Hot rolling method for 65mn fine blanking steel capable of preventing strip breakage in tandem cold rolling

By controlling the final hot rolling temperature and segmented cooling process, a pearlite matrix and island-shaped dispersed ferrite structure are formed, solving the strip breakage problem of 65Mn fine stamping steel during cold continuous rolling, and achieving low-cost, high-efficiency reduction of strip breakage rate and performance matching.

CN123149244APending Publication Date: 2026-11-24HANDAN IRON & STEEL GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610960699.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the existing hot rolling process of 65Mn fine stamping steel, the ferrite content is high and it is distributed in a network. Under the conditions of high tension and high reduction in five-stand cold continuous rolling, it is prone to cracking, resulting in a high strip breakage rate. Existing anti-strip breakage technology has failed to effectively control the matrix structure from the source of hot rolling and partially relies on the addition of high-cost alloys.

Method used

By controlling the final rolling temperature of hot rolling and segmented cooling processes, including high-speed laminar flow cooling and air cooling, a pearlite matrix and island-like dispersed ferrite structure are formed, eliminating network ferrite and reducing the ferrite content to 1% to 3%.

Benefits of technology

It significantly reduces the breakage rate of cold continuous rolling to below 1%, while taking into account the strength and toughness of the material, meeting the performance requirements of fine stamping steel. It is low in cost and easy to promote industrially without the need for additional equipment modification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149244A_ABST
    Figure CN123149244A_ABST
Patent Text Reader

Abstract

This invention discloses a hot rolling method for 65Mn fine-stamping steel that can prevent strip breakage during cold continuous rolling, including hot rolling, cooling, and coiling steps; the hot rolling step: the final rolling temperature is controlled at 850-890℃; the cooling step: first, the strip steel after final rolling is cooled to 650-690℃ at a cooling rate of ≥100℃ / s, then air-cooled for 8-12s, and finally cooled to the coiling temperature at a cooling rate of 30-50℃ / s; after the above treatment, the strip steel structure is pearlite matrix + island-shaped dispersed ferrite, and there is no network ferrite. This method achieves a small amount of ferrite with an island-like dispersed distribution through segmented cooling, completely eliminating network ferrite and suppressing crack initiation and propagation during the five-stand cold rolling process from the source. It avoids preferential cracking of ferrite under high tension and high reduction conditions in cold rolling, reducing the strip breakage rate from 3% to 8% to below 1%. At the same time, it ensures the matching of material strength and toughness, and is suitable for fine blanking processing requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hot rolling technology of steel, and in particular to a hot rolling method for 65Mn fine stamping steel that can prevent strip breakage during cold continuous rolling. Background Technology

[0002] 65Mn, a classic high-carbon precision stamping steel, is widely used in the manufacture of precision stamped parts due to its high strength and good wear resistance. Its production process is usually "smelting → continuous casting → hot rolling → pickling → cold continuous rolling → annealing → precision stamping". Cold continuous rolling mills, especially five-stand cold continuous rolling mills, adopt a continuous rolling mode. In order to avoid strip deviation, it is necessary to maintain a large inter-stand tension and allocate a large reduction rate per stand to achieve the total reduction target. In contrast, ordinary single-stand cold rolling mills have small inlet / outlet tension and low single reduction rate, and the rolling conditions of the two are significantly different.

[0003] Currently, the hot rolling preparation of 65Mn precision stamping steel mostly adopts conventional processes: single-stage laminar flow cooling and coiling temperature of 600-650℃. The resulting microstructure is "network ferrite + pearlite", with a ferrite content usually ≥5%. Under the coupled effect of "high tension + high reduction" in cold continuous rolling, the lower-strength ferrite preferentially deforms and yields, easily initiating microcracks along the grain boundaries of network ferrite. The cracks rapidly propagate to form macroscopic tearing, eventually leading to strip breakage. The strip breakage rate can reach 3%-8%, which seriously restricts production efficiency and yield.

[0004] Existing anti-strip breakage technologies mostly focus on weld control, compositional microalloying, or cold rolling process optimization: such as Shougang Jingtang's automatic weld identification and speed reduction technology, Xinyu Steel's Cr microalloying controlled segregation technology, and Valin Lianyuan Steel's cold rolling reduction rate optimization technology. However, these technologies either only solve localized strip breakage in the weld, rely on high-cost alloy additions, or fail to control the matrix structure from the hot rolling source, thus failing to fundamentally suppress the strip breakage problem of the base material under five-stand cold continuous rolling conditions.

[0005] The existing 65Mn production process has the following problems: 1. The conventional hot rolling process has a high ferrite content (≥5%) and a network distribution. Under the conditions of high tension and high reduction in five-stand cold continuous rolling, the ferrite preferentially deforms and cracks, and the cracks extend along the network, leading to strip breakage. 2. Existing anti-strip breakage technology has not designed a hot rolling material preparation scheme for the special working conditions of five-stand cold continuous rolling, and the organization and control are poorly matched with the cold rolling working conditions; 3. Some technologies rely on the addition of microalloying elements, resulting in high production costs and limited effects on microstructure control. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a hot rolling method for 65Mn fine stamping steel that can prevent strip breakage during cold continuous rolling by suppressing the initiation and propagation of cracks from the source.

[0007] To solve the above-mentioned technical problems, the technical solution adopted by the present invention includes hot rolling, cooling and coiling steps; The hot rolling step: the final rolling temperature is controlled at 850-890℃; The cooling steps are as follows: first, the strip after final rolling is cooled to 650-690°C at a cooling rate of ≥100°C / s, then air-cooled for 8-12s to 630-640°C, and finally cooled to the coiling temperature at a cooling rate of 30-50°C / s. After the above treatment, the microstructure of the strip steel is pearlite matrix + island-shaped dispersed ferrite, and there is no network ferrite.

[0008] Furthermore, the C content of the 65Mn fine stamping steel is 0.62% to 0.72%.

[0009] Furthermore, the composition and mass percentage of the 65Mn fine stamping steel are as follows: C 0.62%~0.72%, Si 0.2%~0.3%, Mn 0.5%~1.5%, P≤0.015%, S≤0.005%, Als 0.02%~0.05%, N≤0.006%, with the balance being Fe and unavoidable impurities.

[0010] Furthermore, in the winding step, the winding temperature is 580–620°C, and the winding is followed by air cooling.

[0011] Furthermore, the ferrite content in the strip structure is 1% to 3%.

[0012] Furthermore, the pearlite matrix is ​​a two-scale pearlite.

[0013] The beneficial effects of adopting the above technical solution are as follows: (1) Eliminate the cause of strip breakage from the source: Through segmented cooling and precise control, a small amount of ferrite is achieved and it is distributed in an island-like manner. The ferrite content can be controlled at 1% to 3%, completely eliminating network ferrite. This suppresses the initiation and expansion of cracks in the five-stand cold continuous rolling process from the source, avoids preferential cracking of ferrite under high tension and high reduction conditions in five-stand cold continuous rolling, and reduces the strip breakage rate. The strip breakage rate in cold continuous rolling is reduced from 3% to 8% to below 1%, while ensuring the matching of material strength and toughness to meet the requirements of fine stamping.

[0014] (2) Strength and toughness match the requirements of fine stamping: The final microstructure of the hot-rolled steel strip is double-scale pearlite + a small amount of island ferrite, with a yield strength of 430-550MPa, tensile strength of 845-1050MPa, and elongation of 10%-15%, which takes into account both high strength and good cold working toughness, and meets the performance requirements of fine stamping steel; for fine stamping steel 65Mn with a width of less than 1300mm, the rolling force can be controlled at 15-22MN under the condition of 40%±5% reduction rate during cold continuous rolling, and most five-stand continuous rolling mills can roll it smoothly.

[0015] (3) Low cost and easy to industrialize: No need to add microalloying elements such as Cr and Nb, the microstructure can be controlled by optimizing the hot rolling cooling process, without increasing production costs; the process parameters are compatible with existing hot rolling mills, no additional equipment modification is required, and it is easy to promote on a large scale.

[0016] (4) Strong structural stability: Within the composition range of the present invention, the fluctuation of composition does not affect the final structure and properties, the process error tolerance is high, and the production stability is good; it solves the problem of strip breakage caused by high tension and high reduction in five-stand cold continuous rolling, and the strip breakage rate is reduced to less than 1%. It takes into account the strength and toughness of the material, does not require micro-alloying, has low cost, and is easy to promote industrialization. Attached Figure Description

[0017] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0018] Figure 1 This is a diagram of the internal structure of the hot-rolled steel strip obtained in Embodiment 1 of the present invention. Detailed Implementation

[0019] The present invention will now be described in further detail with reference to specific embodiments.

[0020] The hot rolling method for 65Mn precision stamping steel that inherently prevents strip breakage during cold rolling includes the following steps: (1) The composition and mass percentage of the 65Mn fine stamping steel are as follows: C 0.62%~0.72%, Si 0.2%~0.3%, Mn 0.5%~1.5%, P≤0.015%, S≤0.005%, Als 0.02%~0.05%, N≤0.006%, with the balance being Fe and unavoidable impurities. Within this composition range, the microstructure and mechanical properties are stable, and composition fluctuations do not affect the final microstructure control effect; the above composition can ensure that, without the addition of any alloys, the pearlite phase transformation precedes the ferrite phase transformation when using the following hot rolling process.

[0021] (2) Hot rolling steps: After the slab is heated to 1150-1200℃, rough rolling and finish rolling are carried out. The final rolling temperature is controlled at 850-890℃, which can ensure that the austenite grains are uniformly refined during the rolling process, providing a uniform microstructure basis for the subsequent pearlite phase transformation.

[0022] (3) Cooling steps: The cooling mode is a combination of laminar flow cooling in the first stage + air cooling + laminar flow cooling in the second stage.

[0023] The first stage of laminar flow cooling: the strip after final rolling is cooled by water spray to 650-690℃ at a cooling rate of ≥100℃ / s. This temperature range is lower than the temperature of steel grade A1 (724℃). The large supercooling promotes the preferential transformation of austenite to pearlite phase. Large pearlite with large interlamellar spacing and high carbon content is generated in the high temperature range of 650-690℃. The volume fraction of the generated large pearlite in the internal structure is 60%-70%.

[0024] Air cooling: After the first stage of laminar flow cooling is completed, air cooling is carried out for 8-12 seconds to cool to 630-640℃. During this stage, the high-carbon pearlite clusters continue to grow through phase transformation, further increasing the volume fraction of high-temperature pearlite, while inhibiting ferrite grain boundary connections and avoiding the formation of network ferrite prototypes.

[0025] The second stage involves laminar flow cooling: water spraying at a cooling rate of 30–50°C / s to achieve a winding temperature of 580–620°C. This process nucleates and generates small-interlaminar pearlite with small interlaminar spacing and low carbon content around the large lamellar pearlite at high temperatures. The resulting small-interlaminar pearlite accounts for 28%–38% of the volume fraction in the internal structure. The large lamellar pearlite promotes the rapid nucleation and growth of the small-interlaminar pearlite, crowding out the space for ferrite precipitation and strictly controlling the ferrite content to 1%–3%.

[0026] (4) Winding steps: After the second stage of laminar flow cooling is completed, the winding temperature is 580-620℃, and after winding, it is air-cooled to room temperature.

[0027] (5) The final microstructure and volume fraction of the obtained hot-rolled steel strip are: 60%–70% large lamellar pearlite + 28%–38% small lamellar pearlite + 1%–3% island-like dispersed ferrite. The ferrite is cut and separated by the pearlite, and there is no network ferrite structure. The mechanical properties of the obtained hot-rolled steel strip are: yield strength 430–550 MPa, tensile strength 845–1050 MPa, elongation 10%–15%. During subsequent cold continuous rolling, under a reduction rate of 40% ± 5%, the rolling force can be controlled at 15–22 MN, which meets the rolling force requirements of most five-stand cold continuous rolling mills. The strip breakage rate of five-stand cold continuous rolling is ≤1%. Example 1

[0028] (1) Composition (mass fraction): C 0.72%, Si 0.25%, Mn 1.0%, P 0.012%, S 0.004%, Als 0.035%, N 0.005%, balance Fe and unavoidable impurities; (2) Hot rolling: The slab is heated to 1200℃ and then rough rolled and finished rolled, with a final rolling temperature of 890℃; (3) Cooling: First stage laminar flow cooling, cooling rate 120℃ / s, cooling to 690℃; air cooling for 10s, cooling to 635℃; second stage laminar flow cooling, cooling rate 40℃ / s, cooling to 620℃; (4) Winding: Winding temperature 620℃, air cool to room temperature after winding; (5) Organization and performance: Figure 1 This is an internal microstructure diagram of the hot-rolled steel strip obtained in this embodiment, wherein the gray blocky structure is large lamellar pearlite, the black blocky structure is small lamellar pearlite, and the bright white dotted structure is island-shaped dispersed ferrite; Figure 1 It can be seen that the internal structure of the obtained hot-rolled steel strip is 68% large lamellar pearlite, 29% small lamellar pearlite, and 3% ferrite (island-like); the yield strength is 550MPa, the tensile strength is 845MPa, and the elongation is 15%; there is no strip breakage problem in the five-stand cold continuous rolling. Example 2

[0029] (1) Composition (mass fraction): C 0.68%, Si 0.28%, Mn 1.2%, P 0.010%, S 0.003%, Als 0.04%, N 0.004%, balance Fe and unavoidable impurities; (2) Hot rolling: The slab is heated to 1170℃ and then rough rolled and finished rolled, with a final rolling temperature of 880℃; (3) Cooling: First stage laminar flow cooling, cooling rate 150℃ / s, cooling to 690℃; air cooling for 12s, cooling to 630℃; second stage laminar flow cooling, cooling rate 50℃ / s, cooling to 580℃; (4) Winding: Winding temperature 580℃, air cool to room temperature after winding; (5) Structure and properties: 65% large lamellar pearlite, 34% small lamellar pearlite, 1% ferrite (island-like); yield strength 540MPa, tensile strength 1050MPa, elongation 10%; no strip breakage problem in five-stand cold continuous rolling. Example 3

[0030] (1) Composition (mass fraction): C 0.62%, Si 0.2%, Mn 0.8%, P 0.015%, S 0.005%, Als 0.02%, N 0.006%, balance Fe and unavoidable impurities; (2) Hot rolling: The slab is heated to 1150℃ and then rough rolled and finished rolled, with a final rolling temperature of 850℃; (3) Cooling: First stage laminar flow cooling, cooling rate 100℃ / s, cooling to 650℃; air cooling for 8s, cooling to 640℃; second stage laminar flow cooling, cooling rate 35℃ / s, cooling to 600℃; (4) Winding: Winding temperature 600℃, air cool to room temperature after winding; (5) Structure and properties: 62% large lamellar pearlite, 36% small lamellar pearlite, 2% ferrite (island-like); yield strength 430MPa, tensile strength 920MPa, elongation 13%; no strip breakage problem in five-stand cold continuous rolling. Example 4

[0031] (1) Composition (mass fraction): C 0.65%, Si 0.22%, Mn 1.5%, P 0.008%, S 0.002%, Als 0.05%, N 0.003%, balance Fe and unavoidable impurities; (2) Hot rolling: The slab is heated to 1180℃ and then rough rolled and finished rolled, with a final rolling temperature of 870℃; (3) Cooling: First stage laminar flow cooling: cooling rate 130℃ / s, cooling to 670℃; air cooling 9s, cooling to 638℃; second stage laminar flow cooling: cooling rate 45℃ / s, cooling to 590℃; (4) Winding: Winding temperature 590℃, air cool to room temperature after winding; (5) Structure and properties: 70% large lamellar pearlite, 28.5% small lamellar pearlite, 1.5% ferrite (island-like); yield strength 490MPa, tensile strength 980MPa, elongation 11.5%; no strip breakage problem in five-stand cold continuous rolling. Example 5

[0032] (1) Composition (mass fraction): C 0.70%, Si 0.3%, Mn 0.5%, P 0.014%, S 0.0045%, Als 0.03%, N 0.0055%, balance Fe and unavoidable impurities; (2) Hot rolling: The slab is heated to 1165℃ and then rough rolled and finished rolled, with a final rolling temperature of 860℃; (3) Cooling: First stage laminar flow cooling, cooling rate 110℃ / s, cooling to 660℃; air cooling 11s, cooling to 632℃; second stage laminar flow cooling, cooling rate 30℃ / s, cooling to 610℃; (4) Winding: Winding temperature 610℃, air cool to room temperature after winding; (5) Structure and properties: 66% large lamellar pearlite, 31.5% small lamellar pearlite, 2.5% ferrite (island-like); yield strength 460MPa, tensile strength 890MPa, elongation 14%; no strip breakage problem in five-stand cold continuous rolling.

Claims

1. A hot rolling method for 65Mn precision stamping steel that can prevent strip breakage during cold continuous rolling, characterized in that: Includes hot rolling, cooling, and coiling steps; The hot rolling step: the final rolling temperature is controlled at 850-890℃; The cooling steps are as follows: first, the strip after final rolling is cooled to 650-690°C at a cooling rate of ≥100°C / s, then air-cooled for 8-12s to 630-640°C, and finally cooled to the coiling temperature at a cooling rate of 30-50°C / s. After the above treatment, the microstructure of the strip steel is pearlite matrix + island-shaped dispersed ferrite, and there is no network ferrite.

2. The hot rolling method for 65Mn fine stamping steel that can prevent strip breakage during cold continuous rolling according to claim 1, characterized in that: The carbon content of the 65Mn fine stamping steel is 0.62% to 0.72%.

3. The hot rolling method for 65Mn fine stamping steel that can prevent strip breakage during cold continuous rolling according to claim 2, characterized in that: The composition and mass percentage of the 65Mn fine stamping steel are as follows: C 0.62%~0.72%, Si 0.2%~0.3%, Mn 0.5%~1.5%, P≤0.015%, S≤0.005%, Als 0.02%~0.05%, N≤0.006%, with the balance being Fe and unavoidable impurities.

4. The hot rolling method for 65Mn fine stamping steel that can prevent strip breakage during cold continuous rolling according to claim 1, characterized in that: The winding step is performed at a temperature of 580–620°C, followed by air cooling.

5. The hot rolling method for 65Mn fine stamping steel that can prevent strip breakage during cold continuous rolling according to claim 1, characterized in that: The ferrite content in the strip structure is 1% to 3%.

6. A hot rolling method for 65Mn fine stamping steel that can prevent strip breakage during cold continuous rolling, as described in any one of claims 1-5, characterized in that: The pearlite matrix is ​​a two-scale pearlite.