious secondary pollution.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] A method for recycling and processing waste printed circuit boards includes the following steps:
[0007] S10. Pre-processing: Remove electronic components from the waste printed circuit board, and then desolder the bare printed circuit board after removing the components.
[0008] S20. Crushing: The waste printed circuit boards are coarsely crushed to obtain coarsely crushed material.
[0009] S30. Ball milling treatment: The coarsely crushed material is mixed with the composite additive and then placed in a ball mill for treatment to obtain the ball-milled material.
[0010] S40. Screening: Screen the ball-milled material to separate the copper-rich coarse particles and the calcium bromide-rich non-metallic powder components.
[0011] S50. The non-metallic powder component rich in calcium bromide is directly used as a flame retardant filler and blended with a polymer matrix material to prepare a flame retardant composite material.
[0012] The composite additive includes nano-calcium oxide, nano-silica, and transition metal oxides, wherein the mass percentage of nano-calcium oxide is 60% to 70%, the mass percentage of nano-silica is 20% to 30%, and the mass percentage of transition metal oxides is 5% to 10%.
[0013] Optionally, in step S10 pretreatment, the waste printed circuit board is heated to the solder melting temperature and then the electronic components are removed by vibration.
[0014] Optionally, step S20 crushing is a two-stage crushing process, which includes a primary shear crushing and a secondary impact crushing. The material after the primary shear crushing is passed through a magnetic separator to separate the ferromagnetic metal components, and then undergoes secondary impact crushing.
[0015] Optionally, in the S30 ball milling process, the ball-to-material ratio in the ball mill is 30-40:1, and the mass ratio of the composite additive to the coarsely crushed material is 3-5:1.
[0016] Optionally, in step S30, the transition metal oxide is Fe2O3 or MnO2.
[0017] Optionally, in the ball milling process of step S30, a gradient ball milling medium is used, which includes large balls, medium balls and small balls, with a mass ratio of 2:2:1 and a diameter ratio of 9:5:2.
[0018] Optionally, the ball milling process in step S30 is carried out in a steam atmosphere, and the ball milling process is carried out in a closed ball milling jar.
[0019] Optionally, during the ball milling process, the gas inside the sealed ball milling jar is extracted and sent to the alkali absorption system.
[0020] Optionally, in step S40, the material on the screen is returned to step S30 for ball milling again.
[0021] Optionally, in step S50, the polymer matrix material is at least one of polypropylene, polyethylene, or ABS resin, and the amount of calcium bromide-rich non-metallic powder component added is 25% to 40% of the mass of the polymer matrix material.
[0022] Compared with the prior art, the beneficial effects of the present invention are:
[0023] The pretreatment process, through disassembly and desoldering, prevents heavy metals from components and solder from entering subsequent processing. The crushing process is carried out in a closed system equipped with a dust removal device, preventing the emission of bromine-containing dust. The ball milling process is conducted in a closed ball milling tank equipped with a negative pressure exhaust and alkaline absorption system, which collects and treats the bromine-containing gas generated during ball milling in real time, preventing the generation and emission of highly toxic substances such as dioxins. In addition, the mechanochemical debromination under a water vapor atmosphere stably fixes bromine to the powder surface in the form of calcium bromide, avoiding the risk of bromide seeping into groundwater when non-metallic components are landfilled.
[0024] In addition, after electronic components are collected and sorted, valuable metals and chips are recycled separately; solder is detinned and recycled as tin resource; ferromagnetic metal components are magnetically separated and recycled as iron resource; the copper purity in the copper-rich coarse-grained components can reach more than 90%; and the non-metallic powder components rich in calcium bromide are directly used as flame-retardant fillers to prepare flame-retardant composite materials, realizing the full high-value utilization of non-metallic components that account for 60% to 70% of the total mass of the circuit board, rather than simple landfilling or incineration. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a schematic diagram of the process steps of the present invention. Detailed Implementation
[0027] In the following description, only certain exemplary embodiments are briefly described. As those skilled in the art will recognize, the described embodiments can be modified in various ways without departing from the spirit or scope of the invention. Therefore, the drawings and description are considered to be exemplary in nature and not restrictive.
[0028] The following disclosure provides many different embodiments or examples for implementing various structures of the invention. To simplify the disclosure, specific examples of components and arrangements are described below. These are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different examples; such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed. In addition, the various specific examples of processes and materials provided in this invention are examples of applications of other processes and / or the use of other materials that will be apparent to those skilled in the art.
[0029] The embodiments of the present invention / invention are described in detail below with reference to the accompanying drawings.
[0030] Example:
[0031] See Figure 1 This invention provides a method for recycling and processing waste printed circuit boards, comprising the following steps:
[0032] S10. Pre-treatment: Before entering the subsequent crushing process, waste printed circuit boards undergo pre-treatment to remove electronic components and solder adhering to the boards. Pre-treatment specifically includes two sub-steps: disassembly and desoldering.
[0033] During the disassembly process, the waste printed circuit boards are placed in a heating device and heated to above 183°C, reaching the solder melting temperature. At this temperature, the solder at the leads of the electronic components on the circuit board melts, reducing the connection strength between the components and the circuit board substrate. Subsequently, mechanical vibration is used to break the connection at the molten solder points, causing the electronic components to detach from the circuit board surface under the vibration.
[0034] Vibration disassembly uses a vibration table, and the vibration frequency and amplitude can be adjusted according to the specific specifications of the circuit board. After being sorted and collected, the detached electronic components can enter different metal recycling processes. Chips, connectors, and other components can be further disassembled and recycled for precious metals.
[0035] After the disassembly process is completed, the bare printed circuit board after the components are removed is detinned to remove the solder residue on the surface of the circuit board. This prevents the tin, lead and other metals in the solder from mixing with non-metallic powders during the subsequent ball milling process, which would affect the quality of the final flame-retardant composite material.
[0036] The desoldering process is carried out using a hot air desoldering furnace. The bare circuit board is placed in the furnace and heated until the solder remelts. Then, the molten solder is separated from the surface of the circuit board by centrifugation. The separated solder can be collected and recycled as tin resources. The amount of residual solder on the surface of the bare circuit board is significantly reduced after the desoldering process, providing clean raw materials for subsequent crushing and ball milling processes.
[0037] By pre-removing electronic components and solder, valuable components can be classified and recycled at the component level, improving overall resource utilization. Furthermore, it prevents elements such as metal leads, plating metals, and lead from the solder from contaminating non-metallic powders during subsequent ball milling, ensuring the purity of the non-metallic powders ultimately used as flame-retardant fillers, meeting the purity requirements of polymer composite materials. Simultaneously, pre-removing solder also helps reduce material handling volume in the ball milling process, lowering energy consumption.
[0038] S20. Crushing: The pre-treated bare printed circuit boards enter the crushing process. The crushing process adopts a two-stage crushing method, which includes a first-stage shear crushing and a second-stage impact crushing, with a magnetic separation step between the two stages.
[0039] The primary shearing crushing process employs a twin-shaft shearing crusher. After the bare circuit board is fed into the crusher, it is cut by the shearing action of the twin-shaft blades. The primary shearing crushing utilizes shear force to selectively dissociate the circuit board along the interface between the resin matrix and the copper foil, allowing the copper foil to be peeled off the resin matrix as a whole. The primary shearing crushing process breaks down waste printed circuit boards to the first particle size range.
[0040] After the primary shearing and crushing process, the crushed material is conveyed into a magnetic separator. Utilizing the property that ferromagnetic metals are attracted by magnetic force in a magnetic field, the ferromagnetic metal components (such as residual iron-nickel alloys in component leads, fragments of iron shielding, etc.) are separated from the crushed material. The ferromagnetic metals separated by magnetic separation can be collected and recycled as iron resources.
[0041] Since the primary shear crushing has already crushed the circuit board to an appropriate particle size, and the ferromagnetic metal components have been fully dissociated from the matrix but have not yet been further refined, magnetic separation can achieve higher separation efficiency at this point. Therefore, the magnetic separation step is set between the primary shear crushing and the secondary impact crushing.
[0042] The material after magnetic separation enters the secondary impact crushing stage. The secondary impact crushing is carried out using a hammer crusher, which further crushes the material to the second particle size range, obtaining coarse crushed material, which is then sent to the subsequent ball milling process.
[0043] In step S20, the primary shear crushing utilizes shear force to selectively dissociate the copper foil along the resin matrix interface, avoiding excessive stretching and wrapping of the copper foil, thus laying the foundation for the efficient separation of copper and non-metals in the subsequent process. The magnetic separation stage between the two crushing stages separates the ferromagnetic metal in advance, which not only recovers valuable metal resources but also prevents the ferromagnetic metal from interfering with or contaminating the debromination reaction in the subsequent ball milling process. The secondary impact crushing refines the material to a suitable particle size range for ball milling, ensuring the feed particle size requirements of the ball milling process and improving ball milling efficiency.
[0044] S30. Ball milling: The coarsely crushed material after crushing enters the ball milling process, which is carried out in a stirred ball mill.
[0045] Before ball milling, the coarsely crushed material needs to be mixed with a composite additive in a certain proportion. The composite additive consists of three components: nano-calcium oxide, nano-silica, and transition metal oxides. Nano-calcium oxide accounts for 60%–70% of the mass and acts as the main additive for debromination; nano-silica accounts for 20%–30% of the mass and acts as the first synergistic additive for interface provision; and transition metal oxides account for 5%–10% of the mass and acts as the second synergistic additive for electron transfer catalysis. The transition metal oxide can be Fe2O3 or MnO2. The preferred particle size of nano-calcium oxide is 50–200 nm, and the preferred particle size of nano-silica is 10–50 nm, to fully utilize the high specific surface area and surface activity advantages of nanoparticles.
[0046] The mass ratio of coarsely crushed material to composite additive is 3~5:1, that is, 3~5 parts of coarsely crushed material are added to every 1 part of composite additive. The ball-to-material ratio in the ball mill is 30~40:1, that is, the mass of the ball milling media is 30~40 times the mass of the material.
[0047] The milling media employs a gradient configuration. The milling media includes three different diameter grinding balls: large, medium, and small. The mass ratio of large, medium, and small balls is 2:2:1, and the diameter ratio is 9:5:2. In a preferred embodiment, the large balls have a diameter of 18 mm, the medium balls 10 mm, and the small balls 4 mm. The large balls provide high-energy impact, primarily acting on the brittle resin matrix and glass fibers in the coarsely crushed material, rapidly breaking them into micron-sized powder. Simultaneously, under the impact, the highly ductile copper foil undergoes plastic deformation and curls into millimeter-sized copper coils. The medium and small balls provide shearing and grinding effects, promoting interfacial contact and reaction between the composite additives and material particles in the debromination reaction, and further refining the resin and glass fibers.
[0048] Furthermore, the ball milling process is carried out in a sealed ball mill jar with a water vapor atmosphere. Specifically, water vapor is continuously introduced into the sealed ball mill jar to maintain a saturated or supersaturated state. During ball milling, the water vapor reacts with nano-calcium oxide to produce calcium hydroxide. Calcium hydroxide then reacts with hydrogen bromide released from the brominated flame retardant during ball milling to produce calcium bromide and water. The generated water further reacts with nano-calcium oxide to produce calcium hydroxide, thus forming a self-sustaining catalytic cycle. In this cycle, water molecules continuously participate in the reaction as a reaction medium and catalyst without being consumed, continuously promoting the capture of hydrogen bromide and the formation of calcium bromide. Simultaneously, nano-silica adsorbs onto the surface of the coarsely crushed material during ball milling, providing a rich active interface for the solid-phase nucleophilic substitution reaction between nano-calcium oxide and the brominated flame retardant. Under the mechanical force generated by ball milling, transition metal oxides undergo electron transfer with the carbon-bromine bond, effectively lowering the activation energy of the nucleophilic substitution reaction and accelerating the breaking of the carbon-bromine bond.
[0049] Furthermore, water vapor has a unique penetrating and carrying effect during ball milling. Water vapor molecules can penetrate into the micropores and microcracks inside the coarsely crushed material particles, carrying hydrogen bromide released from the resin matrix to the surface of the material particles. This allows the reaction between hydrogen bromide and nano-calcium oxide to extend from the particle surface to the bulk phase of the particles, significantly increasing the effective contact area of the reaction and promoting the full progress of the debromination reaction.
[0050] During the ball milling process, a negative pressure extraction device is connected to the sealed ball mill jar. This device operates continuously, extracting the bromine-containing gas (mainly hydrogen bromide gas and a small amount of volatile organic compounds) generated during the ball milling reaction and sending it to the alkaline absorption system for treatment. The alkaline absorption system uses an alkaline spray tower filled with sodium hydroxide solution or calcium hydroxide slurry as the absorbent. Upon entering the spray tower, the bromine-containing gas comes into countercurrent contact with the sprayed alkaline solution. The hydrogen bromide in the gas is absorbed by the alkaline solution, generating sodium bromide or calcium bromide solution. The exhaust gas, after alkaline spray treatment, is then passed through a gas-liquid separator to remove entrained droplets before being released into the atmosphere, preventing fugitive emissions of bromine-containing gas and ensuring the environmental safety of the process.
[0051] During ball milling, under the influence of nano-calcium oxide, nano-silica, and transition metal oxides, and in the combination of a unique gradient milling media and a steam atmosphere, the brominated flame retardant in the coarsely crushed material undergoes a highly efficient nucleophilic substitution debromination reaction. The carbon-bromine bonds break, and bromine is captured in ionic form by nano-calcium oxide and converted into calcium bromide, which is then stably fixed to the surface of the non-metallic powder. After ball milling, the milled material is obtained.
[0052] S40. Screening: After ball milling, the ball-milled material is fed into a vibrating screen for screening, utilizing the naturally formed particle size difference between the copper and non-metallic components in the ball-milled material for separation.
[0053] Vibrating screening is carried out under dry conditions, avoiding the wastewater problems in wet processes and simplifying subsequent treatment procedures.
[0054] After the ball-milled material is fed into a vibrating screen, it is sieved according to particle size differences under vibration. The screen mesh size is selected based on the particle size distribution of copper coils and non-metallic powders in the material, typically using a 100-120 mesh screen. After sieving, the oversize material is a copper-rich coarse-grained component, mainly consisting of millimeter-sized copper coils and a small amount of incompletely dissociated coarse particles; the undersize material is a calcium bromide-rich non-metallic powder component, mainly consisting of micron-sized debrominated non-metallic powders. The copper purity in the copper-rich coarse-grained component can reach over 90%, and it can be directly recovered as copper concentrate.
[0055] For the portion of the oversize material with a particle size larger than the set value (i.e., containing material particles that have not been fully dissociated), it is collected and returned to step S30 for ball milling again to ensure sufficient dissociation and complete debromination of the material, thereby improving the overall recovery rate and treatment effect. For the copper-rich coarse particles in the oversize material that meet the particle size requirements, they are directly collected as the product.
[0056] After collection, the calcium bromide-rich non-metallic powder component directly enters the utilization process in step S50. The mass fraction of calcium bromide in this non-metallic powder component is approximately 5% to 10%.
[0057] In step S40, the particle size difference automatically formed between copper and non-metals during ball milling is utilized to achieve efficient separation of copper and non-metal components through a single vibrating sieve step.
[0058] S50. The non-metallic powder component rich in calcium bromide obtained after sieving is used directly as a flame retardant filler and blended with a polymer matrix material to prepare a flame retardant composite material.
[0059] Before blending and granulation, the calcium bromide-enriched non-metallic powder component is first dried to remove any adsorbed moisture, ensuring good bonding between the non-metallic powder and the polymer matrix material. During drying, the temperature and time are adjusted according to the powder's moisture content. The dried non-metallic powder can then be graded according to particle size; different particle size grades can be used to prepare flame-retardant composite materials with different performance requirements, achieving refined product classification.
[0060] In the blending and granulation process, the dried calcium bromide-enriched non-metallic powder component is mixed with the polymer matrix material in a certain proportion and then fed into a twin-screw extruder for melt blending and granulation. The polymer matrix material can be selected from at least one of polypropylene, polyethylene, or ABS resin, or a mixture of two or more of the above resins. The amount of calcium bromide-enriched non-metallic powder component added is 25% to 40% of the mass of the polymer matrix material, that is, 25 to 40 parts of non-metallic powder filler are added to every 100 parts of polymer matrix material.
[0061] In this flame-retardant composite material, the non-metallic powder component contains in-situ generated calcium bromide and residual antimony trioxide from the circuit board raw materials. When the composite material is heated or burned, the calcium bromide decomposes to release hydrogen bromide. The hydrogen bromide reacts with antimony trioxide to generate antimony tribromide. Antimony tribromide is a highly efficient gas-phase flame-retardant active species that can capture free radicals in the combustion chain reaction in the gas phase, thereby interrupting the combustion reaction and inhibiting flame propagation.
[0062] In step S50, the calcium bromide-rich non-metallic powder component is directly used as a flame-retardant filler, achieving full resource utilization of the non-metallic component and avoiding secondary pollution caused by landfilling or incineration of non-metallic powders in traditional processes. This eliminates the intermediate steps of water washing to remove calcium bromide and surface modification, simplifying the process and reducing production costs. Simultaneously, the synergistic flame-retardant effect of calcium bromide and residual antimony trioxide enables the composite material to achieve a limiting oxygen index of over 28%. Furthermore, the amount of non-metallic powder added can reach 25%–40% of the polymer matrix material mass, resulting in high filler utilization. This flame-retardant composite material can be used to prepare products such as plastic pallets, plastic-wood flooring, and automotive interior parts, showing promising market application prospects.
[0063] In this embodiment, the complete resource recovery of waste printed circuit boards is achieved through five steps: pretreatment, crushing, ball milling, sieving, and utilization. The pretreatment step achieves the classified recycling of components and solder through heating disassembly and detinning. The crushing process achieves selective dissociation of materials and separation of ferromagnetic metals through shear crushing, magnetic separation, and impact crushing. The ball milling step achieves efficient mechanochemical debromination and particle size separation of copper and non-metals through the synergistic effect of composite additives, gradient ball milling media, and steam atmosphere. The sieving step achieves efficient separation of copper and non-metals through one-step vibrating sieving. The utilization step uses calcium bromide-rich non-metallic powder directly as a flame-retardant filler to prepare flame-retardant composite materials.
[0064] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the technical solutions of the present invention. Any technical solution that can be implemented based on the above embodiments without creative effort should be considered to fall within the scope of protection of the patent of the present invention.
Claims
1. A method for recycling and processing waste printed circuit boards, characterized in that, Includes the following steps: S10. Pre-processing: Remove electronic components from the waste printed circuit board, and then desolder the bare printed circuit board after removing the components. S20. Crushing: The waste printed circuit boards are coarsely crushed to obtain coarsely crushed material. S30. Ball milling treatment: The coarsely crushed material is mixed with the composite additive and then placed in a ball mill for treatment to obtain the ball-milled material. S40. Screening: Screen the ball-milled material to separate the copper-rich coarse particles and the calcium bromide-rich non-metallic powder components. S50. The non-metallic powder component rich in calcium bromide is directly used as a flame retardant filler and blended with a polymer matrix material to prepare a flame retardant composite material. The composite additive includes nano-calcium oxide, nano-silica, and transition metal oxides, wherein the mass percentage of nano-calcium oxide is 60% to 70%, the mass percentage of nano-silica is 20% to 30%, and the mass percentage of transition metal oxides is 5% to 10%.
2. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, In step S10 pretreatment, the waste printed circuit board is heated to the solder melting temperature and then the electronic components are removed by vibration.
3. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, The crushing in step S20 is a two-stage crushing process, which includes primary shear crushing and secondary impact crushing. The material after primary shear crushing is separated from the ferromagnetic metal components by a magnetic separator before undergoing secondary impact crushing.
4. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, In the S30 ball milling process, the ball-to-material ratio in the ball mill is 30-40:1, and the mass ratio of the composite additive to the coarsely crushed material is 3-5:
1.
5. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, In step S30, the transition metal oxide is Fe2O3 or MnO2.
6. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, In step S30, the ball milling process uses a gradient ball milling medium, which includes large balls, medium balls, and small balls. The mass ratio of the large balls, medium balls, and small balls is 2:2:1, and the diameter ratio is 9:5:
2.
7. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, The ball milling process in step S30 is carried out in a steam atmosphere and in a sealed ball milling jar.
8. The method for recycling and processing waste printed circuit boards according to claim 7, characterized in that, During the ball milling process, the gas inside the sealed ball mill jar is extracted and sent to the alkali absorption system.
9. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, In step S40, the material on the screen is returned to step S30 for ball milling again.
10. The method for recycling and processing waste printed circuit boards according to claim 1, characterized in that, In step S50, the polymer matrix material is at least one of polypropylene, polyethylene or ABS resin, and the amount of calcium bromide-rich non-metallic powder component added is 25% to 40% of the mass of the polymer matrix material.