Production process of copper-titanium-copper metal composite strip for wiring harness terminal
Through processes such as multi-stage grinding, surface roughening, heterogeneous temperature composite rolling, and multi-pass rolling, the problem of unstable performance in the production of copper-titanium-copper composite strips has been solved, realizing high-strength and high-conductivity copper-titanium-copper metal composite strips suitable for charging guns, motor control systems, automotive wiring harness terminals, and automotive Ethernet connectors.
Patent Information
- Application Number
- CN202611132219.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-24
AI Technical Summary
The existing copper-titanium-copper composite strip production process lacks systematic specifications in terms of base layer surface treatment, passive layer roughness control, heterogeneous temperature composite parameter optimization, and multi-pass rolling deformation distribution. This results in insufficient product performance stability and makes it difficult to meet the dimensional accuracy, mechanical properties, and interlayer bonding strength requirements of wire harness terminal materials.
Through multi-stage grinding, surface roughening, heterogeneous temperature composite rolling, multi-pass rolling and surface passivation, combined with continuous annealing and hydrogen reducing atmosphere, process parameters are controlled to achieve high strength and high conductivity of copper-titanium-copper metal composite strips, forming a strong physical metallurgical bonding layer.
It achieves high strength and high conductivity of copper-titanium-copper metal composite strip, meets the performance requirements of wire harness terminal materials, simplifies the process flow, improves production efficiency and product yield, and replaces expensive beryllium copper materials.
Smart Images

Figure CN123149243A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal composite material processing, and in particular to a manufacturing process for a copper-titanium-copper metal composite strip for wire harness terminals. Background Technology
[0002] In the current domestic electronics and electrical appliance industry, traditional high-strength materials are mainly titanium alloys, and high-conductivity materials are mainly pure copper strips. However, the selection of materials that simultaneously possess both high strength and high conductivity is very limited. Currently, products such as charging guns, motor control systems, automotive wiring harness terminals, and automotive Ethernet connectors are beginning to explore the application of copper-titanium composite metal materials. These materials utilize titanium interlayers to improve strength, temperature resistance, and stress relaxation resistance, while ensuring long-term vibration contact stability, thus replacing expensive beryllium copper materials.
[0003] Currently, the manufacturing process of copper-titanium-copper three-layer materials has achieved continuous differential temperature rolling control and AGC automated rolling production. A surface treatment process using hydrogen as a reducing atmosphere is also applied in the core metal strip deformation zone. This process utilizes the different temperatures of the materials before rolling to induce ultra-high temperature zones through mutual friction during large deformation rolling, reaching the phase transition temperature between the two metals. This allows for atomic diffusion and achieves a strong bond between the interfaces. However, existing technologies still have shortcomings in the production process control of copper-titanium-copper composite strips, particularly in the lack of systematic process specifications for base layer surface treatment, passive layer roughness control, differential temperature composite parameter optimization, multi-pass rolling deformation distribution, and surface passivation treatment. This results in insufficient product performance stability and inconsistent interlayer bonding quality, making it difficult to meet the stringent requirements for dimensional accuracy, mechanical properties, and interlayer bonding strength of wire harness terminal materials.
[0004] Therefore, researching and developing a copper-titanium-copper composite strip production process that features precise control of process parameters, stable product performance, and the ability to meet the requirements of wire harness terminals is of significant practical importance. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a manufacturing process for copper-titanium-copper composite metal strips for wire harness terminals, thus solving the above problems.
[0006] To achieve the above objectives, the present invention provides a manufacturing process for a copper-titanium-copper composite strip for wire harness terminals, comprising the following steps: S1. The upper and lower composite contact surfaces of the base layer titanium strip are subjected to multi-stage grinding treatment, with grinding meshes of 320 mesh, 400 mesh and 1200 mesh respectively. After grinding, the surface is rinsed with clean water and then instantly dried with filtered high-pressure hot air at 80-95℃ until no water stains remain. S2. The surface roughening treatment of the composite bonding surface of the passive layer copper strip is carried out by brushing with a wire brush or grinding with a sander belt, so that the surface roughness Ra of the composite bonding surface is greater than 1.2, in order to increase the mechanical interlocking force and interface bonding area between the copper strip and the titanium strip. S3. Composite rolling is carried out under different temperature conditions, with the copper strip of the composite layer controlled at 80±30℃ and the titanium strip of the base layer controlled at 780±30℃. The continuous composite speed is 1.5±0.5m / min, the material rolling deformation is controlled at 46%-55%, and the maximum rolling force of the composite local rolling is controlled at 340T, so that the metal strip reaches the phase transformation temperature locally in the rolling area to form a strong physical metallurgical bonding layer or solid solution zone. S4. Perform continuous annealing on the composite strip at a heat treatment temperature of 750℃±10℃ and a speed of 8-10m / min. S5. Perform multi-pass rolling on the annealed strip, with the deformation amount controlled at 30%-37% in each pass; S6. The rolled strip is subjected to surface passivation treatment by online spraying of copper passivating agent and drying with continuous constant temperature hot air at 90℃±5℃. The strip moving speed in the drying area is 5-7m / min. S7. The passivated strip is longitudinally cut into the required width to obtain the finished copper-titanium-copper metal composite strip.
[0007] Preferably, the multi-stage grinding process is as follows: using three sets of abrasive belts of 320 mesh, 400 mesh, and 1200 mesh to perform coarse grinding, medium grinding, and fine grinding on the upper and lower composite contact surfaces of the titanium belt in sequence; after grinding, the surface is rinsed with clean water and then instantly dried with filtered high-pressure hot air at 80-95℃ to ensure that there are no water stains remaining on the upper and lower surfaces of the material.
[0008] Preferably, the composite rolling is carried out in a controllable positive pressure composite chamber, which is filled with hydrogen as a reducing atmosphere to ensure that the oxygen-free copper in the passive layer is completely reduced at the interface before composite, with no oxide scale generated, and no additional grinding or polishing of the surface is required during the composite process.
[0009] Preferably, during the composite rolling process, the base layer titanium strip and the passive layer copper strip undergo continuous roll deformation under the action of a large instantaneous rolling force after being subjected to differential temperature control. The metal strip generates an ultra-high temperature zone in a local position in the rolling area due to friction, so that the interface between the two metal materials reaches the phase transformation temperature, realizing atomic diffusion and strong interface bonding.
[0010] Preferably, the multi-pass rolling process includes: S51, Rolling 1: The composite strip is rolled in the first pass, and the rolling deformation is controlled at 30%-37%. Before rolling, the surface of the strip is cleaned to remove surface residues generated during the composite process. S52, Continuous Annealing 2: The strip after rolling 1 is subjected to continuous annealing treatment. The heat treatment temperature is 750℃±10℃, the annealing speed is controlled at 8-10m / min, and the annealing atmosphere is a hydrogen reducing atmosphere or a nitrogen protective atmosphere to eliminate the work hardening generated by rolling 1 and restore the plasticity of the material. S53, Rolling 2: The strip after continuous annealing 2 is rolled in a second pass, and the rolling deformation is controlled at 30%-37% to further reduce the thickness of the strip and improve the surface quality. S54. Edge cutting: The strip after rolling 2 is subjected to edge cutting treatment to remove edge cracks, burrs and uneven deformation areas, and to ensure the flatness and width of the strip edge. S55, Continuous Annealing 3: The strip after edge cutting is subjected to continuous annealing treatment. The heat treatment temperature is 750℃±10℃, the annealing speed is controlled at 8-10m / min, and the annealing atmosphere is a hydrogen reducing atmosphere or a nitrogen protective atmosphere to further eliminate work hardening and provide a suitable microstructure for subsequent finishing rolling. S56, Rolling 3: The strip after continuous annealing 3 is rolled in a third pass, and the rolling deformation is controlled at 30%-37% to make the strip reach the target finished thickness.
[0011] Preferably, the formula for calculating the deformation amount of each rolling pass is: Deformation amount = (thickness before rolling - thickness after rolling) / thickness before rolling × 100%.
[0012] Preferably, the surface passivation treatment includes: uniformly spraying a copper passivating agent that is automatically stirred evenly using an online spraying device onto the surface of the strip; instantaneously drying the sprayed strip with continuous constant temperature hot air at 90℃±5℃; controlling the moving speed of the strip in the drying area to 5m / min-7m / min; and forming an anti-oxidation protective film on the surface of the passivated strip to prevent surface oxidation.
[0013] Preferably, in the longitudinal slitting process, the longitudinal slitting width is 5mm-160mm, and the width tolerance is controlled within ±0.1mm to meet the width requirements of different wire harness terminal materials.
[0014] Preferably, the total thickness of the finished copper-titanium-copper composite strip is controlled between 0.07mm and 0.15mm, the width is controlled between 5mm and 170mm, the tensile strength reaches 460MPa, the thickness of the passive copper layer accounts for 5%-35% of the total material thickness, and the thickness of the base layer titanium accounts for 10%-65% of the total thickness of the composite strip.
[0015] Preferably, the copper-titanium-copper composite strip is a three-layer centered surface-to-surface composite strip structure, consisting of an upper passive layer copper strip, an intermediate base layer titanium strip, and a lower passive layer copper strip; or it is a strip structure formed by slotting copper material, embedding titanium wire, and then rolling.
[0016] Beneficial effects This invention provides a manufacturing process for copper-titanium-copper composite strips for wire harness terminals. Compared with the prior art, it has the following advantages: 1. In this invention, the titanium strip of the base layer undergoes three-stage grinding treatment with 320 mesh, 400 mesh, and 1200 mesh, and the composite bonding surface of the passive layer copper strip is roughened by wire brushing or abrasive belt grinding, resulting in a surface roughness Ra > 1.2. This significantly increases the mechanical interlocking force and interfacial bonding area between the copper and titanium strips. Combined with process control during multi-pass rolling, where the deformation amount per pass is controlled at 30%-37% and the continuous annealing temperature is kept stable at 750℃±10℃, longitudinal cracks caused by rolling deformation are effectively prevented and eliminated. Work hardening restores the material's plasticity, and the final copper-titanium-copper composite strip can be controlled in terms of total thickness (0.07-0.15mm), width (5-170mm), and tensile strength (460MPa). The passive layer has a copper thickness of 5%-35%, and the base layer has a titanium thickness of 10%-65%. This achieves the complementary advantages of titanium's high strength, temperature resistance, and stress relaxation resistance with copper's high conductivity, making it a viable alternative to expensive beryllium copper. It has broad application prospects in charging guns, motor control systems, automotive wiring harness terminals, and automotive Ethernet connectors. 2. In this invention, the composite copper strip is controlled at 80±30℃ and the base titanium strip is controlled at 780±30℃ by using heterothermal composite rolling. This causes the metal strips to generate ultra-high temperature zones locally due to friction in the rolling area, reaching the phase transition temperature between the two metal materials. This achieves atomic diffusion and strong interfacial bonding, forming a physical metallurgical bonding layer or solid solution zone. This solves the problems of insufficient copper-titanium interfacial bonding strength and easy delamination in traditional composite processes. At the same time, hydrogen is filled into the controllable positive pressure composite cavity as a reducing atmosphere, ensuring the complete reduction of the oxygen-free copper passive layer at the interface before composite, avoiding the formation of oxide scale. This eliminates the need for additional grinding or polishing of the surface during the composite process, simplifying the process and improving production efficiency and product yield. Attached Figure Description
[0017] Figure 1 This is a flowchart of the manufacturing process of a copper-titanium-copper metal composite strip for wire harness terminals proposed in this invention. Detailed Implementation The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] Please see Figure 1 The present invention provides two technical solutions, specifically including the following embodiments: Example 1: A manufacturing process for a copper-titanium-copper composite strip for wire harness terminals includes the following steps: S1. The upper and lower composite contact surfaces of the base layer titanium strip are subjected to multi-stage grinding treatment, with grinding mesh sizes of 320 mesh, 400 mesh, and 1200 mesh respectively. After grinding, the surface is rinsed with clean water and then instantly dried with filtered high-pressure hot air at 80-95℃ until no water stains remain. The multi-stage grinding treatment is as follows: three sets of abrasive belts of 320 mesh, 400 mesh, and 1200 mesh are used to perform coarse grinding, medium grinding, and fine grinding on the upper and lower composite contact surfaces of the titanium strip in sequence. After grinding, the surface is rinsed with clean water and then instantly dried with filtered high-pressure hot air at 80-95℃ to ensure that no water stains remain on the upper and lower surfaces of the material. S2. The surface roughening treatment of the composite bonding surface of the passive layer copper strip is carried out by brushing with a wire brush or grinding with a sander belt, so that the surface roughness Ra of the composite bonding surface is greater than 1.2, in order to increase the mechanical interlocking force and interface bonding area between the copper strip and the titanium strip. S3. Composite rolling is carried out under different temperature conditions, with the copper strip of the composite layer controlled at 80±30℃ and the titanium strip of the base layer controlled at 780±30℃. The continuous composite speed is 1.5±0.5m / min, the material rolling deformation is controlled at 46%-55%, and the maximum rolling force of the composite local rolling is controlled at 340T. This allows the metal strip to reach the phase transformation temperature locally in the rolling area, forming a strong physical metallurgical bonding layer or solid solution zone. The composite rolling is carried out in a controllable positive pressure composite cavity, which is filled with hydrogen as a reducing atmosphere to ensure that the oxygen-free copper of the passive layer is completely reduced at the interface before the composite, without the formation of oxide scale. No additional grinding or polishing is required during the composite process. During the composite rolling process, after the base layer titanium strip and the passive layer copper strip are controlled by different temperatures, they undergo continuous rolling deformation under the action of a large instantaneous rolling force. The metal strip generates an ultra-high temperature zone in the local position of the rolling area due to friction, which allows the interface between the two metal materials to reach the phase transformation temperature, achieving atomic diffusion and strong interface bonding. S4. Perform continuous annealing on the composite strip at a heat treatment temperature of 750℃±10℃ and a speed of 8-10m / min. S5. Perform multi-pass rolling on the annealed strip, with the deformation amount controlled at 30%-37% in each pass. The multi-pass rolling includes: S51, Rolling 1: The composite strip is rolled in the first pass, and the rolling deformation is controlled at 30%-37%. Before rolling, the surface of the strip is cleaned to remove surface residues generated during the composite process. S52, Continuous Annealing 2: The strip after rolling 1 is subjected to continuous annealing treatment. The heat treatment temperature is 750℃±10℃, the annealing speed is controlled at 8-10m / min, and the annealing atmosphere is a hydrogen reducing atmosphere or a nitrogen protective atmosphere to eliminate the work hardening generated by rolling 1 and restore the plasticity of the material. S53, Rolling 2: The strip after continuous annealing 2 is rolled in a second pass, and the rolling deformation is controlled at 30%-37% to further reduce the thickness of the strip and improve the surface quality. S54. Edge cutting: The strip after rolling 2 is subjected to edge cutting treatment to remove edge cracks, burrs and uneven deformation areas, and to ensure the flatness and width of the strip edge. S55, Continuous Annealing 3: The strip after edge cutting is subjected to continuous annealing treatment. The heat treatment temperature is 750℃±10℃, the annealing speed is controlled at 8-10m / min, and the annealing atmosphere is a hydrogen reducing atmosphere or a nitrogen protective atmosphere to further eliminate work hardening and provide a suitable microstructure for subsequent finishing rolling. S56, Rolling 3: The strip after continuous annealing 3 is rolled in a third pass, and the rolling deformation is controlled at 30%-37% to make the strip reach the target finished thickness. The formula for calculating the deformation amount in each rolling pass is: Deformation amount = (thickness before rolling - thickness after rolling) / thickness before rolling × 100%.
[0019] S6. The rolled strip undergoes surface passivation treatment using an online spraying copper passivating agent and is dried with continuous constant-temperature hot air at 90℃±5℃. The strip moving speed in the drying area is 5-7m / min. The surface passivation treatment includes: uniformly spraying the strip surface with copper passivating agent that is automatically stirred by an online spraying device; instantaneously drying the sprayed strip with continuous constant-temperature hot air at 90℃±5℃; controlling the strip moving speed in the drying area to 5m / min-7m / min; and forming an anti-oxidation protective film on the surface of the passivated strip to prevent surface oxidation. S7. The passivated strip is longitudinally slit to the required width to obtain the finished copper-titanium-copper composite strip. In the longitudinal slitting process, the longitudinal slitting width is 5mm-160mm, and the width tolerance is controlled within ±0.1mm to meet the width requirements of different wire harness terminal materials. The total thickness of the finished copper-titanium-copper composite strip is controlled between 0.07mm-0.15mm, the width is controlled between 5mm-170mm, and the tensile strength reaches 460MPa. The thickness of the passive copper layer accounts for 5%-35% of the total material thickness, and the thickness of the base layer titanium accounts for 10%-65% of the total thickness of the composite strip. The copper-titanium-copper composite strip is a three-layer centered surface-to-surface composite strip structure, consisting of an upper passive copper strip, a middle base layer titanium strip, and a lower passive copper strip; or it is a strip structure formed by slotting copper material, embedding titanium wire, and then rolling.
[0020] Example 2: Based on Example 1, copper-titanium-copper composite strips were prepared using the following specific process parameters: S1, Surface treatment of the base layer titanium strip (TA1): The upper and lower composite contact surfaces of the titanium strip were coarsely ground, medium ground, and finely ground in sequence using three sets of abrasive belts of 320 mesh, 400 mesh, and 1200 mesh. After grinding, the surface was rinsed with clean water and then instantly dried with filtered high-pressure hot air at 85°C to ensure that there were no water stains remaining on the upper and lower surfaces of the material.
[0021] S2, Passive Layer Copper Strip (TU1) Surface Treatment: The surface roughening treatment of the composite bonding surface of the passive layer copper strip is carried out by brushing with a wire brush, so that the surface roughness Ra of the composite bonding surface is greater than 1.2.
[0022] S3, Differential Temperature Composite Calendering: Composite rolling is carried out under different temperature conditions: the upper passive layer copper strip is controlled at 80℃, the base layer titanium strip is controlled at 780℃, and the lower passive layer copper strip is controlled at 80℃. The continuous composite speed is 1.5m / min, the material rolling deformation is controlled at 50%, the maximum rolling force of the composite local rolling is controlled at 340T, and the composite rolling is carried out in a controllable positive pressure composite cavity, which is filled with hydrogen as a reducing atmosphere.
[0023] S4-S6, multi-pass rolling and annealing: The composite strip was subjected to continuous annealing at a heat treatment temperature of 750℃ and an annealing rate of 9m / min. Perform rolling 1, with the deformation controlled at 33%; Continuous annealing 2, heat treatment temperature is 750℃, annealing speed is controlled at 9m / min, annealing atmosphere is hydrogen reducing atmosphere; Perform rolling step 2, with deformation controlled at 35%; Edge cutting removes edge cracks, burrs, and unevenly deformed areas; Continuous annealing 3, heat treatment temperature is 750℃, annealing speed is controlled at 9m / min, annealing atmosphere is hydrogen reducing atmosphere; Rolling is performed in step 3, with the deformation controlled at 33% to achieve the target finished product thickness for the strip.
[0024] S7. Surface passivation treatment: The copper passivating agent is automatically and evenly mixed using an online spraying device and then uniformly sprayed onto the surface of the strip. The sprayed strip is then instantly dried with continuous constant-temperature hot air at 90°C. The moving speed of the strip in the drying area is controlled at 6 m / min.
[0025] S8. Longitudinal slitting: The passivated strip is longitudinally slit into 125mm wide sections with a width tolerance controlled within ±0.1mm to obtain the finished copper-titanium-copper composite strip.
[0026] Finished product performance test results: Conclusion: This embodiment employs a three-layer copper-titanium-copper heterothermal composite rolling process to prepare a copper-titanium-copper metal composite strip (grade CTC141) with dimensions of 0.06mm × 125mm. Testing and verification showed that the actual thickness of the finished product was 0.062-0.064mm, and the width was 124.93-124.95mm, indicating good dimensional accuracy control. The thickness of the upper copper layer was approximately 0.010-0.011mm, the titanium layer approximately 0.041-0.042mm, and the lower copper layer approximately 0.010-0.011mm. The total thickness accounts for approximately 34%-35%, and the titanium layer accounts for approximately 65%-66%, forming a reasonable copper-titanium-copper three-layer symmetrical structure; the tensile strength is stable at 364.3-365.9MPa, and the elongation reaches 21%-23%, combining high strength and good plasticity; the surface hardness of the copper layer Hv0.05 is 71.4-80.7, the lateral bending is 0.1-0.2mm / m, and the burrs are only 0.002-0.003mm, with excellent surface quality and plate shape; there are no cracks, gaps or delamination when bent at 90°, and the metallurgical bond between the layers is strong; In summary, the parameters of this heterothermal composite rolling process are reasonable and feasible. The prepared copper-titanium-copper metal composite strip has excellent comprehensive performance and can meet the requirements of wire harness terminal materials for high strength, high conductivity and good formability, and is ready for industrial mass production.
[0027] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A production process of a copper-titanium-copper metal composite strip for a wiring harness terminal, characterized by: Includes the following steps: S1. The upper and lower composite contact surfaces of the base layer titanium strip are subjected to multi-stage grinding treatment, with grinding meshes of 320 mesh, 400 mesh and 1200 mesh respectively. After grinding, the surface is rinsed with clean water and then instantly dried with filtered high-pressure hot air at 80-95℃ until no water stains remain. S2. The surface roughening treatment of the composite bonding surface of the passive layer copper strip is carried out by brushing with a wire brush or grinding with a sander belt, so that the surface roughness Ra of the composite bonding surface is greater than 1.2, in order to increase the mechanical interlocking force and interface bonding area between the copper strip and the titanium strip. S3. Composite rolling is carried out under different temperature conditions, with the copper strip of the composite layer controlled at 80±30℃ and the titanium strip of the base layer controlled at 780±30℃. The continuous composite speed is 1.5±0.5m / min, the material rolling deformation is controlled at 46%-55%, and the maximum rolling force of the composite local rolling is controlled at 340T, so that the metal strip reaches the phase transformation temperature locally in the rolling area to form a strong physical metallurgical bonding layer or solid solution zone. S4. Perform continuous annealing on the composite strip at a heat treatment temperature of 750℃±10℃ and a speed of 8-10m / min. S5. Perform multi-pass rolling on the annealed strip, with the deformation amount controlled at 30%-37% in each pass; S6. The rolled strip is subjected to surface passivation treatment by online spraying of copper passivating agent and drying with continuous constant temperature hot air at 90℃±5℃. The strip moving speed in the drying area is 5-7m / min. S7. The passivated strip is longitudinally cut into the required width to obtain the finished copper-titanium-copper metal composite strip.
2. The production process of the copper-titanium-copper metal composite strip for a wire harness terminal according to claim 1, characterized in that: The multi-stage grinding process involves using three sets of abrasive belts of 320 mesh, 400 mesh, and 1200 mesh to perform coarse grinding, medium grinding, and fine grinding on the upper and lower composite contact surfaces of the titanium belt in sequence; after grinding, the surface is rinsed with clean water and then instantly dried with filtered high-pressure hot air at 80-95℃ to ensure that there are no water stains remaining on the upper and lower surfaces of the material.
3. The manufacturing process of a copper-titanium-copper composite metal strip for wire harness terminals according to claim 1, characterized in that: The composite rolling is carried out in a controllable positive pressure composite chamber, which is filled with hydrogen as a reducing atmosphere to ensure that the oxygen-free copper in the passive layer is completely reduced at the interface before composite, and no oxide scale is generated. No additional grinding or polishing is required during the composite process.
4. The manufacturing process of a copper-titanium-copper composite strip for wire harness terminals according to claim 1, characterized in that: During the composite rolling process, the titanium base layer and the copper passive layer undergo continuous rolling deformation under the action of a large instantaneous rolling force after being subjected to temperature control. The metal strip generates an ultra-high temperature zone in a local position in the rolling area due to friction, so that the interface between the two metal materials reaches the phase transformation temperature, realizing atomic diffusion and strong interface bonding.
5. The manufacturing process of a copper-titanium-copper composite strip for wire harness terminals according to claim 1, characterized in that: The multi-pass rolling process includes: S51, Rolling 1: The composite strip is rolled in the first pass, and the rolling deformation is controlled at 30%-37%. Before rolling, the surface of the strip is cleaned to remove surface residues generated during the composite process. S52, Continuous Annealing 2: The strip after rolling 1 is subjected to continuous annealing treatment. The heat treatment temperature is 750℃±10℃, the annealing speed is controlled at 8-10m / min, and the annealing atmosphere is a hydrogen reducing atmosphere or a nitrogen protective atmosphere to eliminate the work hardening generated by rolling 1 and restore the plasticity of the material. S53, Rolling 2: The strip after continuous annealing 2 is rolled in a second pass, and the rolling deformation is controlled at 30%-37% to further reduce the thickness of the strip and improve the surface quality. S54. Edge cutting: The strip after rolling 2 is subjected to edge cutting treatment to remove edge cracks, burrs and uneven deformation areas, and to ensure the flatness and width of the strip edge. S55, Continuous Annealing 3: The strip after edge cutting is subjected to continuous annealing treatment. The heat treatment temperature is 750℃±10℃, the annealing speed is controlled at 8-10m / min, and the annealing atmosphere is a hydrogen reducing atmosphere or a nitrogen protective atmosphere to further eliminate work hardening and provide a suitable microstructure for subsequent finishing rolling. S56, Rolling 3: The strip after continuous annealing 3 is rolled in a third pass, and the rolling deformation is controlled at 30%-37% to make the strip reach the target finished thickness.
6. The manufacturing process of a copper-titanium-copper composite strip for wire harness terminals according to claim 5, characterized in that: The formula for calculating the deformation amount in each rolling pass is: Deformation amount = (thickness before rolling - thickness after rolling) / thickness before rolling × 100%.
7. The manufacturing process of a copper-titanium-copper composite strip for wire harness terminals according to claim 1, characterized in that: The surface passivation treatment includes: uniformly spraying a copper passivating agent that is automatically stirred by an online spraying device onto the surface of the strip; instantaneously drying the sprayed strip with continuous constant temperature hot air at 90℃±5℃; controlling the moving speed of the strip in the drying area at 5m / min-7m / min; and forming an anti-oxidation protective film on the surface of the passivated strip to prevent surface oxidation.
8. The manufacturing process of a copper-titanium-copper composite strip for wire harness terminals according to claim 1, characterized in that: In the longitudinal slitting process, the longitudinal slitting width is 5mm-160mm, and the width tolerance is controlled within ±0.1mm to meet the width requirements of different wire harness terminal materials.
9. The manufacturing process of a copper-titanium-copper composite strip for wire harness terminals according to claim 1, characterized in that: The total thickness of the finished copper-titanium-copper composite strip is controlled between 0.07mm and 0.15mm, the width is controlled between 5mm and 170mm, the tensile strength reaches 460MPa, the thickness of the passive copper layer accounts for 5%-35% of the total material thickness, and the thickness of the base titanium layer accounts for 10%-65% of the total thickness of the composite strip.
10. The manufacturing process of a copper-titanium-copper composite strip for wire harness terminals according to claim 1, characterized in that: The copper-titanium-copper composite strip is a three-layer centered surface-to-surface composite strip structure, consisting of an upper passive layer copper strip, an intermediate base layer titanium strip, and a lower passive layer copper strip; or it is a strip structure formed by slotting copper material, embedding titanium wire, and then rolling.