A method for reducing transverse strip variation in silicon steel products

By setting a differentiated roughness distribution on the surface of the work roll, the problem of the single method for controlling the transverse same-plate difference of silicon steel products is solved, and the transverse same-plate difference of silicon steel products is significantly reduced, meeting the needs of high-end users. Moreover, there is no need to modify the structure of the cold rolling mill, thus improving production efficiency.

CN123149252APending Publication Date: 2026-11-24BENGANG STEEL PLATES CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611241362.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies offer limited options for controlling transverse thickness differences in silicon steel products, failing to effectively reduce them to below 0.008mm. Furthermore, they lack differentiated designs to address frictional differences between the edges and the middle of the strip, making it difficult to meet the needs of high-end users.

Method used

By setting a differentiated roughness distribution on the surface of the work roll, the roughness of the edge area is made smaller than that of the middle area, and a uniform transition area is set between the two, which reduces the friction between the edge of the strip and the roll, optimizes the rolling force distribution, and reduces the pressure concentration at the edge.

Benefits of technology

It significantly reduces the transverse thickness variation of silicon steel products, meets the requirements of high-end users, requires little investment, is quick to implement, has low risk, does not require modification of the main structure of the cold rolling mill, and improves production efficiency and industrial applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149252A_ABST
    Figure CN123149252A_ABST
Patent Text Reader

Abstract

This invention relates to the field of cold rolling technology, and more particularly to a method for reducing transverse sheet thickness variation in silicon steel products. The method involves roughening the surface of the work rolls to ensure that, in the roll surface region corresponding to the width direction of the strip, the roughness of the edge region is less than that of the middle region, and a smooth transition region with uniform roughness is provided between the edge and middle regions. The advantages of this invention are: by optimizing the surface roughness distribution of the work rolls, making the edge region roughness less than the middle region, and setting a smooth transition region between them, the friction between the strip edge and the work rolls is effectively reduced, the rolling force distribution in the width direction is optimized, and the edge pressure concentration is reduced, thereby controlling excessive thinning of the strip edge; starting from the friction state between the rolls and the strip, a differentiated roughness distribution is achieved on the surface of the work rolls through laser texturing, EDM, or shot peening processes, changing the friction characteristics of the rolling interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cold rolling technology, and in particular to a method for reducing transverse plate differences in silicon steel products. Background Technology

[0002] Cold-rolled silicon steel is a key magnetic material in motor manufacturing, and its transverse thickness difference (the maximum thickness difference between any two points in the width direction of the strip) is an important indicator of product quality. Excessive thickness difference directly affects the lamination factor of the motor, reducing motor efficiency and increasing iron loss and temperature rise. Currently, the transverse thickness difference of domestically produced cold-rolled silicon steel products is generally between 0.008mm and 0.015mm, while high-end users require a transverse thickness difference of ≤0.008mm, a standard that existing products struggle to meet.

[0003] To reduce transverse sheet thickness variation in silicon steel products, various technical solutions have been proposed. For example, Chinese utility model patent CN219392394U discloses "a device for controlling transverse sheet thickness variation in cold-rolled non-oriented silicon steel," which includes a five-stand six-roll continuous rolling mill, upper and lower intermediate rolls with roll shifting function, and upper and lower work rolls with special roll surface profiles. However, the roll surface profiles do not adjust with changes in strip width and thickness, and the sheet thickness variation control level still does not meet the user's requirement of ≤0.008mm.

[0004] In their paper "Control Technology of Edge Drop and Plate Difference in Cold-Rolled Silicon Steel" (First Heavy Machinery Technology, 2021, pp. 9-12), Sun Jianting et al. introduced a method to control edge drop and plate difference in silicon steel by modifying the work roll bending and shifting device. This method mainly relies on a single roll shifting control method and does not effectively control the plate difference of hot-rolled incoming materials, resulting in a still high plate difference in the final product.

[0005] In summary, existing technologies still have the following shortcomings in controlling transverse variations within the same plate of silicon steel products: 1. The control methods are limited, relying mainly on mechanical structures or roller adjustment, and lacking precise control over the friction state of the rolling interface. 2. The design did not take into account the frictional differences between the edge and middle areas of the strip. 3. It is impossible to reliably and stably reduce the transverse thickness difference of silicon steel products to below 0.007mm, which makes it difficult to meet the needs of high-end users.

[0006] Therefore, there is an urgent need to develop a new method to effectively reduce the transverse difference between the same strip and the silicon steel product, especially a control method that optimizes the surface roughness distribution of the work roll, reduces the friction of the strip edge, and improves the distribution of rolling force. Summary of the Invention

[0007] The purpose of this invention is to provide a method for reducing the transverse thickness difference of silicon steel products. By setting a differentiated roughness distribution on the surface of the work roll, the roughness of the edge area is made smaller than that of the middle area, and a uniform transition area is set between the two to reduce the friction between the edge of the strip and the roll, optimize the rolling force distribution, reduce the pressure concentration at the edge, thereby controlling the thinning of the strip edge, reducing the transverse thickness difference of silicon steel products, and meeting the strict requirements of high-end users for thickness difference.

[0008] To achieve the above objectives, the present invention provides the following technical solution: A method for reducing transverse thickness variation in silicon steel products includes: The surface roughness of the work rolls for cold-rolled silicon steel is treated so that the roughness of the edge region of the work roll is less than that of the middle region in the roll surface area corresponding to the width direction of the strip, and a transition area with uniform roughness transition is provided between the edge region and the middle region.

[0009] The edge area corresponds to the area within 25mm of each side edge in the width direction of the strip. This area is removed during the subsequent edge trimming process.

[0010] The roughness of the edge region is 1 / 5 of the roughness value of the middle region.

[0011] The length of the transition zone is 8~12mm, and its location is 15~25mm from the edge of the strip.

[0012] The roughness of the intermediate region is 1.0–1.5 μm; The roughness of the edge region is 0.2–0.3 μm; The roughness of the transition region is 0.25–1.3 μm.

[0013] The formula for calculating the maximum roughness length L in the middle region of the work roll is: L = B - 2b; in: B represents the strip width, in mm; b represents the width of the edge area, in mm, and the value of b ranges from 20 to 30 mm.

[0014] When the strip width B=1250mm and b=25mm, the maximum roughness length L in the middle region is 1200mm.

[0015] Roll surface roughness treatment methods include laser roughening, electrical discharge machining, or shot peening.

[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. By optimizing the surface roughness distribution of the work roll, the roughness of the edge area is made smaller than that of the middle area, and a smooth transition area is set between the two. This effectively reduces the friction between the strip edge and the work roll, optimizes the distribution of rolling force in the width direction, reduces the concentration of edge pressure, and thus controls the excessive thinning of the strip edge. 2. Existing technologies mostly rely on mechanical structure adjustments (such as skewed rolls, bent rolls, conical rolls, etc.), with limited control methods and high modification costs. This invention takes a different approach, starting from the friction state between the rolls and the strip, and using laser texturing, EDM or shot peening processes to achieve a differentiated roughness distribution on the surface of the work rolls, fundamentally changing the friction characteristics of the rolling deformation zone. 3. No modification to the main structure of the existing cold rolling mill is required; only the surface treatment process of the work rolls needs to be optimized to achieve a significant reduction in the same-plate difference. Compared with the existing technologies that require modification of the bending and shifting device and addition of the shifting roll system, this invention has the outstanding advantages of low investment, fast implementation and low risk. 4. Taking into full account the actual production situation, for the 1250mm wide silicon steel products, which account for as much as 85.6%, the length of the large roughness in the middle area of ​​the working roll is fixed at 1200mm, which can realize centralized production and improve production efficiency. At the same time, for other widths of strip steel, the spare roll strategy can be flexibly adapted, which has good industrial practicality and promotion value. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the surface roughness distribution of the work roll. Detailed Implementation

[0018] The present invention will now be described in detail with reference to the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.

[0019] The following embodiments are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operation processes. However, the scope of protection of the present invention is not limited to the following embodiments. Unless otherwise specified, the methods used in the following embodiments are conventional methods.

[0020] Example 1:

[0021] A method for reducing transverse thickness variation in silicon steel products, comprising the following steps: I. Surface roughness treatment of the work roll; After the work roll is ground, the surface roughness is differentiated during laser roughening, EDM, or shot peening treatment of the work roll surface: 1. The surface roughness of the work rolls within 25mm of each side of the strip is set to be less than that of the rolls in the middle area. This area will be removed during the edge trimming process of the rewinding unit. That is, this part of the strip edge (25mm wide on each side) will be cut off in subsequent processes and is not part of the final product. Therefore, the surface quality requirements for this area can be appropriately relaxed, and differentiated roughness design is allowed to facilitate the optimization of the rolling process.

[0022] 2. The roughness value of the edge region is 1 / 5 of the roughness value of the middle region; 3. A transition area with uniform roughness is provided between the edge area and the middle area. The length of the transition area is 10mm, and the location of the transition area is 15-25mm away from the edge of the strip.

[0023] By reducing the roughness of the work roll surface area corresponding to a distance of 25mm from both sides of the strip, the friction between the strip edge and the roll can be effectively reduced.

[0024] II. Explanation of working principle; During cold rolling, even when the same rolling force is applied, the distribution of rolling force in the width direction differs between roll surfaces with different roughnesses. Roll surfaces with higher roughness generate greater local friction during rolling, causing the rolling force to concentrate in certain areas of the workpiece rather than be evenly distributed.

[0025] When the roll surface roughness is low, the coefficient of friction between the roll and the strip surface is relatively small, resulting in a more uniform resistance to metal flow in the width direction of the strip. During the rolling process, the strip can deform more smoothly under the action of the roll, and the rolling force is more evenly distributed in the width direction, making it less likely to have significant differences in local pressure that are too high or too low.

[0026] According to rolling theory, the greater the friction between the workpiece and the rolls, the greater the rolling pressure; conversely, the smaller the friction, the smaller the rolling pressure. Therefore, reducing the friction between the rolls and the strip edge can effectively lower the coefficient of friction, allowing for smoother metal flow and helping to reduce excessive rolling pressure caused by high frictional resistance at the edge. Reducing the rolling pressure applied to the strip edge by the rolls decreases edge pressure concentration, thereby controlling the thinning of the strip edge during cold rolling.

[0027] III. Specific Implementation Parameters; 1. Reduce the friction between the strip edge and the rolls. By setting the roughness at both ends of the work roll surface to be less than that in the middle, the friction force at the edge of the strip can be reduced.

[0028] During laser texturing of the work roll, the length L of the central region with the highest roughness along the length of the roll body is determined by the following formula: L = B - 2b; in: B represents the strip width, in mm; b represents the width of the edge area, in mm, b = 25 mm.

[0029] When the strip width B = 1250 mm and b = 25 mm, the maximum roughness length of the middle region of the work roll is: L = 1250 - 2 × 25 = 1200 mm; After a uniform transition of 10mm along the roughness region at both ends of the work roll (the width of which varies with the amount of trimming, typically 25mm), the edge roughness reaches 1 / 5 of the roughness value of the middle region. During the rolling process, the friction between the work roll and the contact area between the strip and the two sides is relatively small, and the rolling pressure is relatively reduced, thereby reducing the edge thinning of the strip.

[0030] In actual production, 1250mm wide silicon steel products account for 85.6% of single-stand production. Therefore, the maximum roughness length in the middle region of the work roll can be fixed at 1200mm and produced centrally. For other strip widths, spare work rolls with different maximum roughness lengths L in the middle region are used. For example, for 1150mm wide strip, the maximum roughness length in the middle region of the work roll is 1100mm.

[0031] 2. Determination of work roll roughness parameters; The maximum surface roughness (Ra) of the middle region of the working roll is 1.0–1.5 μm; The surface roughness (Ra) at both ends of the working roll is 0.2–0.3 μm; The roughness (Ra) of the transition area of ​​the working roll is 0.25–1.3 μm.

[0032] IV. Comparison of the effects of the present invention with existing technologies; A comparative cold-rolling test was conducted using silicon steel with a sheet thickness difference of δh = 0.015 mm from hot-rolled incoming materials. 1. After cold rolling using existing technology (one-way conical roll type and axial movement method of intermediate roll), the transverse difference between the same plate is 0.008mm; 2. By using both existing technology and this method for cold rolling, the transverse difference between the same plate is reduced to 0.0067mm.

[0033] The above results demonstrate that the transverse same-plate variation of silicon steel products is significantly reduced, which is superior to the control level of existing technologies.

[0034] Figure 1 This is a schematic diagram showing the distribution of surface roughness of the work roll along the length of the roll body. Along the length of the work roll body, from the middle area to the two side areas, they are: middle area, transition area, and side area. Middle region: The middle part corresponding to the width direction of the strip has a larger surface roughness, with an Ra value of 1.0 to 1.5 μm; Transition region: Located between the middle region and the edge region, with a length of 10 mm and a position 15-25 mm away from the edge of the strip, its roughness transitions uniformly from 1.3 μm in the middle region to 0.25 μm in the edge region; Edge region: The area within 25mm of each side edge in the width direction of the strip has a smaller roll surface roughness, with an Ra value of 0.2 to 0.3 μm, which is about 1 / 5 of the roughness value of the middle region.

[0035] Figure 1 The paper clearly shows the correspondence between the strip width direction and the surface roughness distribution of the work roll, as well as the position, length and roughness variation trend of each region.

[0036] Example 2:

[0037] In this embodiment, a method for reducing transverse strip width variation in silicon steel products does not rely on a fixed differential distribution of the physical roughness of the work roll surface. Instead, it employs a dynamic local friction coefficient control system based on real-time strip width detection, specifically including: 1. Configure the work rollers; A work roll with uniform high roughness is used, with a surface roughness Ra of 1.0 to 1.5 μm, eliminating the need for regional roughness differentiation treatment.

[0038] 2. Real-time detection of strip width; Laser or vision sensors are installed at the entrance of the cold rolling mill to detect the width of the strip entering the mill and the lateral position of the strip on the rolls in real time and continuously, and the detection data is transmitted to the control unit.

[0039] 3. Calculate the area requiring regulation; Based on the received strip width data, the control unit calculates the area where the friction coefficient needs to be reduced using the following formula: Edge region location = strip edge location; The edge area is defined as 25mm inward from the edge of the strip. The transition zone range is 15mm to 25mm inward from the edge of the strip (i.e., the transition zone is located inside the edge area and has a length of 10mm). The specific calculation process is as follows: set up: The detected strip width is B (unit: mm); The transverse centerline position of the strip on the roll is C (unit: mm); The left edge of the strip is located at ; The right edge of the strip is ; The areas where the coefficient of friction needs to be reduced are: Left side area: mm; Left transition area: mm; Right side area: mm; Right transition area: mm; Based on the above calculation results, the control unit determines the specific nozzle positions and ranges on the work roller where friction modifier needs to be sprayed.

[0040] 4. Dynamically spray friction modifier; A multi-channel precision friction modifier spraying system is arranged along the width of the work roll. This system contains a series of independently controllable micro-nozzles, each corresponding to a specific area on the work roll.

[0041] Based on the control area calculated in step 3, the control unit sends a command to the nozzle at the corresponding position to precisely spray a friction modifier with lubricating properties (such as rolling oil or additives with a specific formulation).

[0042] The specific spraying strategy is as follows: Edge areas: The nozzles spray the full amount to form a complete lubricating film, reducing the coefficient of friction to the target value; Transition zone: By adjusting the amount of coating or the concentration of the modifier, a smooth and gradual change in the coefficient of friction can be achieved. For example, from the edge area towards the inside, the amount of coating decreases linearly from 100% to 0%, so that the coefficient of friction gradually transitions from a low value in the edge area to a high value in the middle area; Middle area: No friction modifier is applied to maintain the original high coefficient of friction of the work roll.

[0043] 5. Dynamic feedback and real-time adjustment; During the rolling process, the control unit continuously receives data from the strip width detection module. When the strip width changes (e.g., switching from 1250mm to 1150mm), the control unit recalculates the area to be adjusted in real time and immediately adjusts the nozzle opening range and spraying amount of the spraying system to ensure that the friction coefficient adjustment area always precisely corresponds to the current strip edge position.

[0044] 6. Effect verification; Cold rolling test was conducted on silicon steel with a sheet thickness difference of δh = 0.015 mm from hot-rolled incoming material: Test conditions: The strip width varied continuously within the range of 1150mm to 1250mm, and the work rolls were not replaced; Test results: The transverse thickness difference of the cold-rolled silicon steel products was 0.0065 to 0.0070 mm, all of which were less than 0.007 mm.

[0045] 7. It has a positive effect; It has the following beneficial effects: No spare work rolls required: A single work roll with uniform roughness can accommodate the production of strips of various widths, significantly reducing the manufacturing cost and inventory of work rolls; Reduce downtime: Avoid production line shutdowns caused by changing work rollers, and improve equipment utilization and production efficiency; Real-time dynamic response: The control area can be automatically adjusted according to the real-time changes in strip width, which is especially suitable for flexible production lines with multiple varieties and small batches. High control precision: By precisely controlling the amount and concentration of coating, a continuous and smooth gradual change in the coefficient of friction can be achieved, resulting in a more uniform distribution of rolling force.

Claims

1. A method for reducing transverse plate variation in silicon steel products, characterized in that, include: The surface roughness of the work rolls for cold-rolled silicon steel is treated so that the roughness of the edge region of the work roll is less than that of the middle region in the roll surface area corresponding to the width direction of the strip, and a transition area with uniform roughness transition is provided between the edge region and the middle region.

2. The method for reducing transverse plate variation in silicon steel products according to claim 1, characterized in that, The aforementioned edge region corresponds to the area within 25mm of each side edge in the width direction of the strip, and this region is removed during subsequent edge trimming.

3. The method for reducing transverse plate variation in silicon steel products according to claim 1, characterized in that, The roughness of the edge region is 1 / 5 of the roughness value of the middle region.

4. The method for reducing transverse plate variation in silicon steel products according to claim 1, characterized in that, The length of the transition area is 8-12mm, and its location is 15-25mm from the edge of the strip.

5. The method for reducing transverse plate variation in silicon steel products according to claim 1, characterized in that: The roughness of the intermediate region is 1.0–1.5 μm; The roughness of the edge region is 0.2–0.3 μm; The roughness of the transition region is 0.25–1.3 μm.

6. The method for reducing transverse plate variation in silicon steel products according to claim 1, characterized in that, The formula for calculating the maximum roughness length L in the middle region of the work roll is: L = B - 2b; in: B represents the strip width, in mm; b represents the width of the edge area, in mm, and the value of b ranges from 20 to 30 mm.

7. A method for reducing transverse plate variation in silicon steel products according to claim 6, characterized in that, When the strip width B=1250mm and b=25mm, the maximum roughness length L in the middle region is 1200mm.

8. A method for reducing transverse plate variation in silicon steel products according to claim 1, characterized in that, The roller surface roughness treatment methods include laser roughening, electrical discharge machining, or shot peening.

Citation Information

Patent Citations

  • Glasses frame capable of preventing lenses from falling off