A 38MnVS6 non-quenched and tempered steel narrow-width nitrogen control whole-process coordinated process based on double-factor nitrogen quantity prediction
By employing a collaborative process throughout the entire process and a two-factor nitrogen content prediction model, the problem of unstable nitrogen content in 38MnVS6 steel was solved, achieving narrow-range control of nitrogen content in the finished product. This improved the consistency of the steel's strength and fatigue performance, making it suitable for high-end automotive parts.
Patent Information
- Application Number
- CN202611521079.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-24
AI Technical Summary
In existing industrial production processes, the nitrogen content of 38MnVS6 steel is not easily controlled, resulting in large fluctuations in the nitrogen content and mechanical properties of the finished product, which cannot meet the quality requirements of high-end automotive parts.
A collaborative process based on two-factor nitrogen content prediction is adopted, including converter smelting, LF refining, RH vacuum degassing and hot rolling processes. Through a two-factor nitrogen content pre-compensation model and gradient vacuum operation, combined with the use of vanadium-nitrogen alloy, the nitrogen content of liquid steel is precisely controlled. With the optimization of hot rolling process, a narrow range of stable control of nitrogen content in the finished product is achieved.
This achieved stable control of the nitrogen content in the finished product within the range of 150–200 ppm, improving the consistency of the steel's strength, fatigue life, and machinability, reducing the discrete fluctuations in mechanical properties, and meeting the requirements for high-end automotive parts.
Smart Images

Figure CN123149245A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of special steel long-process smelting and rolling technology, and in particular relates to a synergistic process for narrow-range nitrogen control of 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction. Background Technology
[0002] 38MnVS6 is a widely used vanadium microalloyed free-machining non-quenched and tempered steel. It achieves strengthening through nanoscale V(C,N) precipitates, eliminating the need for subsequent quenching and tempering heat treatment. It combines high strength, long fatigue life, and excellent machinability, making it widely used in heavy-duty components of automotive powertrains. Nitrogen is the core element for precipitation strengthening in this steel. High-end applications require the nitrogen content of the finished product to be stably controlled within a narrow range of 150–200 ppm. Fluctuations in nitrogen content directly affect the matching of the steel's strength, toughness, fatigue performance, and machinability.
[0003] In existing industrial production processes, nitrogen control of 38MnVS6 suffers from several inherent defects. The technical solutions for each process are fragmented, failing to form a systematic closed-loop control system. Traditional processes only regulate the total nitrogen content within the steelmaking process, completely ignoring the high-temperature heating of the billet and the rolling deformation process, which cause the precipitated V(C,N) to dissolve and decompose into dissolved V and dissolved N, resulting in the loss of effective precipitated nitrogen. Furthermore, the rolling compression ratio is not used as a pre-calculation parameter for nitrogen batching in steelmaking, leading to a poor match between the preset nitrogen amount in steelmaking and the effective precipitated nitrogen in the rolled product, resulting in significant fluctuations in the nitrogen content and mechanical properties of the finished product.
[0004] Conventional RH processes are divided into two modes: full-process high vacuum and full-process nitrogen circulation. Full-process high vacuum has excellent dehydrogenation effect, but a large amount of nitrogen is removed from the liquid steel, and the nitrogen recovery rate fluctuates greatly, making it impossible to stably maintain the target range of 150-200ppm. Full-process nitrogen circulation can increase nitrogen content, but the hydrogen content in the steel exceeds the standard, which can easily cause hydrogen-induced cracking of parts and cannot meet the quality requirements of high-end automotive parts.
[0005] Current processes often use manganese nitride cored wire for late-stage nitrogen replenishment in LF (fermentation recovery) processes. This industrial manganese nitride cored wire has a composition of 72%–78% Mn and 4.0%–6.0% N, with a Mn / N mass ratio of approximately 15:1. Under a precise nitrogen window of 150–200 ppm, LF requires replenishment of 80–120 ppm nitrogen, simultaneously introducing 0.12%–0.18% manganese. The upper limit of manganese content in 38MnVS6 is only 1.50%, and the converter tapping steel already has a manganese content of 1.35%–1.45%, which easily leads to excessive manganese content and amplifies hardenability fluctuations. Simultaneously, localized manganese enrichment promotes the growth of strip-shaped MnS inclusions, becoming a source of fatigue crack initiation and significantly reducing the fatigue life of components. Furthermore, the introduction of free nitrogen by manganese nitride disrupts the V / N ratio, leading to VN precipitation strengthening failure.
[0006] The industry standard for billet heating is 1180-1220℃, with a high-temperature holding time of over 120 minutes. Due to the high heating temperature and long holding time, the fine nano-V(C,N) precipitated in the molten steel in the early stage are completely dissolved back. The driving force for precipitation during the rolling process is insufficient, and the proportion of coarse precipitates increases significantly. Even if the total nitrogen of the finished product meets the standard, the strength and fatigue performance of the steel are still severely inconsistent.
[0007] In summary, existing technologies have not yet formed a fully fluidized nitrogen system adapted to the narrow nitrogen window of 150-200ppm for 38MnVS6 steel, and therefore cannot achieve stable mass production of high-end products of this steel grade. Summary of the Invention
[0008] To address some or all of the technical problems existing in the prior art, this application provides a collaborative process for narrow-range nitrogen control of 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction.
[0009] This application provides a collaborative process for narrow-range nitrogen control in 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction. The process includes converter smelting, LF refining, RH vacuum degassing, continuous casting, and hot rolling. The LF refining process uses a two-factor nitrogen pre-compensation mathematical model, combined with the estimated nitrogen loss amount under RH gradient vacuum and the rolling nitrogen loss compensation value corresponding to the total rolling compression ratio K, to calculate the target nitrogen content at the LF endpoint, and adds vanadium-nitrogen alloy to adjust the nitrogen content of the liquid steel. The RH vacuum degassing process is performed in three stages of gradient vacuum timing: the first stage controls the ultimate vacuum to ≤67Pa and holds the pressure for 3-5 minutes; the second stage controls the medium vacuum to 1500-2500Pa and holds the pressure for 6-10 minutes, while reducing the steel circulation flow rate by 20%; the third stage involves online sampling of the molten steel before breaking the vacuum, and when the nitrogen content is below 150ppm, the circulating gas in the impregnation tube is briefly switched to nitrogen for nitrogen replenishment, with a replenishment time of ≤90s, and the gas is switched back to argon after the nitrogen content reaches the standard. The hot rolling process involves heating the billet, controlling the upper limit of the billet heating temperature and the total duration of high-temperature holding, and then sequentially performing rolling and post-rolling controlled cooling treatment. The finished 38MnVS6 non-quenched and tempered steel produced has the following chemical composition by mass fraction: C 0.36%~0.40%, Si 0.60%~0.75%, Mn 1.30%~1.50%, S 0.020%~0.040%, Cr 0.10~0.20%, V 0.08%~0.13%, Ti 0.010~0.030%, Als 0.010%~0.025%, P≤0.025%, N 150~200ppm, H≤2ppm, with the balance being Fe and unavoidable impurities; the V / N molar ratio of the molten steel is controlled at 3.6~4.2.
[0010] Preferably, the mathematical model formula for the LF refining dual-factor nitrogen pre-compensation is as follows: [N] LF终 =[N] 成品目标 +Δ[N] RH损失 +Δ[N] 轧制补偿(K) ; The target for [N] in the finished product is 150–200 ppm, and Δ[N] RH损失 The value represents the nitrogen loss during the RH gradient vacuum process, ranging from 40 to 80 ppm; Δ[N] 轧制补偿(K) The effective nitrogen loss compensation value for the rolling process is determined by segmenting the values according to the total rolling compression ratio K: when K < 12, the compensation is 10 ppm; when 12 ≤ K ≤ 20, the compensation is 15 ppm; when K > 20, the compensation is 25 ppm.
[0011] Preferably, the converter smelting process includes: KR hot metal pre-desulfurization to control the sulfur content of hot metal to ≤0.002%; low-nitrogen clean scrap steel with a nitrogen content of ≤40ppm is selected as the raw material, and the scrap steel ratio is ≤10%; bottom blowing argon gas is used throughout the converter smelting process, and high carbon extraction is used for one-time tapping of steel, with an end point carbon content of ≥0.12% and a nitrogen content of ≤60ppm in the liquid steel leaving the converter.
[0012] Preferably, the LF refining process involves: producing high-basicity white slag with an alkalinity of 2.8 to 3.2 during the smelting process, with submerged arc heating throughout and bottom-blown argon flow rate of 2 to 4 NL / (min·t); adding vanadium-nitrogen alloy after the molten steel has an Als ≥ 0.012%; and finely adjusting the sulfur content in the steel in the later stages of the LF process using a sulfur feeding line.
[0013] Preferably, the continuous casting process employs a double-sealed argon gas protection system with both a long nozzle and an immersion nozzle; the secondary cooling section uses a weak cooling regime.
[0014] Preferably, after the RH vacuum process is completed, the ladle is subjected to soft argon blowing treatment for 8 to 12 minutes, and the nitrogen content of the RH exiting steel is controlled at 160 to 200 ppm.
[0015] Preferably, the hot rolling process parameters are as follows: preheating zone temperature of billet ≤ 950℃, maximum temperature of soaking zone 1140~1170℃, total high temperature holding time ≤ 70min; roughing rolling start temperature 1080~1130℃, single pass reduction rate ≥ 18%; finishing rolling finish temperature 850~900℃; post-rolling cooling rate 2~4℃ / s, and natural air cooling after cooling to 600℃.
[0016] The synergistic process for narrow-range nitrogen control in the entire process of 38MnVS6 non-quenched and tempered steel based on two-factor nitrogen content prediction has the following advantages and positive effects: This application constructs an integrated nitrogen control system for the entire process from converter to LF-RH to continuous casting to hot rolling. By using a two-factor nitrogen pre-compensation model, it establishes a quantitative prediction link for nitrogen loss between steelmaking and rolling processes. Combined with the synergistic constraints of time-sharing dehydrogenation and nitrogen retention in RH, prevention of secondary nitrogen absorption in continuous casting, and temperature control and nitrogen locking in hot rolling, it avoids the problem of nitrogen loss control caused by the fragmentation of traditional processes. It stably maintains the optimal V / N molar ratio in molten steel, increases the proportion of nanoscale V(C,N) fine precipitates, and achieves narrow-range stable control of nitrogen content in finished products. Overall, it improves the consistency of steel strength, fatigue life, and machinability, and effectively suppresses the discrete fluctuations in mechanical properties. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only for further understanding of the embodiments of this application and constitute a part of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. In the drawings: Figure 1 This is an electron microscope image of the 38MnVS6 of this application; Figure 2 This is a metallographic diagram of 38MnVS6 in this application; Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions of this application will be clearly and completely described below in conjunction with specific embodiments and corresponding drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.
[0019] This application provides a collaborative process for narrow-range nitrogen control in 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction. The process includes converter smelting, LF refining, RH vacuum degassing, continuous casting, and hot rolling. Converter smelting process: KR hot metal pre-desulfurization is adopted to control the sulfur content of hot metal to ≤0.002%; low-nitrogen clean scrap steel with a nitrogen content ≤40ppm is selected for the raw materials, and the scrap steel ratio is ≤10%; bottom blowing of argon gas is used throughout the converter smelting process, and bottom blowing of nitrogen gas is prohibited; high carbon extraction is adopted for one-time tapping, and the final carbon content is ≥0.12%, eliminating post-blowing gas absorption; the nitrogen content of the molten steel leaving the converter is ≤60ppm. The converter tapping temperature is controlled at 1640~1660℃, and slag-blocking operation is performed throughout the process; deoxidation of the steel is carried out in the order of silicon-manganese, ferrosilicon, and aluminum-iron, and no nitriding alloys are added during the tapping stage, so as to build a low-nitrogen stable steel base and reduce interference from external nitrogen sources; the smelting process avoids the risk of gas absorption in molten steel caused by bottom blowing of nitrogen gas and post-blowing operation.
[0020] LF refining process: The smelting process produces high-basicity white slag with an alkalinity of 2.8 to 3.2. The entire process is carried out with submerged arc heating and bottom blowing argon flow rate of 2 to 4 NL / (min·t). After the Als of the molten steel is ≥0.012%, the nitrogen content is accurately calculated and vanadium-nitrogen alloy is added. In the later stage of the LF process, the sulfur content in the steel is finely adjusted by feeding sulfur wire. Feeding manganese nitride alloy and manganese nitride cored wire is prohibited to avoid local nitrogen segregation and bubble defects.
[0021] Current processes often use manganese nitride cored wire for LF nitrogen supplementation. The Mn / N mass ratio of this material is about 15:1. Under the narrow nitrogen window of this steel grade, nitrogen supplementation will simultaneously introduce a large amount of manganese, which can easily cause the manganese content to exceed the limit of 1.50%, resulting in uncontrolled hardenability. It will also promote the growth of strip-shaped MnS inclusions, reducing fatigue life. Free nitrogen will destroy the optimal V / N molar ratio of 3.6 to 4.2, resulting in a sharp reduction in the amount of nano VN precipitation and failure of the strengthening effect. Moreover, the rapid dissolution of manganese nitride will cause local nitrogen supersaturation, inducing defects such as subcutaneous bubbles and nozzle nodules in the billet.
[0022] This application uses a vanadium-nitrogen alloy with V≥78% and N=16%~18%, which does not introduce additional manganese elements and can naturally match the optimal precipitation range of V / N molar ratio of 3.6~4.2, and the nitrogen supplementation accuracy is controllable.
[0023] In the LF refining process, a two-factor nitrogen pre-compensation mathematical model is adopted. Combined with the nitrogen loss estimated by RH gradient vacuum and the rolling nitrogen loss compensation value corresponding to the total rolling compression ratio K, the target nitrogen content at the LF endpoint is calculated, and vanadium-nitrogen alloy is added to adjust the nitrogen content of the liquid steel. The mathematical model formula for the two-factor nitrogen pre-compensation model in LF refining is as follows: [N] LF终 =[N] 成品目标 +Δ[N] RH损失 +Δ[N] 轧制补偿(K) ; The target for [N] in the finished product is 150–200 ppm, and Δ[N] RH损失The value represents the nitrogen loss during the RH gradient vacuum process, ranging from 40 to 80 ppm; Δ[N] 轧制补偿(K) The effective nitrogen loss compensation value for the rolling process is determined by segmenting the values according to the total rolling compression ratio K: when K < 12, the compensation is 10 ppm; when 12 ≤ K ≤ 20, the compensation is 15 ppm; when K > 20, the compensation is 25 ppm.
[0024] The temperature of molten steel entering the RH station is controlled at 1595~1610℃. Through three-stage gradient vacuum time-sharing treatment, dehydrogenation, denitrification inhibition, and micro-nitrogen replenishment are completed in sequence to resolve the process contradiction between RH dehydrogenation and nitrogen preservation. The RH vacuum degassing process employs a three-stage gradient vacuum sequence: In the first stage, the ultimate vacuum is controlled to ≤67Pa, held for 3–5 minutes, prioritizing dehydrogenation of the molten steel to achieve low-hydrogen metallurgy. In the second stage, the intermediate vacuum is controlled to 1500–2500Pa, held for 6–10 minutes, while simultaneously reducing the molten steel circulation flow rate by 20%, significantly suppressing the denitrification rate and maintaining the pre-compensated nitrogen base. In the third stage, before venting, the molten steel is sampled online. When the nitrogen content is below 150ppm, the circulating gas in the impregnation tube is briefly switched to nitrogen for supplementation, with a supplementation time ≤90s. Once the nitrogen content reaches the target, argon is switched back to prevent excessive nitrogen addition and hydrogen content rebound. After the RH vacuum process is completed, the ladle undergoes soft argon blowing for 8–12 minutes. The nitrogen content of the RH-exited molten steel is controlled at 160–200ppm, reserving a small amount for continuous casting to offset nitrogen loss during subsequent continuous casting and billet heating processes.
[0025] Continuous casting process: The casting process adopts double-sealed argon protection with long nozzle and submerged nozzle to prevent secondary nitrogen absorption; the second cooling section adopts a weak cooling system to reduce macroscopic nitrogen segregation in the billet, reduce internal microcracks, and ensure the uniformity of nitrogen in the billet.
[0026] In the hot rolling process, the billet is heated, and the upper limit of the billet heating temperature and the total high-temperature holding time are controlled. Then, it is rolled and cooled after rolling. The process parameters of the hot rolling process are as follows: the billet preheating zone temperature is ≤950℃, the maximum temperature of the soaking zone is 1140~1170℃, and the total high-temperature holding time is ≤70min. This process is different from the traditional high-temperature long-time heating process, which effectively inhibits the re-dissolution and decomposition of V(C,N) and retains the effective dissolved nitrogen reserved in the steelmaking process. The rough rolling opening temperature is 1080~1130℃, and the single-pass reduction rate is ≥18%. The uniform precipitation of nano-sized V(C,N) is induced by large deformation. The finishing rolling finishing temperature is 850~900℃. The post-rolling cooling rate is 2~4℃ / s. After cooling to 600℃, it is naturally air-cooled to complete the dispersion precipitation of the remaining dissolved nitrogen, and finally locks the nitrogen content of the finished product to 150~200ppm.
[0027] The finished 38MnVS6 non-quenched and tempered steel produced has the following chemical composition by mass fraction: C 0.36%~0.40%, Si 0.60%~0.75%, Mn 1.30%~1.50%, S 0.020%~0.040%, Cr 0.10~0.20%, V 0.08%~0.13%, Ti 0.010~0.030%, Als 0.010%~0.025%, P≤0.025%, N 150~200ppm, H≤2ppm, with the balance being Fe and unavoidable impurities; the V / N molar ratio of the molten steel is controlled at 3.6~4.2.
[0028] The technical solution of this application will be further described in detail below with reference to specific embodiments.
[0029] Example 1 This embodiment uses a 100t converter steelmaking production line to produce Φ90mm 38MnVS6 hot-rolled round steel; a 320mm×420mm rectangular cross-section continuous casting billet is selected, and the total rolling compression ratio is calculated. The cross-sectional area of the billet is S1=320×420=134400mm². 2 The cross-sectional area of the finished round steel bar is S2 = π × 45 2 ≈6362mm 2 The total rolling compression ratio K = S1 / S2 ≈ 21.1 falls within the range of K > 20, and the corresponding rolling nitrogen loss compensation value is taken as 25 ppm; the target nitrogen content of the finished product is set to the midpoint of the range, 170 ppm. Based on the actual working conditions of the RH vacuum equipment in this production line, the estimated nitrogen loss of RH is taken as 55 ppm.
[0030] Converter smelting process: The raw material is molten iron that has undergone KR pre-desulfurization treatment, with a measured sulfur content of 0.0018%; the feedstock is low-nitrogen clean scrap steel with a nitrogen content of 35ppm, and the scrap steel ratio is controlled at 7.5%; the converter smelting process is carried out with bottom blowing argon gas throughout, and a high-carbon single-pass tapping operation is performed, with a final measured carbon content of 0.13%, without supplementary blowing or post-blowing to avoid post-blowing gas intake; slag is blocked throughout the tapping process, and deoxidation is added in the order of ferrosilicon, ferrosilicon, and ferroaluminum, and no nitriding alloys are added during the tapping stage; the measured nitrogen content of the molten steel leaving the converter station is 55ppm, which meets the low-nitrogen base control requirement of ≤60ppm.
[0031] LF refining process: After the LF enters the station, it is smelted to produce high-basicity white slag with an alkalinity of 3.0, and the entire process is carried out by submerged arc heating. The bottom blowing argon stirring flow rate is set to 3NL / (min·t) to homogenize the composition and temperature of the molten steel. After the measured aluminum (Als) in the molten steel reaches 0.014% and the molten steel is sufficiently deoxidized, the two-factor nitrogen pre-compensation mathematical model of this application is used to calculate the final nitrogen content of LF = finished product target 170ppm + RH loss 55ppm + rolling compensation 25ppm = 200ppm. According to the calculated target value, vanadium-nitrogen alloy is added to adjust the nitrogen content of the molten steel to 200ppm and the V / N molar ratio of the molten steel is controlled to 3.88, which is within the target range of 3.6~4.2. In the later stage of the LF process, only a small flow rate sulfur feed line is used to fine-tune the sulfur element in the steel. The final sulfur content of the molten steel is adjusted to 0.042ppm, and no other nitrogen addition operations are carried out.
[0032] RH vacuum degassing process: The measured temperature of the molten steel entering the RH station was 1605℃; a three-stage gradient vacuum sequence operation was performed. In the first stage, the ultimate vacuum was set at 62Pa, and the pressure was maintained for 4 minutes to complete the dehydrogenation of the molten steel; in the second stage, the vacuum was switched to 2000Pa, and the molten steel circulation flow rate was reduced by 20%, and the pressure was maintained for 7 minutes to inhibit the denitrification of the molten steel; in the third stage, online sampling was carried out before the vacuum was broken, and the measured nitrogen content of the molten steel was 173ppm, which was higher than the lower limit of 150ppm, so there was no need to replenish nitrogen through nitrogen circulation; after the vacuum was broken, the ladle was treated with soft argon blowing for 9 minutes to homogenize the composition and temperature of the molten steel. The measured nitrogen content of the molten steel leaving the RH station was 165ppm, which was within the control range of 160~200ppm.
[0033] Continuous casting process: The entire casting process adopts double-sealed argon protection with a long nozzle and an immersion nozzle to isolate air and prevent secondary nitrogen absorption by the molten steel; the second cooling section adopts a weak cooling system to reduce macroscopic segregation of nitrogen in the billet and reduce the generation of microcracks inside the billet.
[0034] Hot rolling process: The billet enters the heating furnace and is heated in sections with controlled temperature. The temperature of the preheating section is controlled at 950℃, the maximum heating temperature of the soaking section is 1160℃, and the total high temperature holding time is 62min. The rough rolling start temperature is 1105℃, and the single pass reduction rate of the rough rolling is 18%. The finishing rolling finish temperature is controlled at 875℃. The laminar cooling rate after rolling is set to 3℃ / s. After cooling to 600℃, it is switched to natural air cooling to complete the dispersion precipitation of the remaining dissolved nitrogen.
[0035] Finished product testing results: This example produced Φ90mm finished round steel bars. The measured nitrogen content of the finished product was 168ppm, which remained stable within the target narrow range of 150~200ppm, with a single-furnace nitrogen content fluctuation of only 3ppm; the proportion of fine V(C,N) precipitates with a size of less than 20nm in the steel reached 89%, such as... Figure 1 As shown, there are no coarse vanadium-nitrogen precipitates; as Figure 2As shown, the metallographic structure consists of pearlite and ferrite; the tensile strength of the rolled material ranges from 940 to 958 MPa, and the mechanical property fluctuation is ≤28 MPa. The steel exhibits excellent fatigue performance and machinability, meeting the mass production standards for high-end automotive pistons, crankshafts, and connecting rods.
[0036] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application.
Claims
1. A collaborative process for narrow-range nitrogen control in 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction, comprising converter smelting, LF refining, RH vacuum degassing, continuous casting, and hot rolling processes, characterized in that, The LF refining process uses a two-factor nitrogen pre-compensation mathematical model, combined with the estimated nitrogen loss amount under RH gradient vacuum and the rolling nitrogen loss compensation value corresponding to the total rolling compression ratio K, to calculate the target nitrogen content at the LF endpoint, and adds vanadium-nitrogen alloy to adjust the nitrogen content of the liquid steel. The RH vacuum degassing process is performed using a three-stage gradient vacuum sequence: the first stage controls the ultimate vacuum to ≤67Pa and holds the pressure for 3–5 minutes; the second stage controls the medium vacuum to 1500–2500Pa and holds the pressure for 6–10 minutes, while simultaneously reducing the molten steel circulation flow rate by 20%. In the third stage, before breaking the air, the molten steel is sampled online. When the nitrogen content is lower than 150 ppm, the circulating gas in the impregnation tube is briefly switched to nitrogen for nitrogen replenishment. The nitrogen replenishment time is ≤90s. After the nitrogen content reaches the standard, the gas is switched back to argon. The hot rolling process involves heating the billet, controlling the upper limit of the billet heating temperature and the total duration of high-temperature holding, and then sequentially performing rolling and post-rolling controlled cooling treatment. The finished 38MnVS6 non-quenched and tempered steel produced has the following chemical composition by mass fraction: C 0.36%~0.40%, Si 0.60%~0.75%, Mn 1.30%~1.50%, S 0.020%~0.040%, Cr 0.10~0.20%, V 0.08%~0.13%, Ti 0.010~0.030%, Als 0.010%~0.025%, P≤0.025%, N 150~200ppm, H≤2ppm, with the balance being Fe and unavoidable impurities; the V / N molar ratio of the molten steel is controlled at 3.6~4.
2.
2. The 38MnVS6 non-quenched and tempered steel narrow control nitrogen full-process synergistic process based on the double-factor nitrogen quantity prediction according to claim 1, characterized in that, The mathematical model formula for the LF refining dual-factor nitrogen pre-compensation is as follows: [N] LF终 =[N] 成品目标 +Δ[N] RH损失 +Δ[N] 轧制补偿(K) ; Wherein, [N] product target is 150-200 ppm, Δ[N] RH损失 RH gradient vacuum process nitrogen loss, 40-80 ppm; Δ[N] 轧制补偿(K) Rolling process effective nitrogen loss compensation value, according to the total compression ratio K segment value: K < 12, compensation 10 ppm; 12 ≤ K ≤ 20, compensation 15 ppm; K > 20, compensation 25 ppm.
3. The collaborative process for narrow-range nitrogen control of 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction according to claim 1, characterized in that, The converter smelting process is as follows: KR hot metal pre-desulfurization is adopted to control the S content of hot metal to ≤0.002%; low-nitrogen clean scrap steel with nitrogen content ≤40ppm is selected as the raw material, and the scrap steel ratio is ≤10%; bottom blowing argon gas is used throughout the converter smelting process, and high carbon extraction is adopted for one-time tapping of steel, with C ≥0.12% at the end point, and the nitrogen content of the liquid steel leaving the converter station is ≤60ppm.
4. The collaborative process for narrow-range nitrogen control of 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction according to claim 1, characterized in that, The LF refining process involves: producing high-basicity white slag with an alkalinity of 2.8 to 3.2 during the smelting process, with submerged arc heating throughout and bottom-blown argon flow rate of 2 to 4 NL / (min·t); adding vanadium-nitrogen alloy after the molten steel has an Als ≥ 0.012%; and fine-tuning the sulfur content in the steel in the later stages of the LF process using a sulfur feeding line.
5. The collaborative process for narrow-range nitrogen control of 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction according to claim 1, characterized in that, The continuous casting process employs a double-sealed argon gas protection system with both a long nozzle and an immersion nozzle; the secondary cooling section utilizes a weak cooling regime.
6. The collaborative process for narrow-range nitrogen control of 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction according to claim 1, characterized in that, After the RH vacuum process is completed, the ladle undergoes soft argon blowing treatment for 8 to 12 minutes, and the nitrogen content of the liquid steel leaving the RH station is controlled at 160 to 200 ppm.
7. The collaborative process for narrow-range nitrogen control of 38MnVS6 non-quenched and tempered steel based on dual-factor nitrogen content prediction according to claim 1, characterized in that, The hot rolling process parameters are as follows: preheating zone temperature of billet ≤950℃, maximum temperature of soaking zone 1140~1170℃, total high temperature holding time ≤70min; roughing rolling start temperature 1080~1130℃, single pass reduction rate ≥18%; finishing rolling finish temperature 850~900℃; post-rolling cooling rate 2~4℃ / s, and natural air cooling after cooling to 600℃.