Modified waste incineration fly ash and preparation method thereof

By modifying the preparation method of waste incineration fly ash, using a solvent and modifier to chelate heavy metals, and nano-titanium dioxide catalyst to degrade dioxins, the stability and degradation problems of fly ash treatment in the existing technology are solved, and low-cost and efficient harmless treatment of fly ash is achieved.

CN123149237APending Publication Date: 2026-11-24SHANGHAI JINTANG TEXTILE NEW MATERIALS TECHCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611399149.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-24

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a modified waste incineration fly ash and its preparation method, relating to the field of solid waste treatment and resource utilization technology. The raw materials include: fly ash, water, a solvent, a modifier, a neutralizing agent, and an oxidation catalyst. The preparation method includes: adding fly ash to water and stirring to obtain a fly ash slurry; treating the fly ash slurry sequentially with a solvent, a modifier, and a neutralizing agent, then filtering by pressure to obtain a filtrate and a solid filter cake; mixing the solid filter cake with water, stirring, adding the oxidation catalyst, stirring again, filtering by pressure, and drying to obtain the modified waste incineration fly ash. The modified waste incineration fly ash of this invention has the advantages of low heavy metal leaching concentration and high dioxin degradation rate, and the preparation method is simple and suitable for industrial production, providing a new approach for green and environmentally friendly waste incineration fly ash treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid waste treatment and resource utilization technology, specifically to a modified waste incineration fly ash and its preparation method. Background Technology

[0002] With the continuous improvement of the harmless treatment system for municipal solid waste, waste-to-energy incineration has become the mainstream method of municipal solid waste disposal due to its significant advantages in volume reduction, harmlessness, and resource recovery. During waste incineration, the flue gas purification system collects a large amount of fine particulate matter, namely fly ash, which accounts for approximately 3-5% of the total waste incineration output. As a core byproduct of waste incineration, fly ash is enriched with various toxic and harmful pollutants from the waste, including easily leached heavy metals such as lead, cadmium, mercury, and chromium, as well as highly toxic and persistent dioxin-like organic pollutants. If not effectively treated and directly dumped or landfilled, heavy metals will leach into the soil and groundwater with rainwater, and dioxins can persist in the ecological environment for a long time, harming the human nervous and endocrine systems through bioaccumulation, seriously threatening ecological security and human health.

[0003] Currently, the mainstream methods for harmless treatment of fly ash in the industry mainly include chemical solidification, cement kiln co-processing, and high-temperature pyrolysis. However, their practical applications all have significant technical shortcomings and limitations. Among them, traditional chemical solidification technology can only achieve simple heavy metal encapsulation and fixation, but it has no effect on degrading dioxins in fly ash. After treatment, highly toxic dioxin components still remain in the fly ash, making it unable to escape its hazardous waste status. Landfilling occupies land resources and poses a long-term risk of secondary pollution. Although high-temperature pyrolysis, melting, and other heat treatment processes can degrade dioxins, they involve large equipment investments, high operating energy consumption, and expensive treatment costs. Moreover, dioxin de novo resynthesis reactions are prone to occur under high-temperature conditions, resulting in poor degradation effects. Cement kiln co-processing is limited by operating conditions and blending ratios, resulting in a limited treatment scale, which is difficult to meet the needs of large-scale harmless treatment of fly ash. It also has problems such as pollutant migration and impact on product quality. Overall, existing fly ash treatment technologies generally suffer from drawbacks such as poor stability of heavy metal solidification, incomplete dioxin removal, high treatment costs, and easy generation of secondary pollution. These shortcomings make it difficult to achieve the complete transformation of fly ash from hazardous waste to general solid waste, thus hindering the green and sustainable development of the waste incineration industry.

[0004] Therefore, in order to solve the many drawbacks of existing technologies and break through the technical bottleneck of fly ash harmless treatment, it is urgent to develop a low-cost, high-efficiency, and non-secondary pollution-free fly ash co-process for harmless treatment. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention provides a modified waste incineration fly ash and its preparation method.

[0006] The objective of this invention can be achieved through the following technical solutions: A method for preparing modified waste incineration fly ash includes the following steps: Step (1): Add fly ash to water and stir to obtain fly ash slurry. Add a solvent to the fly ash slurry and stir. Then add a modifier and continue stirring to obtain modified fly ash slurry. Add a neutralizer to the modified fly ash slurry, adjust the pH, stir, and filter under pressure to obtain filtrate and solid filter cake. Step (2): Mix the solid filter cake and water, stir to obtain a composite slurry, add an oxidation catalyst to the composite slurry, stir, filter under pressure, and dry to obtain modified waste incineration fly ash.

[0007] Furthermore, the preparation method of modified waste incineration fly ash includes the following specific steps: Step (1): Add fly ash to water and stir for 5-10 minutes to obtain fly ash slurry. Add a solvent to the fly ash slurry and stir for 15-20 minutes. Then add a modifier and continue stirring for 1-1.5 hours to obtain modified fly ash slurry. Add a neutralizer to the modified fly ash slurry to adjust the pH to 9.5-10.5. Stir for 40-50 minutes and filter under pressure to obtain filtrate and solid filter cake. Step (2): Mix the solid filter cake and water, stir for 10-15 minutes to obtain a composite slurry, add an oxidation catalyst to the composite slurry, stir for 2-3 hours, filter by pressure, and dry the obtained filter cake at 75-80℃ for 12-13 hours to obtain modified waste incineration fly ash.

[0008] Furthermore, the amount of the co-solvent added is 2-3% of the fly ash mass; the co-solvent is prepared by mixing citric acid, sodium bicarbonate and deionized water in a ratio of 3-5g: 1-2g: 93-96mL.

[0009] Furthermore, the preparation method of the modifier includes the following steps: Deionized water, sodium citrate, and sodium diethyldithiocarbamate were mixed and stirred to obtain a premixed solution. Sodium metasilicate was prepared into a sodium metasilicate solution and added dropwise to the premixed solution. The mixture was heated and stirred, then cooled to obtain mixture 1. Calcined kaolin was added to mixture 1 and ultrasonically dispersed under stirring conditions. The mixture was then allowed to stand and mature to obtain a modifier.

[0010] Furthermore, the preparation method of the modifier includes the following specific steps: Deionized water, sodium citrate, and sodium diethyldithiocarbamate were mixed and stirred for 20-25 minutes to obtain a premix. Sodium metasilicate was prepared into a sodium metasilicate solution and added dropwise to the premix. The addition of the sodium metasilicate solution was completed within 20-30 minutes. The mixture was heated to 45-50℃ and stirred for 30-35 minutes. After cooling, a mixture 1 was obtained. Calcined kaolin was added to mixture 1 and ultrasonically dispersed under stirring conditions for 40-45 minutes. The mixture was then allowed to stand for 1-1.2 hours to mature, thus obtaining the modifier.

[0011] Furthermore, the ratio of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin is 46-57 mL: 5-7 g: 14-16 g: 9-11 g: 15-20 g.

[0012] Furthermore, the method for preparing the sodium metasilicate solution is as follows: add sodium metasilicate to deionized water and stir for 10-15 minutes to obtain the sodium metasilicate solution; in the sodium metasilicate solution, the ratio of sodium metasilicate to deionized water is 9-11g:20-25mL.

[0013] Furthermore, the amount of modifier added is 4-6% of the fly ash mass; the neutralizing agent is prepared by mixing calcium hydroxide, magnesium sulfate, and deionized water in a dosage ratio of 8-12g: 2-3g: 85-90mL.

[0014] Furthermore, in the composite slurry, the ratio of solid filter cake to water is 25-26 g: 100 mL; the amount of oxidation catalyst added is 5-7% of the fly ash mass in step (I).

[0015] Furthermore, the preparation method of the oxidation catalyst includes the following steps: Nano-titanium dioxide was dried, cooled, and sieved to obtain pretreated nano-titanium dioxide. Deionized water and oxalic acid were mixed and stirred. Ferrous sulfate was added and stirred continuously. The pretreated nano-titanium dioxide was added in batches, heated, and ultrasonically dispersed under stirring conditions. After cooling, sodium persulfate was added, stirred, and allowed to stand for aging to obtain an oxidation catalyst.

[0016] Furthermore, the preparation method of the oxidation catalyst includes the following specific steps: Nano-titanium dioxide was dried at 140-150℃ for 2 hours, cooled, and sieved to obtain pretreated nano-titanium dioxide. Deionized water and oxalic acid were mixed and stirred for 15-20 minutes. Ferrous sulfate was added and stirring was continued for 25-30 minutes. The pretreated nano-titanium dioxide was added in batches. After the pretreated nano-titanium dioxide was added, the mixture was heated to 35-40℃ and ultrasonically dispersed under stirring for 30-35 minutes. The mixture was cooled, sodium persulfate was added, and stirring was carried out for 20-30 minutes. The mixture was allowed to stand for 20-30 minutes to mature, thus obtaining the oxidation catalyst.

[0017] Furthermore, the ratio of oxalic acid, deionized water, ferrous sulfate, pretreated nano-titanium dioxide, and sodium persulfate is 2-3g: 64-70mL: 3-4g: 10-12g: 15-17g.

[0018] The modified waste incineration fly ash prepared by the above-mentioned method is a modified waste incineration fly ash.

[0019] The beneficial effects of this invention are: This invention discloses a modified waste incineration fly ash and its preparation method, comprising the following raw materials: fly ash, water, a solvent, a modifier, a neutralizing agent, and an oxidation catalyst. The preparation method includes: adding fly ash to water and stirring to obtain a fly ash slurry; treating the fly ash slurry sequentially with a solvent, a modifier, and a neutralizing agent, then filtering by pressure to obtain a filtrate and a solid filter cake; mixing the solid filter cake with water, stirring, adding the oxidation catalyst, stirring again, filtering by pressure, and drying to obtain the modified waste incineration fly ash.

[0020] This invention utilizes a co-solvent prepared from citric acid and sodium bicarbonate to promote the release of easily leached, unstable, and toxic heavy metals from fly ash into the liquid phase. A modifier is then used, in which sodium citrate and sodium diethyldithiocarbamate form a coordination activation structure, exposing numerous sulfur-based active sites. This allows for efficient chelation and capture of heavy metal ions, generating extremely insoluble and stable chelates. The hydrolysis and cross-linking of sodium metasilicate forms an organic-inorganic composite colloidal network that can encapsulate fly ash particles and form a lattice-solidified structure, preventing subsequent re-dissolution and precipitation of heavy metals. Finally, a neutralizing agent is used to adjust the system pH to 9.5-10.5, enhancing the stability of the heavy metal chelates and ensuring that the leaching concentration of heavy metals from the treated fly ash does not exceed the standard.

[0021] This invention utilizes an oxidation catalyst to treat solid-phase filter cake. The oxidation catalyst employs a proprietary preparation process involving high-temperature activation of nano-titanium dioxide, complexation and stabilization with oxalic acid, in-situ support of ferrous iron, and low-temperature coupling with sodium persulfate. This effectively addresses the shortcomings of traditional catalysts, such as low activity, easy oxidation and deactivation, and low free radical utilization. The activated nano-titanium dioxide possesses abundant defect sites, which can anchor the ferrous active component. Oxalic acid can effectively inhibit the oxidation and deactivation of ferrous iron. By synergistically activating sodium persulfate, a large number of highly oxidizing sulfate and hydroxyl radicals are continuously generated at room temperature. These radicals can efficiently break the aromatic ring structure of dioxins, achieving ring-opening and mineralization degradation of dioxins. Furthermore, high-temperature pyrolysis is not required, effectively avoiding the industry pain points of high energy consumption, large equipment investment, and high-temperature resynthesis of dioxins in high-temperature processes. This significantly reduces treatment costs and achieves green and harmless degradation of dioxins.

[0022] The waste incineration fly ash treatment method adopted in this invention has the advantages of low energy consumption, simple operation, and controllable operating conditions, and is suitable for industrial production. It provides a new idea for green and environmentally friendly waste incineration fly ash treatment methods. Detailed Implementation

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] Example 1 A method for preparing modified waste incineration fly ash includes the following steps: Step (1): Add fly ash (source: Everbright Environmental Energy (Suzhou) Co., Ltd. (Qizishan Municipal Solid Waste Incineration Power Plant)) to water and stir at room temperature for 5 minutes to obtain fly ash slurry. Add a solvent to the fly ash slurry and stir at room temperature for 15 minutes. Then add a modifier and continue stirring at room temperature for 1 hour to obtain modified fly ash slurry. Add a neutralizer to the modified fly ash slurry to adjust the pH to 9.5. Stir at room temperature for 40 minutes and filter under pressure at 0.5 MPa to obtain filtrate and solid filter cake. Step (2): Mix the solid filter cake and water, stir at room temperature for 10 min to obtain a composite slurry, add an oxidation catalyst to the composite slurry, stir at room temperature for 2 h, filter by pressure at a pressure of 0.8 MPa, and dry the obtained filter cake at 75℃ for 12 h to obtain modified waste incineration fly ash.

[0025] The amount of solvent added is 2% of the fly ash mass; the solvent is prepared by mixing citric acid, sodium bicarbonate and deionized water in a ratio of 3g:1g:93mL. The preparation method of the modifier includes the following steps: Deionized water, sodium citrate, and sodium diethyldithiocarbamate were mixed and stirred at room temperature for 20 minutes to obtain a premix. Sodium metasilicate was prepared into a sodium metasilicate solution, which was then added dropwise to the premix over 20 minutes. The mixture was heated to 45°C and stirred for 30 minutes, then cooled to room temperature to obtain mixture 1. Calcined kaolin (supplier: Hebei Guanchuan New Material Technology Co., Ltd., 6000 mesh) was added to mixture 1 and stirred at room temperature and 500 rpm. The modifier was ultrasonically dispersed at 300W for 40 minutes under stirring conditions and allowed to stand at room temperature for 1 hour to mature. The ratio of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin was 46mL:5g:14g:9g:15g. The sodium metasilicate solution was prepared by adding sodium metasilicate to deionized water and stirring at room temperature for 10 minutes. The ratio of sodium metasilicate to deionized water in the sodium metasilicate solution was 9g:20mL.

[0026] The amount of modifier added is 4% of the fly ash mass; The neutralizing agent is prepared by mixing calcium hydroxide, magnesium sulfate, and deionized water in a ratio of 8g:2g:85mL.

[0027] In the composite slurry, the ratio of solid filter cake to water is 25g:100mL; the amount of oxidation catalyst added is 5% of the fly ash mass in step (I); The preparation method of the oxidation catalyst includes the following steps: Nano-titanium dioxide (supplier: Shijiazhuang Jinghuang Technology Co., Ltd., particle size distribution (D50): 15nm) was dried at 140℃ for 2h, cooled to room temperature, and passed through a 400-mesh sieve to obtain pretreated nano-titanium dioxide. Deionized water and oxalic acid were mixed and stirred at room temperature for 15min. Ferrous sulfate was added and stirred at room temperature for another 25min. The pretreated nano-titanium dioxide was added in three equal portions, with stirring for 3min after each addition. After the addition of pretreated nano-titanium dioxide, the mixture was heated to 35℃ and ultrasonically dispersed at 300W power for 30min under stirring at 500rpm. The mixture was cooled to room temperature, and sodium persulfate was added. The mixture was stirred at room temperature in the dark for 20min and then allowed to stand and mature at room temperature in the dark for 20min to obtain an oxidation catalyst. The ratio of oxalic acid, deionized water, ferrous sulfate, pretreated nano-titanium dioxide, and sodium persulfate was 2g:64mL:3g:10g:15g.

[0028] Example 2 A method for preparing modified waste incineration fly ash includes the following steps: Step (1): Add fly ash (source: Everbright Environmental Energy (Suzhou) Co., Ltd. (Qizishan Municipal Solid Waste Incineration Power Plant)) to water and stir at room temperature for 8 minutes to obtain fly ash slurry. Add a solvent to the fly ash slurry and stir at room temperature for 18 minutes. Then add a modifier and continue stirring at room temperature for 1.3 hours to obtain modified fly ash slurry. Add a neutralizer to the modified fly ash slurry to adjust the pH to 10.0. Stir at room temperature for 45 minutes and filter under pressure at 0.5 MPa to obtain filtrate and solid filter cake. Step (2): Mix the solid filter cake and water, stir at room temperature for 13 min to obtain a composite slurry, add an oxidation catalyst to the composite slurry, stir at room temperature for 2.5 h, filter by pressure at 0.8 MPa, and dry the obtained filter cake at 78℃ for 12.5 h to obtain modified waste incineration fly ash.

[0029] The amount of solvent added is 2.5% of the fly ash mass; the solvent is prepared by mixing citric acid, sodium bicarbonate and deionized water in a ratio of 4g:1.5g:94mL. The preparation method of the modifier includes the following steps: Deionized water, sodium citrate, and sodium diethyldithiocarbamate were mixed and stirred at room temperature for 23 minutes to obtain a premix. Sodium metasilicate was prepared into a sodium metasilicate solution, which was then added dropwise to the premix over 25 minutes. The mixture was heated to 48°C and stirred for 33 minutes, then cooled to room temperature to obtain mixture 1. Calcined kaolin (supplier: Hebei Guanchuan New Material Technology Co., Ltd., 6000 mesh) was added to mixture 1, and the mixture was stirred at room temperature with a stirring bar at 550 rpm. The modifier was ultrasonically dispersed at 300W for 43 minutes and allowed to stand at room temperature for 1.1 hours to mature. The ratio of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin was 52mL:6g:15g:10g:18g. The sodium metasilicate solution was prepared by adding sodium metasilicate to deionized water and stirring at room temperature for 13 minutes. The ratio of sodium metasilicate to deionized water in the sodium metasilicate solution was 10g:23mL.

[0030] The amount of modifier added is 5% of the fly ash mass; The neutralizing agent is prepared by mixing calcium hydroxide, magnesium sulfate, and deionized water in a ratio of 10g:2.5g:88mL.

[0031] In the composite slurry, the ratio of solid filter cake to water is 25.5 g: 100 mL; the amount of oxidation catalyst added is 6% of the fly ash mass in step (I); The preparation method of the oxidation catalyst includes the following steps: Nano-titanium dioxide (supplier: Shijiazhuang Jinghuang Technology Co., Ltd., particle size distribution (D50): 15nm) was dried at 145℃ for 2h, cooled to room temperature, and passed through a 400-mesh sieve to obtain pretreated nano-titanium dioxide. Deionized water and oxalic acid were mixed and stirred at room temperature for 18min. Ferrous sulfate was added, and stirring was continued at room temperature for 28min. The pretreated nano-titanium dioxide was added in three equal batches, with stirring for 3min after each addition. After the addition of pretreated nano-titanium dioxide, the mixture was heated to 38℃ and ultrasonically dispersed at 300W power for 33min under stirring at 550rpm. The mixture was cooled to room temperature, and sodium persulfate was added. The mixture was stirred at room temperature in the dark for 25min, and then allowed to stand and mature at room temperature in the dark for 25min to obtain an oxidation catalyst. The ratio of oxalic acid, deionized water, ferrous sulfate, pretreated nano-titanium dioxide, and sodium persulfate was 2.5g:67mL:3.5g:11g:16g.

[0032] Example 3 A method for preparing modified waste incineration fly ash includes the following steps: Step (1): Add fly ash (source: Everbright Environmental Energy (Suzhou) Co., Ltd. (Qizishan Municipal Solid Waste Incineration Power Plant)) to water and stir at room temperature for 10 minutes to obtain fly ash slurry. Add a solvent to the fly ash slurry and stir at room temperature for 20 minutes. Then add a modifier and continue stirring at room temperature for 1.5 hours to obtain modified fly ash slurry. Add a neutralizer to the modified fly ash slurry to adjust the pH to 10.5. Stir at room temperature for 50 minutes and filter under pressure at 0.5 MPa to obtain filtrate and solid filter cake. Step (2): Mix the solid filter cake and water, stir at room temperature for 15 minutes to obtain a composite slurry, add an oxidation catalyst to the composite slurry, stir at room temperature for 3 hours, filter by pressure at a pressure of 0.8 MPa, and dry the obtained filter cake at 80°C for 13 hours to obtain modified waste incineration fly ash.

[0033] The amount of solvent added is 3% of the fly ash mass; the solvent is prepared by mixing citric acid, sodium bicarbonate and deionized water in a ratio of 5g:2g:96mL. The preparation method of the modifier includes the following steps: Deionized water, sodium citrate, and sodium diethyldithiocarbamate were mixed and stirred at room temperature for 25 minutes to obtain a premix. Sodium metasilicate was prepared into a sodium metasilicate solution, which was then added dropwise to the premix over a period of 30 minutes. The mixture was heated to 50°C and stirred for 35 minutes, then cooled to room temperature to obtain mixture 1. Calcined kaolin (supplier: Hebei Guanchuan New Material Technology Co., Ltd., 6000 mesh) was added to mixture 1, and the mixture was stirred at room temperature with a stirring bar at 600 rpm. The modifier was ultrasonically dispersed at 300W for 45 minutes and allowed to stand at room temperature for 1.2 hours to mature. The ratio of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin was 57 mL: 7 g: 16 g: 11 g: 20 g. The sodium metasilicate solution was prepared by adding sodium metasilicate to deionized water and stirring at room temperature for 15 minutes. The ratio of sodium metasilicate to deionized water in the sodium metasilicate solution was 11 g: 25 mL.

[0034] The amount of modifier added is 6% of the fly ash mass; The neutralizing agent is prepared by mixing calcium hydroxide, magnesium sulfate, and deionized water in a ratio of 12g:3g:90mL.

[0035] In the composite slurry, the ratio of solid filter cake to water is 26g:100mL; the amount of oxidation catalyst added is 7% of the fly ash mass in step (I); The preparation method of the oxidation catalyst includes the following steps: Nano-titanium dioxide (supplier: Shijiazhuang Jinghuang Technology Co., Ltd., particle size distribution (D50): 15nm) was dried at 150℃ for 2h, cooled to room temperature, and passed through a 400-mesh sieve to obtain pretreated nano-titanium dioxide. Deionized water and oxalic acid were mixed and stirred at room temperature for 20min. Ferrous sulfate was added and stirred at room temperature for another 30min. The pretreated nano-titanium dioxide was added in three equal portions, with stirring for 3min after each addition. After the addition of pretreated nano-titanium dioxide, the mixture was heated to 40℃ and ultrasonically dispersed at 300W power for 35min under stirring at 600rpm. The mixture was cooled to room temperature, and sodium persulfate was added. The mixture was stirred at room temperature in the dark for 30min and then allowed to stand and mature at room temperature in the dark for 30min to obtain an oxidation catalyst. The ratio of oxalic acid, deionized water, ferrous sulfate, pretreated nano-titanium dioxide, and sodium persulfate was 3g:70mL:4g:12g:17g.

[0036] Comparative Example 1 Compared with Example 3, no solvent was used, but everything else was exactly the same as in Example 3, and modified waste incineration fly ash was obtained.

[0037] Comparative Example 2 Compared with Example 3, the modifier was replaced with a mixture of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin in a ratio of 82 mL: 7 g: 16 g: 11 g: 20 g, while the rest was exactly the same as in Example 3, to obtain modified waste incineration fly ash. The preparation method of the modifier includes the following steps: Deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin were mixed and stirred at room temperature for 135 min, and then allowed to stand and mature at room temperature for 1.2 h to obtain the modifier. The ratio of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin was 82 mL: 7 g: 16 g: 11 g: 20 g.

[0038] Comparative Example 3 Compared with Example 3, the modifier was replaced by sodium diethyldithiocarbamate by the same mass, and the rest was exactly the same as in Example 3, to obtain modified waste incineration fly ash.

[0039] Comparative Example 4 Compared with Example 3, the oxidation catalyst was replaced with sodium persulfate by the same mass, while everything else was exactly the same as in Example 3, to obtain modified waste incineration fly ash.

[0040] Comparative Example 5 Compared with Example 3, no neutralizing agent was used to adjust the pH, but everything else was exactly the same as in Example 3, and modified waste incineration fly ash was obtained.

[0041] The modified waste incineration fly ash prepared in Examples 1-3 and Comparative Examples 1-5 of the present invention were further tested below, and the test results are shown in the figure.

[0042] Referencing HJ / T 300-2007, the leaching concentrations of heavy metals (Pb, Cd, Cr, Cu, Zn) in the modified waste incineration fly ash were tested.

[0043] Referring to HJ 77.3-2008, the dioxin toxicity equivalent (ng / kg) in the original fly ash and the obtained modified waste incineration fly ash was tested, and the dioxin degradation rate was calculated. The calculation formula is: Dioxin degradation rate = (Dioxin toxicity equivalent in original fly ash - Dioxin toxicity equivalent in modified waste incineration fly ash) / Dioxin toxicity equivalent in original fly ash × 100%.

[0044] The specific results are recorded in Table 1.

[0045] Table 1: Performance Test Results of Modified Waste Incineration Fly Ash

[0046] According to the data in Table 1, the modified waste incineration fly ash prepared in Examples 1-3 of the present invention has the advantages of low leaching concentration of heavy metals (Pb, Cd, Cr, Cu, Zn) and high dioxin degradation rate.

[0047] Comparing Example 3 with Comparative Example 1, it can be seen that Comparative Example 1 does not use a solvent, which is not conducive to promoting the release of easily leached, unstable, and toxic heavy metals from fly ash into the liquid phase. It is difficult to convert them into insoluble chelates, which is not conducive to reducing the leaching concentration of heavy metals in fly ash, and the dioxin degradation rate also decreases.

[0048] Comparing Example 3 with Comparative Example 2, it can be seen that in Comparative Example 2, the modifier was replaced by a mixture of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin in a specific ratio, instead of being obtained through reaction. This reduced the ability to convert heavy metals into insoluble stable chelates and was not conducive to reducing the leaching concentration of heavy metals. The dioxin degradation rate also decreased.

[0049] A comparison of Example 3 and Comparative Example 3 shows that replacing the modifier with sodium diethyldithiocarbamate by the same mass in Comparative Example 3 significantly reduced the ability to convert heavy metals into insoluble, stable chelates, and was not conducive to reducing the leaching concentration of heavy metals, and also reduced the dioxin degradation rate.

[0050] A comparison of Example 3 and Comparative Example 4 shows that, although replacing the oxidation catalyst with sodium persulfate in Comparative Example 4 did not affect the ability to convert heavy metals into insoluble stable chelates, it significantly reduced the ability to degrade dioxins, resulting in a substantial decrease in the dioxin degradation rate.

[0051] A comparison of Example 3 and Comparative Example 5 shows that in Comparative Example 5, the lack of a neutralizing agent to adjust the pH resulted in decreased stability of the heavy metal chelate and hindered the reduction of the leaching concentration of heavy metals, also leading to a decrease in the dioxin degradation rate.

[0052] The above description is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the concept of the invention or exceed the scope defined in the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing modified waste incineration fly ash, characterized in that: Includes the following steps: Step (1): Add fly ash to water and stir to obtain fly ash slurry. Add a solvent to the fly ash slurry and stir. Then add a modifier and continue stirring to obtain modified fly ash slurry. Add a neutralizer to the modified fly ash slurry, adjust the pH, stir, and filter under pressure to obtain filtrate and solid filter cake. Step (2): Mix the solid filter cake and water, stir to obtain a composite slurry, add an oxidation catalyst to the composite slurry, stir, filter under pressure, and dry to obtain modified waste incineration fly ash.

2. The method for preparing modified waste incineration fly ash according to claim 1, characterized in that: In step (i), the amount of the solvent added is 2-3% of the fly ash mass; the solvent is prepared by mixing citric acid, sodium bicarbonate and deionized water in a ratio of 3-5g: 1-2g: 93-96mL.

3. The method for preparing modified waste incineration fly ash according to claim 1, characterized in that: In step (i), the preparation method of the modifier includes the following steps: Deionized water, sodium citrate, and sodium diethyldithiocarbamate were mixed and stirred to obtain a premixed solution. Sodium metasilicate was prepared into a sodium metasilicate solution and added dropwise to the premixed solution. The mixture was heated and stirred, then cooled to obtain mixture 1. Calcined kaolin was added to mixture 1 and ultrasonically dispersed under stirring conditions. The mixture was then allowed to stand and mature to obtain a modifier.

4. The method for preparing modified waste incineration fly ash according to claim 3, characterized in that: The ratio of deionized water, sodium citrate, sodium diethyldithiocarbamate, sodium metasilicate, and calcined kaolin is 46-57 mL: 5-7 g: 14-16 g: 9-11 g: 15-20 g.

5. The method for preparing modified waste incineration fly ash according to claim 3, characterized in that: The sodium metasilicate solution is prepared by adding sodium metasilicate to deionized water and stirring for 10-15 minutes to obtain a sodium metasilicate solution; the ratio of sodium metasilicate to deionized water in the sodium metasilicate solution is 9-11g:20-25mL.

6. The method for preparing modified waste incineration fly ash according to claim 1, characterized in that: In step (i), the amount of the modifier added is 4-6% of the fly ash mass; the neutralizing agent is obtained by mixing calcium hydroxide, magnesium sulfate and deionized water in a ratio of 8-12g: 2-3g: 85-90mL.

7. The method for preparing modified waste incineration fly ash according to claim 1, characterized in that: In step (ii), the ratio of solid filter cake to water in the composite slurry is 25-26 g: 100 mL; the amount of oxidation catalyst added is 5-7% of the fly ash mass in step (i).

8. The method for preparing modified waste incineration fly ash according to claim 1, characterized in that: In step (ii), the preparation method of the oxidation catalyst includes the following steps: Nano-titanium dioxide was dried, cooled, and sieved to obtain pretreated nano-titanium dioxide. Deionized water and oxalic acid were mixed and stirred. Ferrous sulfate was added and stirred continuously. The pretreated nano-titanium dioxide was added in batches, heated, and ultrasonically dispersed under stirring conditions. After cooling, sodium persulfate was added, stirred, and allowed to stand for aging to obtain an oxidation catalyst.

9. The method for preparing modified waste incineration fly ash according to claim 8, characterized in that: The ratio of oxalic acid, deionized water, ferrous sulfate, pretreated nano-titanium dioxide, and sodium persulfate is 2-3g: 64-70mL: 3-4g: 10-12g: 15-17g.

10. Modified waste incineration fly ash prepared by the method of any one of claims 1-9.