Method and system for recycling waste crystalline silicon photovoltaic cell based on impurity threshold control

By dismantling and analyzing the composition of waste crystalline silicon photovoltaic cells, dynamically adjusting the process route, and employing impurity threshold control and electrochemical testing, the problem of unstable recycling performance caused by component fluctuations in existing technologies has been solved, achieving efficient silver recovery and silicon resource utilization.

CN123149236APending Publication Date: 2026-11-24SUZHOU XIRE ENERGY SAVING ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611441134.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing recycling processes for waste crystalline silicon photovoltaic cells are ill-suited to materials with large compositional fluctuations. This leads to co-dissolution of impurities during the leaching stage and easy co-deposition of impurities during electrodeposition, making it difficult to balance silver recovery quality, silicon substrate protection, and stable mother liquor circulation.

Method used

By dismantling and analyzing the composition of waste crystalline silicon photovoltaic modules, the process route is dynamically adjusted, and impurity threshold control and electrochemical testing are adopted to selectively purify and electrodeposit, forming a closed-loop circulation system.

Benefits of technology

It improves the purity and efficiency of silver recovery, reduces reagent consumption, reduces the generation of heavy metal waste liquid, realizes the synergistic utilization of silver and silicon resources, and enhances the economic value of resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149236A_ABST
    Figure CN123149236A_ABST
Patent Text Reader

Abstract

This invention discloses a method and system for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control, belonging to the field of resource utilization technology for waste photovoltaic modules. The method includes the following steps: disassembling waste crystalline silicon photovoltaic modules, removing non-cell components to obtain crystalline silicon cell material containing silver grid lines; pre-treating the cell material to remove residual adhesive and solder ribbon residue; performing aluminum back electrode pre-removal or passivation treatment on the pre-treated cells; adding the aluminum-treated cells to a silver selective leaching solution to allow metallic silver from the silver grid lines to enter the solution, forming a silver-containing leaching solution; performing solid-liquid separation to obtain the silver-containing leaching solution and low-silver silicon residue; performing impurity detection and threshold judgment on the silver-containing leaching solution; when the concentration of one or more impurities among Al, Cu, Pb, and Sn exceeds a set threshold, initiating a silver-containing solution purification step to reduce the impurity concentration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of resource utilization technology of waste photovoltaic modules, and relates to a method and system for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control. Background Technology

[0002] Crystalline silicon photovoltaic (PV) modules typically consist of glass, encapsulating film, solar cells, solder ribbons, backsheets, aluminum frames, and junction boxes. Silver primarily exists on the surface of the crystalline silicon solar cells as fine grid lines and main grid lines on the front side, while aluminum is mainly distributed in the aluminum back field or back electrode on the back side of the cells. Copper, tin, and lead mainly originate from solder ribbons, busbars, or solder residue. As early large-scale PV power plants gradually reach their designed service life, a large number of crystalline silicon PV modules are entering the retirement and scrapping stage, leading to a year-on-year increase in the volume of waste crystalline silicon PV modules. Silver is a scarce precious metal, silicon is a core raw material for the photovoltaic industry, and aluminum and copper also have high recycling value. How to achieve efficient separation and high-value resource utilization of silver, aluminum, silicon, and solder ribbon-related metal components in waste modules, reduce hazardous waste generation, and build a green closed-loop development chain for photovoltaic materials has become a crucial issue that the industry urgently needs to address.

[0003] Public research indicates that the composition of waste crystalline silicon solar cells fluctuates significantly, varying considerably depending on the original module model, production year, power plant operating environment, dismantling and crushing process, and whether metal components such as solder ribbons and busbars are mixed in during dismantling. The content of Si, Ag, and Al elements in waste solar cells from different sources varies considerably, with silicon being the main component. Silver and aluminum are the key targets for recycling and separation. When solder ribbons, busbars, and solder debris are mixed in the dismantled material, the content of heavy metal impurities such as Cu, Pb, and Sn increases dramatically. Most existing recycling processes use a fixed set of process parameters to process all incoming materials without adapting to differences in material composition. They directly apply fixed acid leaching conditions or fixed electrodeposition parameters, failing to switch process routes and dynamically control the process based on raw material composition, impurity levels, and the morphology of silver within the leaching system. This results in poor process adaptability to complex incoming materials.

[0004] In existing technologies, nitric acid leaching is a commonly used method for dissolving silver grid lines. However, the nitric acid leaching process generates toxic nitrogen oxide tail gas, leading to tail gas treatment pressure, and also results in high acid consumption. Furthermore, this system has poor selectivity, easily causing metals such as Al, Pb, Cu, and Sn to dissolve simultaneously with silver, entering the leaching solution, and a large number of impurity ions enter subsequent processes with the leaching solution. Alkali treatment can remove aluminum back electrodes; however, improper control of process parameters can not only lead to hydrogen evolution safety risks but also cause etching of the silicon substrate, resulting in silicon substrate loss and reducing the recycling value of silicon residue. The ammonia-hydrogen peroxide leaching system can generate silver ammonia complex ions, achieving selective dissolution of silver. However, this system has stringent operational control requirements; excessively rapid hydrogen peroxide addition or a sharp increase in system temperature can cause ineffective reagent decomposition. At the same time, ammonia is volatile, causing both reagent loss and waste gas pollution. Electrodeposition is widely used in the field of hydrometallurgical precious metal recovery due to its advantages of high-purity silver products, low reagent dosage, and recyclable mother liquor. However, the forms in which silver exists differ fundamentally under different leaching systems. In acidic leaching systems, silver exists primarily as Ag. + Silver exists in the form of [Ag(NH3)2] in ammoniacal leaching systems. + The presence of complexed ions leads to significant differences in the reduction potential windows for different silver species. Current processes mostly use preset fixed potentials or constant current densities for electrodeposition without considering the actual composition of the leaching solution to determine the effective reduction range of silver. This easily leads to the simultaneous co-deposition of impurity ions such as Cu, Pb, and Sn, ultimately reducing the purity of the metallic silver product. It also results in a loose, easily pulverized electrodeposition layer structure and lowers the current efficiency of the electrodeposition process. Furthermore, impurity ions continuously accumulate in the circulating mother liquor, further exacerbating the process instability of subsequent batches.

[0005] In summary, existing silver recycling processes for waste crystalline silicon photovoltaic cells are difficult to adapt to waste cells with large compositional fluctuations. The problem of impurity co-dissolution is prominent in the leaching stage, and the electrodeposition stage lacks potential window calibration for the actual material solution, making it easy for impurities to co-deposit and reduce the quality of silver products. At the same time, there is a lack of dynamic process control methods to address material differences, making it difficult to meet the multiple requirements of efficient silver recovery, silicon substrate protection, reagent reduction, and stable mother liquor circulation. Summary of the Invention

[0006] The purpose of this invention is to solve the technical problems in the existing silver recycling process of waste crystalline silicon photovoltaic cells, such as poor adaptability to fluctuations in the composition of the incoming material, co-dissolution of leaching impurities, easy co-deposition of impurities in electrodeposition, and difficulty in balancing the quality of silver recovery, silicon substrate protection, and stable circulation of mother liquor. The invention provides a method and system for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control.

[0007] To achieve the above objectives, the present invention employs the following technical solution: In a first aspect, this invention discloses a method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control, comprising the following steps: Dismantle waste crystalline silicon photovoltaic modules, remove non-cell components, and obtain crystalline silicon cell material containing silver grid lines; The composition of the battery cell material is analyzed, and the elements to be tested include at least Ag, Al, Cu, Pb and Sn. The subsequent process route is determined based on the test results. The battery cell material is pretreated to remove residual adhesive and solder ribbon residue; The pre-treated solar cells undergo aluminum back electrode pre-removal or passivation treatment. The aluminum-treated battery cells are added to a silver selective leaching solution, allowing the metallic silver in the silver grid lines to enter the solution and form a silver-containing leaching solution. Solid-liquid separation was performed to obtain a silver-containing leachate and a low-silver silicon residue; The silver-containing leachate is subjected to impurity detection and threshold determination. When the concentration of one or more impurities among Al, Cu, Pb, and Sn exceeds a set threshold, the silver-containing solution purification step is initiated to reduce the concentration of the impurities. Electrochemical tests were performed on the purified or regulated silver-containing leachate to determine the potential window in which silver preferentially deposits and impurity co-deposition is suppressed. Electrodeposition is performed within the potential window, causing silver to be reduced and deposited as metallic silver on the cathode surface; The silver-poor solution after electrodeposition is adjusted in composition and then returned to the silver selective leaching step for recycling.

[0008] Further improvements are made in the following aspects: The composition detection employs one or more of XRF, ICP-OES, ICP-MS, AAS, or chemical titration; the process route determination includes at least one of the following decision logics: When the Al content is higher than the set threshold, the aluminum back electrode is first pre-removed or passivated. When the contents of Cu, Pb, and Sn are higher than the set threshold, the solder strip strengthening separation is performed first, or an impurity control step is set before silver electrodeposition. When the residual adhesive content is high, the residual adhesive should be removed first; When the Ag content is low, silver-rich component sorting, multi-stage countercurrent leaching, circulating leaching, or leachate enrichment methods can be used to increase the concentration of silver-containing solution.

[0009] The pre-removal or passivation treatment of the aluminum back electrode adopts an acidic or alkaline system. The conditions for the acidic system are: hydrochloric acid mass fraction of 2% to 10%, temperature of 15 to 60°C, treatment time of 1 to 4 hours, and liquid-to-solid ratio of 5 to 50 mL / g. The conditions for the alkaline system are: NaOH or KOH concentration of 10 to 100 g / L, temperature of 20 to 80°C, treatment time of 10 to 90 minutes, and liquid-to-solid ratio of 5 to 50 mL / g.

[0010] The pretreatment includes one or more of the following: heat treatment, swelling and softening, mechanical peeling, sieving, air separation, magnetic separation, gravity separation, alkaline washing, or surface cleaning; The composition adjustment of the silver-poor solution includes at least one of the following operations: stopping electrodeposition when the Ag concentration is below the electrodeposition endpoint threshold; replenishing acid, ammonia, or complexing agent concentrations when they are below the required leaching range; replenishing oxidant or performing electrochemical re-oxidation when the redox potential is below the required silver leaching range; initiating bypass purification when Al, Cu, Pb, Sn, or Fe impurity ions exceed the circulation threshold; and partially draining and refreshing the mother liquor when the number of mother liquor circulations reaches a set value.

[0011] The selective silver leaching solution employs an acidic oxidative leaching system or an alkaline silver ammonia complex leaching system; the acidic oxidative leaching system includes nitric acid, methanesulfonic acid, organic acids or combinations thereof, and is combined with one or more of hydrogen peroxide, dissolved oxygen, ferric salts, persulfates or electrochemical oxidation systems; the alkaline silver ammonia complex leaching system includes ammonia and hydrogen peroxide.

[0012] When the acidic oxidative leaching system uses nitric acid-hydrogen peroxide, the nitric acid concentration is 0.1–4 mol / L, H2O2 is added in batches, the reaction temperature is 20–70℃, the reaction time is 10–180 min, and the liquid-to-solid ratio is 5–50 mL / g. When the alkaline silver ammonia complex leaching system uses ammonia-hydrogen peroxide, the ammonia concentration is 0.5–5 mol / L, H2O2 is added in batches, the pH is 9–12, the reaction temperature is 15–50℃, the reaction time is 10–90 min, and the liquid-to-solid ratio is 5–50 mL / g.

[0013] The impurity control methods include one or more of pH-adjusted precipitation, ion exchange, adsorption, membrane separation, extraction, or stepwise electrochemical treatment; the set threshold is determined based on the purity of the target silver product, the type of leaching system, the electrodeposition window, and the number of mother liquor cycles.

[0014] The electrochemical tests include one or more of cyclic voltammetry, linear sweep voltammetry, chronoamperometry, or chronopotentialometry; the electrochemical tests are at least used to determine the reduction peak or reduction initiation potential of silver species in silver-containing leachates, the co-deposition potential of impurity ions, and the potential range in which silver preferentially deposits and impurity co-deposition is suppressed.

[0015] The electrodeposition is performed using constant potential, constant current, pulse electrodeposition, or stepped potential electrodeposition methods; the cathode material is stainless steel, titanium plate, graphite, carbon felt, carbon cloth, conductive carbon material, or its surface-modified material; the anode material is titanium-based coated anode, graphite anode, or platinum-titanium anode.

[0016] Secondly, this invention discloses a waste crystalline silicon photovoltaic cell recycling system based on impurity threshold control using the above-described method, comprising: An impurity detection unit is used to detect impurities in silver-containing leachate, and the elements to be detected include at least Al, Cu, Pb and Sn; The threshold judgment and control unit is connected to the impurity detection unit and is used to receive the impurity detection results. When the concentration of one or more impurities among Al, Cu, Pb, and Sn exceeds the set threshold, a purification start signal is issued. A purification unit, connected to the threshold judgment and control unit, is used to initiate the silver-containing liquid purification step after receiving the purification start signal, so as to reduce the impurity concentration; The electrochemical testing unit is used to perform electrochemical tests on purified or unpurified silver-containing leachates to determine the potential window in which silver preferentially deposits and impurity co-deposition is suppressed. An electrodeposition unit, connected to the electrochemical testing unit, is used to perform electrodeposition within the potential window, so that silver is reduced and deposited as metallic silver on the cathode surface.

[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control. By using raw material composition detection as a pre-processing step, it solves the fundamental problem of unstable recycling results caused by using fixed leaching schemes due to the complex sources and large differences in element content of waste cells in existing technologies. This method dynamically determines the removal methods for residual adhesive and solder ribbon, the pretreatment intensity of the aluminum back electrode, the selection of the silver leaching system, and the impurity control strategy before electrodeposition based on the detected content of key elements such as Ag, Al, Cu, Pb, and Sn. This allows the same method framework to adapt to waste cell materials of different grades and sources, avoiding a decrease in silver leaching rate or deterioration of silver product purity due to material fluctuations. Furthermore, by judging the impurity threshold of the silver-containing leaching solution and selectively initiating purification steps, intervention is only performed when the impurity concentration reaches a level that affects the electrodeposition effect. This ensures the quality of the silver-containing solution entering the electrodeposition unit while avoiding reagent waste and silver loss due to excessive purification, achieving a balance between impurity control effectiveness and operating costs. This method introduces an electrochemical testing step before silver electrodeposition for recovery, characterizing the actual silver-containing leaching solution using voltammetry. This precisely determines the potential window where silver preferentially deposits while co-deposition of impurities such as copper, lead, and tin is suppressed, rather than using a preset fixed potential or current density. This allows the electrodeposition process to adapt to the differences in silver species morphologies in different leaching systems (acidic silver ion systems or alkaline silver ammonia complex systems), ensuring high selectivity and high current efficiency in silver deposition from an electrochemical perspective. The resulting silver product has significantly improved purity, and the deposited layer is dense and easy to peel off. Furthermore, the silver-poor solution after electrodeposition is not directly discharged but is recycled back to the silver leaching step after composition adjustment. Combined with a bypass purification mechanism to remove impurities accumulated during the recycling process, a closed-loop recycling system is formed. This significantly reduces the consumption of acids, alkalis, oxidants, and complexing agents, and reduces the generation and discharge of heavy metal-containing wastewater, demonstrating good environmental friendliness. In addition, the silver, aluminum, copper, lead, tin and other metal content in the low-silver silicon residue after silver leaching and washing is significantly reduced. It can be used as a raw material for silicon powder, metallurgical silicon, silicon-based composite materials or for further purification to prepare high-purity silicon. This realizes the synergy between silver recovery and silicon resource utilization, and enhances the economic value of the overall resource utilization of waste crystalline silicon photovoltaic modules.

[0018] Furthermore, by employing multiple detection methods such as XRF and ICP-OES, the appropriate detection method can be flexibly selected according to different material characteristics and detection accuracy requirements, ensuring accurate acquisition of composition data. More importantly, this method does not simply record the detection results as information, but directly embeds them into the process decision chain: when aluminum content exceeds the limit, aluminum removal pretreatment is strengthened, fundamentally reducing the interference load of aluminum on subsequent leaching and electrodeposition; when copper, lead, and tin content exceeds the limit, solder strip enhanced separation or pre-electrodeposition purification is initiated, avoiding damage to the purity of silver products from these easily co-deposited impurities; when silver content is low, multi-stage countercurrent leaching or leaching solution enrichment strategies are adopted, ensuring that economically feasible silver recovery efficiency can be maintained even under low-grade material conditions. This branching decision mechanism based on raw material detection results allows the same methodological framework to cover a wide range of materials from high to low grade and from low to high impurities, effectively overcoming the technical defects of fixed process flows being sensitive to raw material fluctuations, and significantly broadening the applicability and industrial practicality of the method.

[0019] Furthermore, existing technologies typically employ electrodeposition at a fixed potential or a fixed current density, because silver in different leaching systems is in the form of Ag. + Silver can exist in different forms, such as silver-ammonia complexes, and their reduction potentials vary significantly. Using fixed parameters easily leads to the co-deposition of impurities. This claim explicitly employs electrochemical testing methods such as cyclic voltammetry and linear sweep voltammetry, and specifies that at least the reduction peak or reduction initiation potential of silver species, the co-deposition potential of impurity ions, and the potential range for preferential silver deposition must be measured. This ensures that the operator can obtain the optimal deposition window for the actual composition of the current silver-containing solution. This window determination method based on real-time electrochemical characterization can dynamically respond to fluctuations in silver concentration, complexing agent concentration, pH value, and impurity levels in the leachate, thus ensuring high selectivity and high current efficiency in the silver deposition process in principle. The purity of the obtained silver product and the quality of the deposited layer are significantly better than those obtained by operating with fixed parameters.

[0020] Furthermore, the specific electrodeposition method and the selection of anode and cathode materials are defined, ensuring the high efficiency and stability of the silver deposition process from an engineering operation perspective. It covers a variety of optional deposition methods, including constant potential, constant current, pulsed electrodeposition, and stepped potential electrodeposition. Among them, pulsed electrodeposition, by adjusting the pulse current density, on-time, off-time, and duty cycle, can effectively reduce concentration polarization on the cathode surface, improve the density and peelability of the silver deposition layer, and avoid peeling difficulties and product quality degradation caused by loose deposition layers or dendrite growth. Regarding electrode materials, this claim provides a variety of cathode options, including stainless steel, titanium plates, graphite, carbon felt, carbon cloth, conductive carbon materials and their surface-modified materials, as well as a variety of inert anode options such as titanium-based coated anodes, graphite anodes, and platinum-titanium anodes. This allows operators to flexibly configure suitable electrode systems based on the acidity, alkalinity, corrosiveness, and conductivity characteristics of the silver-containing solution, ensuring both electrodeposition efficiency and the corrosion resistance and service life of the electrode materials, providing reliable engineering guarantees for the continuous industrial operation of the method.

[0021] This invention discloses a waste crystalline silicon photovoltaic cell recycling system based on impurity threshold control. Through the coordinated operation of multiple functional units, it achieves efficient purification and selective electrodeposition recovery of silver-containing leachate, significantly improving the automation, controllability, and economy of the silver recovery process. The system first utilizes an impurity detection unit to rapidly detect key impurity elements in the silver-containing leachate, covering at least aluminum, copper, lead, and tin. This accurately determines the composition and concentration distribution of impurities in the leachate, providing a reliable data foundation for subsequent purification decisions. The threshold judgment and control unit, based on the detection results, determines in real time whether the concentration of each impurity exceeds a set threshold. When the threshold is exceeded, it automatically issues a purification start signal, effectively avoiding the lag and uncertainty of manual judgment and ensuring the timeliness and targeted nature of the purification process. Upon receiving the start signal, the purification unit selectively initiates purification steps, rather than indiscriminately purifying all leachate. This on-demand purification strategy effectively reduces the consumption of purification reagents and operation time, lowers processing costs, and avoids interference from over-purification of the silver-containing leachate system. The electrochemical testing unit precisely determines the potential window where silver preferentially deposits and impurity co-deposition is suppressed by performing electrochemical tests on purified or unpurified silver-containing leaching solutions. This provides optimal electrodeposition parameters for the leaching solution under specific compositional conditions, ensuring that silver ions are preferentially reduced at the cathode surface during electrodeposition, while impurities such as aluminum, copper, lead, and tin are suppressed and difficult to co-deposit, thus guaranteeing the purity of the deposited silver product. Operating within this potential window, the electrodeposition unit efficiently reduces silver ions to metallic silver at the cathode surface, achieving efficient separation of silver from impurities. The deposited product meets the quality requirements of high-purity silver products without further deep purification. The entire system forms a complete closed-loop control chain of "detection—judgment—purification—testing—deposition," with accurate signal transmission and timely action responses between units. This avoids the problem of decreased purity of electrodeposited silver due to excessive impurities and prevents unnecessary over-purification that could lead to silver loss. While ensuring the quality of recovered silver, it maximizes the direct recovery rate and resource utilization efficiency, resulting in significant environmental and economic benefits. It is suitable for large-scale application in the recycling and processing of waste crystalline silicon photovoltaic cells. Meanwhile, when dealing with waste photovoltaic cells from different sources and batches, the system can flexibly switch working modes according to the actual impurity status of the leachate. For leachate with impurity concentrations within the standard, it can directly enter the electrodeposition stage, improving processing efficiency. For leachate with impurity concentrations exceeding the standard, it automatically triggers the purification and retesting process, ensuring the system's adaptability and the stability of the processing effect. Attached Figure Description

[0022] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0023] Figure 1 This is a flowchart illustrating a method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control, as described in an embodiment of the present invention. Detailed Implementation

[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.

[0025] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.

[0026] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.

[0027] The present invention will now be described in further detail with reference to the accompanying drawings: See Figure 1 This invention discloses a method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control, comprising the following steps: S1, dismantle the waste crystalline silicon photovoltaic modules, remove non-cell components, and obtain crystalline silicon cell material containing silver grid lines; S2, perform composition detection on the battery cell material, and detect at least Ag, Al, Cu, Pb and Sn, and determine the subsequent process route based on the detection results; The composition detection employs one or more of XRF, ICP-OES, ICP-MS, AAS, or chemical titration; the process route determination includes at least one of the following decision logics: When the Al content is higher than a set threshold, the aluminum back electrode is first pre-removed or passivated. The pre-removed or passivated aluminum back electrode uses an acidic or alkaline system. The conditions for the acidic system are: hydrochloric acid mass fraction of 2% to 10%, temperature of 15 to 60°C, treatment time of 1 to 4 hours, and liquid-to-solid ratio of 5 to 50 mL / g. The conditions for the alkaline system are: NaOH or KOH concentration of 10 to 100 g / L, temperature of 20 to 80°C, treatment time of 10 to 90 minutes, and liquid-to-solid ratio of 5 to 50 mL / g.

[0028] When the contents of Cu, Pb, and Sn are higher than the set threshold, the solder strip is first strengthened and separated, or an impurity control step is set before silver electrodeposition. The impurity control method includes one or more of the following: pH adjustment precipitation, ion exchange, adsorption, membrane separation, extraction, or stepwise electrochemical treatment. The set threshold is determined according to the purity of the target silver product, the type of leaching system, the electrodeposition window, and the number of mother liquor cycles.

[0029] When the residual adhesive content is high, the residual adhesive should be removed first; When the Ag content is low, silver-rich component sorting, multi-stage countercurrent leaching, circulating leaching, or leachate enrichment methods can be used to increase the concentration of silver-containing solution.

[0030] S3, pre-treat the battery cell material to remove residual adhesive and solder ribbon residue; the pre-treatment includes one or more of the following: heat treatment, swelling and softening, mechanical peeling, screening, air separation, magnetic separation, gravity separation, alkaline washing or surface cleaning. S4, perform aluminum back electrode pre-removal or passivation treatment on the pre-treated solar cells; S5, the aluminum-treated battery cells are added to a silver selective leaching solution, allowing the metallic silver in the silver grid lines to enter the solution and form a silver-containing leaching solution; the silver selective leaching solution adopts an acidic oxidation leaching system or an alkaline silver ammonia complex leaching system; the acidic oxidation leaching system includes nitric acid, methanesulfonic acid, organic acids or combinations thereof, and is combined with one or more of hydrogen peroxide, dissolved oxygen, ferric salts, persulfates or electrochemical oxidation systems; the alkaline silver ammonia complex leaching system includes ammonia and hydrogen peroxide. When the acidic oxidative leaching system uses nitric acid-hydrogen peroxide, the nitric acid concentration is 0.1–4 mol / L, H2O2 is added in batches, the reaction temperature is 20–70℃, the reaction time is 10–180 min, and the liquid-to-solid ratio is 5–50 mL / g. When the alkaline silver ammonia complex leaching system uses ammonia-hydrogen peroxide, the ammonia concentration is 0.5–5 mol / L, H2O2 is added in batches, the pH is 9–12, the reaction temperature is 15–50℃, the reaction time is 10–90 min, and the liquid-to-solid ratio is 5–50 mL / g.

[0031] S6, perform solid-liquid separation to obtain silver-containing leachate and low-silver silicon residue; S7, perform impurity detection and threshold judgment on the silver-containing leachate. When the concentration of one or more impurities among Al, Cu, Pb, and Sn exceeds the set threshold, start the silver-containing liquid purification step to reduce the impurity concentration. S8, perform electrochemical testing on the purified or regulated silver-containing leachate to determine the potential window in which silver preferentially deposits and impurity co-deposition is suppressed; the electrochemical testing includes one or more of cyclic voltammetry, linear sweep voltammetry, chronoamperometry, or chronopotentiometrics; the electrochemical testing is at least used to determine the reduction peak or reduction initiation potential of silver species in the silver-containing leachate, the co-deposition potential of impurity ions, and the potential range in which silver preferentially deposits and impurity co-deposition is suppressed.

[0032] S9, electrodeposition is performed within the potential window to reduce and deposit silver as metallic silver on the cathode surface; the electrodeposition adopts constant potential, constant current, pulse electrodeposition or stepped potential electrodeposition method; the cathode material is stainless steel, titanium plate, graphite, carbon felt, carbon cloth, conductive carbon material or its surface modified material; the anode material is titanium-based coated anode, graphite anode or platinum-titanium anode.

[0033] S10, the silver-poor solution after electrodeposition is returned to the silver selective leaching step for recycling after composition adjustment.

[0034] The composition adjustment of the silver-poor solution includes at least one of the following operations: stopping electrodeposition when the Ag concentration is below the electrodeposition endpoint threshold; replenishing acid, ammonia, or complexing agent concentrations when they are below the required leaching range; replenishing oxidant or performing electrochemical re-oxidation when the redox potential is below the required silver leaching range; initiating bypass purification when Al, Cu, Pb, Sn, or Fe impurity ions exceed the circulation threshold; and partially draining and refreshing the mother liquor when the number of mother liquor circulations reaches a set value.

[0035] This invention discloses a method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control. By using raw material composition detection as a pre-processing step, it solves the fundamental problem of unstable recycling results caused by using fixed leaching schemes due to the complex sources and large differences in element content of waste cells in existing technologies. This method dynamically determines the removal methods for residual adhesive and solder ribbon, the pretreatment intensity of the aluminum back electrode, the selection of the silver leaching system, and the impurity control strategy before electrodeposition based on the detected content of key elements such as Ag, Al, Cu, Pb, and Sn. This allows the same method framework to adapt to waste cell materials of different grades and sources, avoiding a decrease in silver leaching rate or deterioration of silver product purity due to material fluctuations. Furthermore, by judging the impurity threshold of the silver-containing leaching solution and selectively initiating purification steps, intervention is only performed when the impurity concentration reaches a level that affects the electrodeposition effect. This ensures the quality of the silver-containing solution entering the electrodeposition unit while avoiding reagent waste and silver loss due to excessive purification, achieving a balance between impurity control effectiveness and operating costs. This method introduces an electrochemical testing step before silver electrodeposition for recovery, characterizing the actual silver-containing leaching solution using voltammetry. This precisely determines the potential window where silver preferentially deposits while co-deposition of impurities such as copper, lead, and tin is suppressed, rather than using a preset fixed potential or current density. This allows the electrodeposition process to adapt to the differences in silver species morphologies in different leaching systems (acidic silver ion systems or alkaline silver ammonia complex systems), ensuring high selectivity and high current efficiency in silver deposition from an electrochemical perspective. The resulting silver product has significantly improved purity, and the deposited layer is dense and easy to peel off. Furthermore, the silver-poor solution after electrodeposition is not directly discharged but is recycled back to the silver leaching step after composition adjustment. Combined with a bypass purification mechanism to remove impurities accumulated during the recycling process, a closed-loop recycling system is formed. This significantly reduces the consumption of acids, alkalis, oxidants, and complexing agents, and reduces the generation and discharge of heavy metal-containing wastewater, demonstrating good environmental friendliness. In addition, the silver, aluminum, copper, lead, tin and other metal content in the low-silver silicon residue after silver leaching and washing is significantly reduced. It can be used as a raw material for silicon powder, metallurgical silicon, silicon-based composite materials or for further purification to prepare high-purity silicon. This realizes the synergy between silver recovery and silicon resource utilization, and enhances the economic value of the overall resource utilization of waste crystalline silicon photovoltaic modules.

[0036] The present invention will be described in detail below with reference to specific embodiments: Example 1 This embodiment provides a method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control, including the following steps.

[0037] Step 1: Raw material grading and cell enrichment Dismantle waste crystalline silicon photovoltaic modules, remove aluminum frames, junction boxes, glass, backsheets and encapsulation films to obtain crystalline silicon cells or cell fragments containing silver grid lines.

[0038] Furthermore, the obtained materials are classified into at least the following categories: (1) silver-rich silicon wafers mainly composed of crystalline silicon solar cells; (2) mixed materials containing a large amount of solder strips, busbars or metal connectors; and (3) non-target components such as glass, backsheets, and encapsulants.

[0039] Silver-rich silicon wafers are given priority in the selective leaching process of silver grid lines; for mixtures containing a large amount of solder ribbon, mechanical sorting, shearing separation, sieving, air classification, density sorting or other metal separation treatments are given priority.

[0040] Step 2: Raw material composition detection and process route determination Composition analysis is performed on the battery cell materials entering the wet recycling process, with at least Si, Ag, Al, Cu, Pb, and Sn being analyzed. This composition analysis can employ XRF, ICP-OES, ICP-MS, AAS, chemical titration, or a combination thereof. The test results are used to determine the subsequent process route. When the Al content is higher than the set threshold, the aluminum back electrode is pre-removed or passivated first; in a preferred example, Al > 6wt% can be used as the reference threshold for starting the enhanced aluminum removal process. When the contents of Cu, Pb, and Sn are higher than the set threshold, the solder strip strengthening separation is performed first, or an impurity control step is set before silver electrodeposition. When the Ag content is high and the solder ribbon residue is low, the silver selective leaching step is preferentially initiated. When the residual adhesive content in the battery cells is high, the residual adhesive should be removed first to avoid organic matter affecting the stability of the leachate and the electrodeposition process.

[0041] The threshold can be determined based on different batches of materials, the purity of the target silver product, and the utilization direction of silicon residue. As a preferred control method, the following logic can be adopted: When the Al content increases, the intensity of the aluminum removal pretreatment should be increased or the aluminum removal time should be extended. When the content of Cu, Pb and Sn increases, add a solder strip sorting step or start the pre-electrode deposition purification unit. When the Ag content is low, silver-rich component sorting, multi-stage countercurrent leaching, circulating leaching, or leachate enrichment methods should be used to increase the concentration of silver-containing solution. If necessary, the silver leaching rate can be further improved by optimizing the liquid-solid ratio, extending the leaching time, or improving the mass transfer efficiency. When the target application of silicon residue has high requirements, washing, secondary purification or shallow etching steps can be added.

[0042] Step 3: Removal of residual adhesive and solder ribbon The battery cell material obtained in step one is pretreated to remove residual EVA / POE film, copper solder strips, tin-lead solder and mechanical inclusions.

[0043] The pretreatment method includes one or more of the following: heat treatment, swelling and softening, mechanical stripping, sieving, air separation, magnetic separation, gravity separation, alkaline washing, or surface cleaning. Preferably, after pretreatment, the silver grid lines are exposed on the surface of the solar cell, and solder ribbons and obvious metal connectors are removed as much as possible to reduce the interference of Cu, Pb, and Sn on the silver electrodeposition process.

[0044] Step 4: Pre-removal or passivation treatment of aluminum back electrode The pretreated crystalline silicon solar cells are placed in an aluminum selective removal solution to preferentially remove or passivate the aluminum back electrode on the back of the cells. The aluminum selective removal solution can be an acidic or alkaline system. As a preferred method, a hydrochloric acid system can be used to remove aluminum; as another preferred method, a sodium hydroxide or potassium hydroxide system can be used to remove aluminum.

[0045] Preferably, the acidic dealuminization conditions are: hydrochloric acid mass fraction of 2%–10%; temperature of 15–60℃; treatment time of 1–4h; and liquid-to-solid ratio of 5–50mL / g.

[0046] Preferably, the alkaline aluminum removal conditions are: NaOH or KOH concentration of 10–100 g / L; temperature of 20–80 °C; treatment time of 10–90 min; and liquid-to-solid ratio of 5–50 mL / g.

[0047] Step 5: Selective leaching of silver grid lines The pretreated battery cells are added to a silver selective leaching solution, causing the metallic silver in the silver grid lines to oxidize and enter the solution, forming silver ions, silver complexes, or other electrochemically recoverable silver species. This invention preferably employs one of the following two silver leaching routes, the specific route being determined by the raw material composition detection results in step S2 and the suitability for subsequent electrodeposition.

[0048] Route A: Acidic Oxidative Leaching System The acidic oxidative leaching system includes nitric acid, methanesulfonic acid, organic acids or combinations thereof, and is combined with one or more of hydrogen peroxide, dissolved oxygen, ferric salts, persulfates or electrochemical oxidation systems.

[0049] Preferably, when using the nitric acid-hydrogen peroxide system, the nitric acid concentration is 0.1–4 mol / L, H2O2 is added in batches according to the ORP or reaction rate, the reaction time is 10–180 min, and the liquid-to-solid ratio is 5–50 mL / g. When using the HNO3 / H2O2 system, the preferred temperature is 20–70℃, more preferably 25–60℃; H2O2 should be added in batches or continuously at a low rate, and temperature monitoring, exhaust gas control, and excess oxidant control should be implemented. If the temperature exceeds 70℃, the H2O2 addition rate should be reduced or another oxidation system should be used.

[0050] Route B: Alkaline silver ammonia complex leaching system The alkaline silver ammonia complex leaching system includes ammonia and hydrogen peroxide, and achieves selective silver leaching by oxidizing silver and forming a soluble silver ammonia complex.

[0051] Preferably, the ammonia concentration is 0.5–5 mol / L, H2O2 is added in batches, the pH is 9–12, the temperature is 15–50℃, the reaction time is 10–90 min, and the liquid-to-solid ratio is 5–50 mL / g. This route should not be mixed with strongly acidic leaching systems, and measures should be implemented to control ammonia volatilization, control reaction temperature rise, and add hydrogen peroxide in batches.

[0052] Silver ammonia complex leaching solution, its filtration residue, and electrode surface residues should be kept moist and promptly introduced into the electrodeposition or waste liquid stabilization treatment process to avoid long-term exposure of silver ammonia residues and subsequent drying and accumulation after ammonia volatilization. Waste liquids should undergo acidification, complexation stabilization, or other safe conversion treatments before disposal to prevent the formation of unstable silver-containing deposits.

[0053] Step 6, Leaching endpoint control The silver leaching process is endpoint-determined using pH, ORP, conductivity, Ag concentration, and reaction time. Preferably, the leaching endpoint meets any of the following conditions: the rate of change of Ag concentration in the leachate is below a set threshold; the silver grid lines on the cell surface essentially disappear; the Ag leaching rate reaches a set target value; ORP or conductivity enters a stable range; or the reaction time reaches a preset upper limit.

[0054] In acidic systems, the ORP reference range is calibrated through preliminary experiments based on the reference electrode and leaching system used; in silver ammonia complex systems, Ag leaching rate, pH, residual H2O2, and ammonia concentration should be used as control indicators.

[0055] Step 7: Solid-liquid separation and washing of silicon residue After silver leaching, the reaction system undergoes solid-liquid separation to obtain a silver-containing leachate and low-silver silicon residue. The solid-liquid separation methods include filtration, centrifugation, sedimentation, sieving, or membrane separation. The silicon residue is subjected to multi-stage washing to recover the silver-containing leachate entrained on its surface. The washing solution is returned to the silver leaching solution or enters the subsequent electrodeposition unit.

[0056] Preferably, the content of Ag, Al, Cu, Pb, and Sn in the low-silver silicon residue is significantly reduced, and it can be used as a raw material for silicon powder, metallurgical silicon, silicon-based composite materials, or for further purification to prepare high-purity silicon.

[0057] Step 8: Impurity Threshold Control and Purification of Silver-Containing Leachate Impurity detection and threshold determination are performed on the silver-containing leachate. The detection targets include one or more of Ag, Al, Cu, Pb, Sn, and Fe. When the concentration of Al, Cu, Pb, Sn, or Fe exceeds the set threshold, or when the concentration reaches a level that affects the purity, current efficiency, or morphology of the silver electrodeposition layer, the silver-containing solution purification step is initiated.

[0058] The impurity control methods include pH-adjusted precipitation, ion exchange, adsorption, membrane separation, extraction, or stepwise electrochemical treatment without significant silver loss. For systems containing Cl- or prone to silver precipitation, non-target silver loss in the form of AgCl, Ag2O, etc., should be avoided unless the precipitation step is designed as part of the silver recovery process.

[0059] Electrochemical pretreatment can be used to adjust the redox state of silver-containing solutions, or to remove easily co-deposited impurities if a selective window is confirmed by voltammetry testing; otherwise, ion exchange, adsorption, precipitation, extraction, or membrane separation should be used to reduce the concentration of impurities such as Cu, Pb, and Sn.

[0060] Preferably, the impurity threshold is not a fixed absolute value, but is determined based on the purity of the target silver product, the leaching system used, the electrodeposition window, and the number of mother liquor cycles. For applications requiring high-purity silver products, the concentrations of Pb, Cu, and Sn entering the electrodeposition unit should be reduced; for the circulating mother liquor, an upper limit for impurity accumulation should be set, and bypass purification or partial drainage and replacement should be initiated once the upper limit is exceeded.

[0061] Step 9: Determining the electrochemical selective deposition window Before electrodeposition to recover silver, electrochemical tests are performed on the purified or controlled silver-containing leachate to determine the potential window in which silver preferentially deposits and impurity co-deposition is suppressed. The electrochemical tests include cyclic voltammetry, linear sweep voltammetry, chronoamperometry, chronopotentiometry, or combinations thereof.

[0062] Electrochemical tests are used to determine at least the following: reduction peaks or reduction initiation potentials of silver species in silver-containing leachates; possible co-deposition potentials of impurity ions such as Cu, Pb, and Sn; variations in the silver deposition potential window under different pH, complexing agent concentrations, Ag concentrations, and impurity concentrations; the potential range in which silver preferentially deposits and impurity co-deposition is suppressed; and the range of parameters suitable for constant potential, constant current, pulse electrodeposition, or step potential electrodeposition.

[0063] For acidic Ag+ systems, the potential range for Ag+ reduction to Ag0 can be determined by voltammetry; for silver ammonia complex systems, the potential range for the reduction of silver ammonia complex to Ag0 at the cathode surface can be determined by voltammetry. The actual electrodeposition potential is not preset to a fixed value, but should be calibrated based on the leaching solution composition, electrode material, reference electrode system, and impurity concentration.

[0064] Step 10: Electrodeposition to recover silver The silver-containing leaching solution with the determined electrochemical window is sent into the electrodeposition tank, and electrodeposition is carried out within the silver preferential deposition potential window, so that silver is reduced and deposited as metallic silver on the cathode surface.

[0065] For acidic silver ion systems, the electrodeposition reaction can be represented as: Ag++e-→Ag0. For silver-ammonia complex systems, the electrodeposition process involves the reduction of the silver complex to metallic silver on the cathode surface; the actual reaction pathway depends on the complex morphology, pH, and electrode material.

[0066] Preferably, the electrodeposition tank includes a cathode, an anode, an electrolyte circulation system, a temperature control system, and an online detection system. The cathode material can be stainless steel, titanium plate, graphite, carbon felt, carbon cloth, conductive carbon material, or its surface-modified material; the anode material can be a titanium-based coated anode, a graphite anode, a platinum-titanium anode, or other inert anodes.

[0067] Preferably, the electrodeposition method is constant potential, constant current, pulsed electrodeposition, or stepped potential electrodeposition. More preferably, the electrodeposition parameters are determined by: determining the silver preferential deposition potential window by voltammetry; determining the morphology and peelability of the silver deposition layer by short-time electrodeposition experiments; determining the optimal current density or pulse parameters by current efficiency and silver product purity; determining the electrodeposition endpoint by Ag residual concentration; and correcting the potential window or initiating front-end purification by Cu, Pb, and Sn co-deposition conditions.

[0068] Preferably, when using pulse electrodeposition, concentration polarization is reduced and the density and peelability of the silver deposition layer are improved by adjusting the pulse current density, energizing time, energizing time, and duty cycle.

[0069] Step 11: Regeneration and Recycling of Silver-Lean Solution After electrodeposition, the silver-poor solution is subjected to pH, ORP, acid concentration, ammonia concentration, complexing agent concentration, Ag concentration, and impurity ion concentration tests, and then regenerated according to the set logic.

[0070] Electrodeposition is stopped when the Ag concentration falls below the electrodeposition endpoint threshold. When the acid concentration, ammonia concentration, or complexing agent concentration is below the required leaching range, it should be added; When the ORP is below the range required for silver leaching, add oxidant or perform electrochemical re-oxidation. When impurity ions such as Al, Cu, Pb, Sn, or Fe exceed the circulation threshold, bypass purification is initiated. When the number of mother liquor circulations reaches the set value and impurities cannot be effectively controlled, partial drainage and replacement will be performed.

[0071] This forms a closed-loop recovery system consisting of "raw material testing, route determination, selective leaching, impurity threshold control, electrochemical window determination, electrodeposition recovery, silver-poor solution regeneration, and mother liquor recycling".

[0072] Example 2 This embodiment first involves acid removal of aluminum, followed by acid immersion in silver and electrodeposition to recover silver, including the following steps: Dismantle and delaminate waste crystalline silicon photovoltaic modules to obtain solar cells containing silver grid lines; The contents of Ag, Al, Cu, Pb and Sn were determined by composition analysis, and surface residues, solder ribbons and mechanical inclusions were removed. When the Al content is higher than a set threshold, aluminum back electrode pretreatment is performed; in a preferred example, when Al > 6 wt%, enhanced dealuminization treatment is initiated. Treatment with 2%–10% HCl at 15–60℃ for 1–4 h preferentially removes the aluminum back electrode, achieving an Al extraction rate of 98.6%. The silver grid wires were leached using HNO3, HNO3 / H2O2, methanesulfonic acid / oxidant, or other acidic oxidation systems, achieving an Ag extraction rate of 99.2%. Solid-liquid separation yielded a silver-containing leachate and a low-silver silicon residue with a silicon purity of 99.83%. Determine and purify the impurity thresholds of silver-containing leachate, including Pb, Cu, and Sn. The silver preferential deposition potential window was determined by cyclic voltammetry or linear sweep voltammetry. Silver was recovered using constant potential, constant current, or pulse electrodeposition methods, with Ag purity > 99.5% and overall Ag recovery rate of 95.7%. The silver-depleted solution after electrodeposition is recycled after being replenished with acid and oxidant and purified by bypass.

[0073] Example 3 This embodiment first performs alkaline aluminum removal, then silver is leached with silver ammonia complexation and recovered by electrodeposition, including the following steps: Dismantle and delaminate waste crystalline silicon photovoltaic modules to obtain solar cells containing silver grid lines; The contents of Ag, Al, Cu, Pb, and Sn were determined by compositional analysis; within a sample composition reference range, Si is typically about 84–94 wt%, Al about 3–14 wt%, and Ag about 0.03–1.95 wt%. Remove surface residue, solder ribbon, and mechanical inclusions; When the Al content is higher than a set threshold, aluminum back electrode pretreatment is performed; in a preferred example, when Al > 6 wt%, enhanced dealuminization treatment is initiated. Treatment with NaOH or KOH alkaline solution at 20–80℃ for 10–90 min preferentially removes the aluminum back electrode, with an actual Al extraction rate of 96.5%. Wash with water until near neutral, and control silicon loss rate; The silver grid lines were selectively leached using an NH3 / H2O2 system at pH 9–12 and 15–50℃, with an actual Ag extraction rate of 95.3%. Solid-liquid separation yields a silver-containing ammonia complex solution and a low-silver silicon residue. The silver-containing solution was filtered, impurity thresholds were determined and purified, and the silver-containing ammonia residue was subjected to wet transfer and stabilization treatment. The potential window for the preferential reduction of silver ammonia complex to metallic silver was determined by cyclic voltammetry or linear sweep voltammetry. Within this window, metallic silver was recovered using either constant potential or pulse electrodeposition, with an overall Ag recovery rate of 92.3% as measured. The silver-poor ammonia solution after electrodeposition is recycled after adjusting the ammonia concentration, H2O2 dosage, and impurity concentration.

[0074] This invention also discloses a waste crystalline silicon photovoltaic cell recycling system based on impurity threshold control using the above method, comprising: An impurity detection unit is used to detect impurities in silver-containing leachate, and the elements to be detected include at least Al, Cu, Pb and Sn; The threshold judgment and control unit is connected to the impurity detection unit and is used to receive the impurity detection results. When the concentration of one or more impurities among Al, Cu, Pb, and Sn exceeds the set threshold, a purification start signal is issued. A purification unit, connected to the threshold judgment and control unit, is used to initiate the silver-containing liquid purification step after receiving the purification start signal, so as to reduce the impurity concentration; The electrochemical testing unit is used to perform electrochemical tests on purified or unpurified silver-containing leachates to determine the potential window in which silver preferentially deposits and impurity co-deposition is suppressed. An electrodeposition unit, connected to the electrochemical testing unit, is used to perform electrodeposition within the potential window, so that silver is reduced and deposited as metallic silver on the cathode surface.

[0075] This invention discloses a waste crystalline silicon photovoltaic cell recycling system based on impurity threshold control. Through the coordinated operation of multiple functional units, it achieves efficient purification and selective electrodeposition recovery of silver-containing leachate, significantly improving the automation, controllability, and economy of the silver recovery process. The system first utilizes an impurity detection unit to rapidly detect key impurity elements in the silver-containing leachate, covering at least aluminum, copper, lead, and tin. This accurately determines the composition and concentration distribution of impurities in the leachate, providing a reliable data foundation for subsequent purification decisions. The threshold judgment and control unit, based on the detection results, determines in real time whether the concentration of each impurity exceeds a set threshold. When the threshold is exceeded, it automatically issues a purification start signal, effectively avoiding the lag and uncertainty of manual judgment and ensuring the timeliness and targeted nature of the purification process. Upon receiving the start signal, the purification unit selectively initiates purification steps, rather than indiscriminately purifying all leachate. This on-demand purification strategy effectively reduces the consumption of purification reagents and operation time, lowers processing costs, and avoids interference from over-purification of the silver-containing leachate system. The electrochemical testing unit precisely determines the potential window where silver preferentially deposits and impurity co-deposition is suppressed by performing electrochemical tests on purified or unpurified silver-containing leaching solutions. This provides optimal electrodeposition parameters for the leaching solution under specific compositional conditions, ensuring that silver ions are preferentially reduced at the cathode surface during electrodeposition, while impurities such as aluminum, copper, lead, and tin are suppressed and difficult to co-deposit, thus guaranteeing the purity of the deposited silver product. Operating within this potential window, the electrodeposition unit efficiently reduces silver ions to metallic silver at the cathode surface, achieving efficient separation of silver from impurities. The deposited product meets the quality requirements of high-purity silver products without further deep purification. The entire system forms a complete closed-loop control chain of "detection—judgment—purification—testing—deposition," with accurate signal transmission and timely action responses between units. This avoids the problem of decreased purity of electrodeposited silver due to excessive impurities and prevents unnecessary over-purification that could lead to silver loss. While ensuring the quality of recovered silver, it maximizes the direct recovery rate and resource utilization efficiency, resulting in significant environmental and economic benefits. It is suitable for large-scale application in the recycling and processing of waste crystalline silicon photovoltaic cells. Meanwhile, when dealing with waste photovoltaic cells from different sources and batches, the system can flexibly switch working modes according to the actual impurity status of the leachate. For leachate with impurity concentrations within the standard, it can directly enter the electrodeposition stage, improving processing efficiency. For leachate with impurity concentrations exceeding the standard, it automatically triggers the purification and retesting process, ensuring the system's adaptability and the stability of the processing effect.

[0076] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control, characterized in that, Includes the following steps: Dismantle waste crystalline silicon photovoltaic modules, remove non-cell components, and obtain crystalline silicon cell material containing silver grid lines; The composition of the battery cell material is analyzed, and the elements to be tested include at least Ag, Al, Cu, Pb and Sn. The subsequent process route is determined based on the test results. The battery cell material is pretreated to remove residual adhesive and solder ribbon residue; The pre-treated solar cells undergo aluminum back electrode pre-removal or passivation treatment. The aluminum-treated battery cells are added to a silver selective leaching solution, allowing the metallic silver in the silver grid lines to enter the solution and form a silver-containing leaching solution. Solid-liquid separation was performed to obtain a silver-containing leachate and a low-silver silicon residue; The silver-containing leachate is subjected to impurity detection and threshold determination. When the concentration of one or more impurities among Al, Cu, Pb, and Sn exceeds a set threshold, the silver-containing solution purification step is initiated to reduce the concentration of the impurities. Electrochemical tests were performed on the purified or regulated silver-containing leachate to determine the potential window in which silver preferentially deposits and impurity co-deposition is suppressed. Electrodeposition is performed within the potential window, causing silver to be reduced and deposited as metallic silver on the cathode surface; The silver-poor solution after electrodeposition is adjusted in composition and then returned to the silver selective leaching step for recycling.

2. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 1, characterized in that, The composition detection employs one or more of XRF, ICP-OES, ICP-MS, AAS, or chemical titration; the process route determination includes at least one of the following decision logics: When the Al content is higher than the set threshold, the aluminum back electrode is first pre-removed or passivated. When the contents of Cu, Pb, and Sn are higher than the set threshold, the solder strip strengthening separation is performed first, or an impurity control step is set before silver electrodeposition. When the residual adhesive content is high, the residual adhesive should be removed first; When the Ag content is low, silver-rich component sorting, multi-stage countercurrent leaching, circulating leaching, or leachate enrichment methods can be used to increase the concentration of silver-containing solution.

3. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 2, characterized in that, The pre-removal or passivation treatment of the aluminum back electrode adopts an acidic or alkaline system. The conditions for the acidic system are: hydrochloric acid mass fraction of 2% to 10%, temperature of 15 to 60°C, treatment time of 1 to 4 hours, and liquid-to-solid ratio of 5 to 50 mL / g. The conditions for the alkaline system are: NaOH or KOH concentration of 10 to 100 g / L, temperature of 20 to 80°C, treatment time of 10 to 90 minutes, and liquid-to-solid ratio of 5 to 50 mL / g.

4. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 1, characterized in that, The pretreatment includes one or more of the following: heat treatment, swelling and softening, mechanical peeling, sieving, air separation, magnetic separation, gravity separation, alkaline washing, or surface cleaning; The composition adjustment of the silver-poor solution includes at least one of the following operations: stopping electrodeposition when the Ag concentration is below the electrodeposition endpoint threshold; replenishing acid, ammonia, or complexing agent concentrations when they are below the required leaching range; replenishing oxidant or performing electrochemical re-oxidation when the redox potential is below the required silver leaching range; initiating bypass purification when Al, Cu, Pb, Sn, or Fe impurity ions exceed the circulation threshold; and partially draining and refreshing the mother liquor when the number of mother liquor circulations reaches a set value.

5. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 1, characterized in that, The selective silver leaching solution employs an acidic oxidative leaching system or an alkaline silver ammonia complex leaching system; the acidic oxidative leaching system includes nitric acid, methanesulfonic acid, organic acids or combinations thereof, and is combined with one or more of hydrogen peroxide, dissolved oxygen, ferric salts, persulfates or electrochemical oxidation systems; the alkaline silver ammonia complex leaching system includes ammonia and hydrogen peroxide.

6. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 5, characterized in that, When the acidic oxidative leaching system uses nitric acid-hydrogen peroxide, the nitric acid concentration is 0.1–4 mol / L, H2O2 is added in batches, the reaction temperature is 20–70℃, the reaction time is 10–180 min, and the liquid-to-solid ratio is 5–50 mL / g. When the alkaline silver ammonia complex leaching system uses ammonia-hydrogen peroxide, the ammonia concentration is 0.5–5 mol / L, H2O2 is added in batches, the pH is 9–12, the reaction temperature is 15–50℃, the reaction time is 10–90 min, and the liquid-to-solid ratio is 5–50 mL / g.

7. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 1, characterized in that, The impurity control methods include one or more of pH-adjusted precipitation, ion exchange, adsorption, membrane separation, extraction, or stepwise electrochemical treatment; the set threshold is determined based on the purity of the target silver product, the type of leaching system, the electrodeposition window, and the number of mother liquor cycles.

8. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 1, characterized in that, The electrochemical tests include one or more of cyclic voltammetry, linear sweep voltammetry, chronoamperometry, or chronopotentialometry; the electrochemical tests are at least used to determine the reduction peak or reduction initiation potential of silver species in silver-containing leachates, the co-deposition potential of impurity ions, and the potential range in which silver preferentially deposits and impurity co-deposition is suppressed.

9. The method for recycling waste crystalline silicon photovoltaic cells based on impurity threshold control according to claim 1, characterized in that, The electrodeposition is performed using constant potential, constant current, pulse electrodeposition, or stepped potential electrodeposition methods; the cathode material is stainless steel, titanium plate, graphite, carbon felt, carbon cloth, conductive carbon material, or its surface-modified material; the anode material is titanium-based coated anode, graphite anode, or platinum-titanium anode.

10. A waste crystalline silicon photovoltaic cell recycling system based on impurity threshold control using the method of any one of claims 1-9, characterized in that, include: An impurity detection unit is used to detect impurities in silver-containing leachate, and the elements to be detected include at least Al, Cu, Pb and Sn; The threshold judgment and control unit is connected to the impurity detection unit and is used to receive the impurity detection results. When the concentration of one or more impurities among Al, Cu, Pb, and Sn exceeds the set threshold, a purification start signal is issued. A purification unit, connected to the threshold judgment and control unit, is used to initiate the silver-containing liquid purification step after receiving the purification start signal, so as to reduce the impurity concentration; The electrochemical testing unit is used to perform electrochemical tests on purified or unpurified silver-containing leachates to determine the potential window in which silver preferentially deposits and impurity co-deposition is suppressed. An electrodeposition unit, connected to the electrochemical testing unit, is used to perform electrodeposition within the potential window, so that silver is reduced and deposited as metallic silver on the cathode surface.