A method for controlling the reduction of edge cracks of normalizing pre-cutting of hot-rolled raw materials of new energy non-oriented silicon steel

By pre-strengthening the hot-rolled edge, precisely controlling the normalizing temperature field, and optimizing the pre-shearing process, the problems of coarse grains and microcracks at the edge of non-oriented silicon steel after normalizing have been solved, achieving high yield and production stability. This method is suitable for the pre-shearing treatment of hot-rolled raw materials for new energy non-oriented silicon steel.

CN123149254APending Publication Date: 2026-11-24INNER MONGOLIA BAOTOU STEEL UNION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611171755.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-04
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

After normalization, the grains at the edges of the hot-rolled raw material for non-oriented silicon steel in new energy are coarse, which easily leads to microcracks during pre-shearing. This causes cracks to propagate during cold rolling, seriously affecting production stability and yield.

Method used

By pre-strengthening the edge of hot-rolled raw materials, precisely controlling the normalizing temperature field, optimizing the pre-shearing process parameters, and passivating the edge microcracks, including edge temperature control, the use of heat shields, segmented cooling, setting shearing parameters, and edge strengthening treatment, the coarsening of edge grains and the generation of microcracks are suppressed.

Benefits of technology

It effectively suppressed the coarsening of edge grains after normalization, reduced the pre-shearing edge microcrack generation rate, improved the yield and production stability, reduced the risk of cold rolling strip breakage, and met the high-end performance requirements of new energy motors.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for controlling and reducing edge cracking during normalization pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel. Through four core technologies—pre-strengthening of the edge of hot-rolled raw materials, precise control of the normalization temperature field, optimization of pre-shearing process parameters, and passivation treatment of edge microcracks—this method solves the problems of coarse grains at the edges and easy cracking during pre-shearing of high-silicon non-oriented silicon steel after normalization, suppresses the generation of initial microcracks, reduces the breakage rate of subsequent cold rolling, and improves product yield and production stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of non-oriented silicon steel technology, and particularly relates to a method for controlling and reducing edge cracking during normalization pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel. Background Technology

[0002] Non-oriented silicon steel used in high-end equipment such as drive motors for new energy vehicles and wind power converters often requires normalizing treatment after hot rolling to improve microstructure and reduce resistance to cold rolling deformation. However, after normalizing, high-silicon (Si≥3.0%) non-oriented silicon steel raw materials are prone to grain coarsening and plasticity deterioration at the edges. Microcracks are easily generated during pre-shearing, and crack propagation during subsequent cold rolling can lead to strip breakage, which seriously restricts production stability and yield.

[0003] Reference 1 (application number 202111069865.X) proposes a method to improve the control of strip breakage during cold rolling of high-grade non-oriented silicon steel. This patent reduces edge cracking during cold rolling by controlling the load distribution of the cold rolling mill stand and the parameters of the work roll shifting. However, it does not control the pre-shearing stage after normalization. After normalization, the edge grains are coarse and brittle, and initial microcracks are easily generated during pre-shearing. Adjusting the cold rolling parameters alone cannot eliminate the risk of edge cracking at its source, and the strip breakage rate is still ≥1.2 times / 10,000 tons.

[0004] Reference 2 (application number 201910833451.6) proposes a production method to reduce edge crack defects in hot-rolled non-oriented silicon steel. This patent reduces edge cracks during the hot rolling stage by controlling the temperature drop and finishing rolling parameters. However, it only focuses on the hot rolling process and does not consider the deteriorating effect of normalizing treatment on the edge microstructure; normalizing after hot rolling of high-silicon steel will aggravate the coarsening of edge grains, and edge cracks will still occur during pre-shearing, which cannot meet the production requirements of high-grade silicon steel for new energy.

[0005] Reference 3 (application number 202310660826.X) proposes a method for handling edge defects in the production of non-oriented silicon steel using a cold continuous rolling mill. This patent treats edge defects before cold rolling by edge trimming. However, this is a post-processing of defects, requiring the removal of a large amount of edge metal, reducing the yield by 4%-6%; moreover, edge trimming can easily cause new stress concentration, and subsequent rolling may still trigger crack propagation, failing to suppress edge cracking from the source of the process.

[0006] In summary, existing technologies suffer from problems such as deterioration of the microstructure at the normalized edge, inability to suppress initial cracks at the pre-sheared edge, low yield, and high risk of strip breakage. Therefore, there is an urgent need to develop a multi-dimensional synergistic control method that integrates normalized microstructure regulation, pre-shearing process optimization, and edge strengthening treatment to solve the problem of edge cracking at the pre-sheared edge of normalized non-oriented silicon steel for new energy applications. Summary of the Invention

[0007] To address the shortcomings of existing technologies, this invention aims to provide a method for controlling and reducing edge cracking during normalization pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel. This method utilizes four core technologies: edge pre-strengthening of hot-rolled raw materials, precise control of the normalization temperature field, optimization of pre-shearing process parameters, and passivation treatment of edge microcracks. These technologies solve the problems of coarse grains at the edges and easy cracking during pre-shearing of high-silicon non-oriented silicon steel after normalization, suppress the generation of initial microcracks, reduce the subsequent cold rolling strip breakage rate, and improve product yield and production stability.

[0008] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0009] This invention discloses a method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel, comprising the following steps:

[0010] Step 1: Composition of hot-rolled raw materials and edge pre-strengthening

[0011] Hot-rolled coils of non-oriented silicon steel for new energy are selected. The chemical composition by mass percentage is: C≤0.003%, Si 3.2%-4.5%, Al 0.6%-1.2%, Mn 0.2%-0.5%, P≤0.015%, S≤0.003%, N≤0.003%, Sn 0.04%-0.06%, with the balance being Fe and unavoidable impurities.

[0012] The thickness of the hot-rolled coil is 2.0-2.8mm and the width is 800-1250mm. In the hot rolling process, an edge heater is introduced in the finishing stage to raise the edge temperature of the strip by 30-50℃ compared with the core temperature. The final rolling temperature is controlled at 860-880℃. The layer cooling adopts the back-stage cooling mode to suppress abnormal coarsening of edge grains, so that the edge grain size is controlled at 40-60μm and the core grain size is 50-70μm after hot rolling, thereby reducing the difference between edge and core grains.

[0013] Step 2: Precise control of the normalization temperature field

[0014] A continuous normalizing furnace is adopted, and the furnace body is divided into an oxidation-free preheating section, a radiant tube heating section, a soaking section, and a cooling section. To address the problem of overheating and roughening of the edges of high-silicon steel, detachable aluminum silicate heat insulation covers are installed on both sides of the strip in the oxidation-free preheating section and the radiant tube heating section. The heat insulation covers are 50-80mm wide and cover a 30-50mm area of ​​the strip edge. Circulating cooling water is circulated inside to reduce the heat intensity on the edges.

[0015] Non-oxidizing preheating section: temperature 600-700℃, strip running speed 80-100m / min, edge temperature 20-30℃ lower than the core temperature to avoid premature recrystallization at the edge;

[0016] Radiant tube heating section: temperature 850-920℃, holding time 40-60s, edge temperature controlled at 830-880℃, core temperature 870-920℃, to suppress rapid grain growth at the edge, so that the normalized edge grain size is ≤70μm, the core grain size is 80-100μm, and the difference between edge and core grain size is ≤30μm;

[0017] Heating zone: Temperature 880-930℃, holding time 20-30s, to promote homogenization of heart tissue;

[0018] Cooling section: Segmented cooling is adopted. First, it is slowly cooled to 700-750℃ at a rate of 15-20℃ / s, and then rapidly cooled to below 400℃ at a rate of 30-40℃ / s to suppress the precipitation of brittle phases at grain boundaries.

[0019] Step 3: Optimization of pre-trimming process after normalization

[0020] After normalizing, when the strip temperature drops to 150-200℃, it enters the pre-shearing process, using a disc shear equipped with an edge compaction device and a burr removal mechanism.

[0021] Edge trimming control: Based on the degree of edge defects of hot-rolled raw materials, the single-sided edge trimming amount is controlled at 5-12mm. Priority is given to removing defects such as edge oxidation and micro-cracks to avoid excessive trimming and reduced yield.

[0022] Shearing parameter settings: disc shear blade gap 0.05-0.15mm, blade overlap 0.5-1.0mm, shearing speed 60-80m / min; during shearing, apply 5-10kN pressure to the edge of the strip steel through the edge compaction device to reduce shear stress concentration;

[0023] Burr and microcrack passivation: Immediately after shearing, use a rotating wire brush to clean the burrs on the edge, and at the same time use a special roller polishing device to perform micro-polishing on the sheared edge to passivate the tips of the microcracks generated by shearing and reduce the risk of crack propagation.

[0024] Step 4: Edge reinforcement and quality inspection after cutting

[0025] After pre-shearing, the strip edge is subjected to low-temperature induction strengthening treatment. The induction heating temperature is 250-300℃ and the heating time is 1-2s, which causes slight plastic deformation of the edge metal, releases residual shear stress, and improves the plasticity and toughness of the edge.

[0026] An online visual inspection system is used to perform full-surface inspection on the sheared edge with an accuracy of 0.1mm. Microcracks with a depth of ≥0.2mm are identified and marked. The marked defects are locally polished to ensure that there are no microcracks visible to the naked eye before proceeding to the pickling and cold rolling processes.

[0027] Step 5: Connection with subsequent processes

[0028] After processing, the strip steel is pickled to remove the surface iron oxide scale, and then enters the 18-roll 6-stand rolling mill for cold rolling. During the cold rolling process, the edge tension is controlled at 100-130 N / mm² to avoid excessive tension causing edge crack propagation.

[0029] Furthermore, the wire brush has a wire diameter of 0.1-0.3 mm and a rotation speed of 1000-1500 r / min.

[0030] Furthermore, the pickling process involves a hydrochloric acid concentration of 15%-20% and a temperature of 75-85℃.

[0031] Furthermore, the chemical composition by mass percentage is: C 0.002%, Si 3.5%, Al 0.8%, Mn 0.35%, P 0.01%, S 0.002%, N 0.0025%, Sn 0.05%, with the balance being Fe and impurities.

[0032] Furthermore, the chemical composition by mass percentage is: C 0.0025%, Si 4.0%, Al 1.0%, Mn 0.3%, P 0.012%, S 0.0022%, N 0.002%, Sn 0.055%, with the balance being Fe and impurities.

[0033] Furthermore, the chemical composition by mass percentage is: C 0.0022%, Si 4.5%, Al 1.1%, Mn 0.25%, P 0.013%, S 0.0025%, N 0.002%, Sn 0.045%, with the balance being Fe and impurities.

[0034] Furthermore, the hot-rolled coil width is 1000mm, the final rolling temperature is 870℃, the edge grain size is 50μm, and the core grain size is 60μm.

[0035] Normalization control: Non-oxidizing preheating section 650℃, speed 90m / min, the edge is 25℃ lower than the center; radiant tube heating section 880℃, hold for 50s, edge 850℃, center 890℃; cooling section slowly cools to 720℃, then quickly cools to 350℃; after normalization, the edge grain size is 65μm, and the center grain size is 85μm.

[0036] Pre-shearing: strip temperature 180℃, single-sided shearing amount 8mm; blade gap 0.1mm, overlap 0.8mm, shearing speed 70m / min; wire brush speed 1200r / min, and microcrack tips are blunted after polishing.

[0037] Edge strengthening and inspection: Induction heating to 280℃ for 1.5s; online inspection revealed no microcracks ≥0.2mm.

[0038] Results: Pre-sheared edge microcrack rate 1.2%, cold rolling strip breakage rate 0.2 times / 10,000 tons, yield 96.8%, finished product B50=1.76T, P1.5 / 50=3.7W / kg.

[0039] Furthermore, the hot-rolled coil width is 900mm, the final rolling temperature is 865℃, the edge grain size is 45μm, and the core grain size is 55μm.

[0040] Normalization control: Non-oxidizing preheating section 680℃, speed 85m / min, the edge is 28℃ lower than the center; radiant tube heating section 900℃, hold for 45s, edge 860℃, center 910℃; cooling section slow cooling to 730℃, fast cooling to 380℃; after normalization, the edge grain size is 68μm, and the center grain size is 90μm;

[0041] Pre-shearing: strip temperature 160℃, single-sided shearing amount 10mm; blade gap 0.12mm, overlap 0.9mm, shearing speed 65m / min; wire brush speed 1300r / min, and microcrack tips are blunted after polishing.

[0042] Edge strengthening and inspection: Induction heating to 260℃ for 2 seconds; online inspection revealed no microcracks ≥0.2mm.

[0043] Results: Pre-shearing edge microcrack rate 0.8%, cold rolling strip breakage rate 0.15 times / 10,000 tons, yield 97.2%, finished product B50=1.77T, P1.5 / 50=3.6W / kg.

[0044] Furthermore, the hot-rolled coil width is 1250mm, the final rolling temperature is 875℃, the edge grain size is 55μm, and the core grain size is 65μm.

[0045] Normalization control: Non-oxidizing preheating section 620℃, speed 95m / min, the edge is 22℃ lower than the center; radiant tube heating section 910℃, hold for 55s, edge 870℃, center 920℃; cooling section slow cooling to 710℃, fast cooling to 320℃; after normalization, the edge grain size is 70μm, and the center grain size is 95μm;

[0046] Pre-shearing: strip temperature 190℃, single-sided shearing amount 12mm; blade gap 0.15mm, overlap 1.0mm, shearing speed 75m / min; wire brush speed 1400r / min, and microcrack tips are blunted after polishing.

[0047] Edge strengthening and inspection: Induction heating to 290℃ for 1.2s; online inspection revealed no microcracks ≥0.2mm.

[0048] Results: Pre-shearing edge microcrack rate 1.5%, cold rolling strip breakage rate 0.25 times / 10,000 tons, yield 96.5%, finished product B50=1.78T, P1.5 / 50=3.5W / kg.

[0049] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0050] 1. Suppress edge cracking at its source

[0051] By pre-strengthening the hot-rolled edge and precisely controlling the normalizing temperature field, the grain size of the normalized edge is controlled to ≤70μm, and the grain size difference between the edge and the center is ≤30μm. This completely solves the problem of coarse grains and high brittleness at the edge in traditional processes, and eliminates the cause of edge cracking at the microstructure level.

[0052] 2. The quality of pre-trimmed edges is significantly improved.

[0053] By optimizing shearing parameters and providing burr removal and microcrack passivation treatment, there are no obvious burrs on the edge after shearing, and the tips of microcracks are passivated, reducing the microcrack generation rate by more than 85%, thus avoiding strip breakage caused by subsequent cold rolling crack propagation.

[0054] 3. Improved yield and production efficiency

[0055] The single-sided shearing amount is controlled at 5-12mm, which reduces metal loss by 4%-6% compared with traditional edge cutting, and increases the yield to over 96%; the strip breakage rate is ≤0.3 times / 10,000 tons, which is 75% lower than existing technologies, and increases production efficiency by 20%-25%.

[0056] 4. The product has stable and reliable performance.

[0057] Low-temperature induction strengthening treatment at the edges releases residual stress and improves edge toughness. After cold rolling, there are no cracks at the edges and the sheet shape is good. The finished product has a magnetic induction B5000≥1.75T and an iron loss P1.5 / 50≤3.8W / kg, meeting the high-end performance requirements of new energy motors.

[0058] 5. Highly adaptable and cost-controllable

[0059] It can be stably applied to the entire range of hot-rolled raw materials for new energy non-oriented silicon steel with Si 3.2%-4.5% and thickness 2.0-2.8mm; the equipment such as heat shield and induction strengthening are simple to modify, with low maintenance costs, and the overall production cost is reduced by 10%-15%. Detailed Implementation

[0060] Example 1:

[0061] 1. Hot-rolled raw material: Chemical composition (wt%): C 0.002%, Si 3.5%, Al 0.8%, Mn 0.35%, P 0.01%, S 0.002%, N 0.0025%, Sn 0.05%, balance Fe; hot-rolled coil width 1000mm, final rolling temperature 870℃, edge grain 50μm, core grain 60μm.

[0062] 2. Normalization control: Non-oxidizing preheating section 650℃, speed 90m / min, the edge is 25℃ lower than the center; radiant tube heating section 880℃, hold for 50s, edge 850℃, center 890℃; cooling section slowly cools to 720℃, then quickly cools to 350℃; after normalization, the edge grain size is 65μm, and the center grain size is 85μm.

[0063] 3. Pre-shearing: strip temperature 180℃, single-sided shearing amount 8mm; blade gap 0.1mm, overlap 0.8mm, shearing speed 70m / min; wire brush speed 1200r / min, and microcrack tips are blunted after polishing.

[0064] 4. Edge strengthening and inspection: Induction heating to 280℃ for 1.5s; online inspection showed no microcracks ≥0.2mm.

[0065] 5. Results: The pre-shearing edge micro-crack rate was 1.2%, the cold rolling strip breakage rate was 0.2 times / 10,000 tons, the yield was 96.8%, the finished product B50 was 1.76T, and P1.5 / 50 was 3.7W / kg.

[0066] Example 2:

[0067] 1. Hot-rolled raw material: Chemical composition (wt%): C 0.0025%, Si 4.0%, Al 1.0%, Mn 0.3%, P 0.012%, S 0.0022%, N 0.002%, Sn 0.055%, balance Fe; hot-rolled coil width 900mm, final rolling temperature 865℃, edge grain 45μm, core grain 55μm.

[0068] 2. Normalization control: Non-oxidizing preheating section 680℃, speed 85m / min, the edge is 28℃ lower than the center; radiant tube heating section 900℃, hold for 45s, edge 860℃, center 910℃; cooling section slowly cools to 730℃, then quickly cools to 380℃; after normalization, the edge grain size is 68μm, and the center grain size is 90μm.

[0069] 3. Pre-shearing: strip temperature 160℃, single-sided shearing amount 10mm; blade gap 0.12mm, overlap 0.9mm, shearing speed 65m / min; wire brush speed 1300r / min, and microcrack tips are blunted after polishing.

[0070] 4. Edge strengthening and inspection: Induction heating to 260℃ for 2 seconds; online inspection revealed no microcracks ≥0.2mm.

[0071] 5. Results: Pre-shearing edge micro-crack generation rate is 0.8%, cold rolling strip breakage rate is 0.15 times / 10,000 tons, yield is 97.2%, finished product B50=1.77T, P1.5 / 50=3.6W / kg.

[0072] Example 3:

[0073] 1. Hot-rolled raw material: Chemical composition (wt%): C 0.0022%, Si 4.5%, Al 1.1%, Mn 0.25%, P 0.013%, S 0.0025%, N 0.002%, Sn 0.045%, balance Fe; hot-rolled coil width 1250mm, final rolling temperature 875℃, edge grain 55μm, core grain 65μm.

[0074] 2. Normalization control: Non-oxidizing preheating section 620℃, speed 95m / min, the edge is 22℃ lower than the center; radiant tube heating section 910℃, hold for 55s, edge 870℃, center 920℃; cooling section slowly cools to 710℃, then quickly cools to 320℃; after normalization, the edge grains are 70μm and the center grains are 95μm.

[0075] 3. Pre-shearing: strip temperature 190℃, single-sided shearing amount 12mm; blade gap 0.15mm, overlap 1.0mm, shearing speed 75m / min; wire brush speed 1400r / min, and microcrack tips are blunted after polishing.

[0076] 4. Edge strengthening and inspection: Induction heating to 290℃ for 1.2s; online inspection showed no microcracks ≥0.2mm.

[0077] 5. Results: Pre-shearing edge micro-crack generation rate 1.5%, cold rolling strip breakage rate 0.25 times / 10,000 tons, yield rate 96.5%, finished product B50=1.78T, P1.5 / 50=3.5W / kg.

[0078] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel, characterized in that: Includes the following steps: Step 1: Composition of hot-rolled raw materials and edge pre-strengthening Hot-rolled coils of non-oriented silicon steel for new energy are selected. The chemical composition by mass percentage is: C≤0.003%, Si 3.2%-4.5%, Al 0.6%-1.2%, Mn 0.2%-0.5%, P≤0.015%, S≤0.003%, N≤0.003%, Sn 0.04%-0.06%, with the balance being Fe and unavoidable impurities. The thickness of the hot-rolled coil is 2.0-2.8mm and the width is 800-1250mm. In the hot rolling process, an edge heater is introduced in the finishing stage to raise the edge temperature of the strip by 30-50℃ compared with the core temperature. The final rolling temperature is controlled at 860-880℃. The layer cooling adopts the back-stage cooling mode to suppress abnormal coarsening of edge grains, so that the edge grain size is controlled at 40-60μm and the core grain size is 50-70μm after hot rolling, thereby reducing the difference between edge and core grains. Step 2: Precise control of the normalization temperature field A continuous normalizing furnace is adopted, and the furnace body is divided into an oxidation-free preheating section, a radiant tube heating section, a soaking section, and a cooling section. To address the problem of overheating and roughening of the edges of high-silicon steel, detachable aluminum silicate heat insulation covers are installed on both sides of the strip in the oxidation-free preheating section and the radiant tube heating section. The heat insulation covers are 50-80mm wide and cover a 30-50mm area of ​​the strip edge. Circulating cooling water is circulated inside to reduce the heat intensity on the edges. Non-oxidizing preheating section: temperature 600-700℃, strip running speed 80-100m / min, edge temperature 20-30℃ lower than the core temperature to avoid premature recrystallization at the edge; Radiant tube heating section: temperature 850-920℃, holding time 40-60s, edge temperature controlled at 830-880℃, core temperature 870-920℃, to suppress rapid grain growth at the edge, so that the normalized edge grain size is ≤70μm, the core grain size is 80-100μm, and the difference between edge and core grain size is ≤30μm; Heating zone: Temperature 880-930℃, holding time 20-30s, to promote homogenization of heart tissue; Cooling section: Segmented cooling is adopted. First, it is slowly cooled to 700-750℃ at a rate of 15-20℃ / s, and then rapidly cooled to below 400℃ at a rate of 30-40℃ / s to suppress the precipitation of brittle phases at grain boundaries. Step 3: Optimization of pre-trimming process after normalization After normalizing, when the strip temperature drops to 150-200℃, it enters the pre-shearing process, using a disc shear equipped with an edge compaction device and a burr removal mechanism. Edge trimming control: Based on the degree of edge defects of hot-rolled raw materials, the single-sided edge trimming amount is controlled at 5-12mm. Priority is given to removing defects such as edge oxidation and micro-cracks to avoid excessive trimming and reduced yield. Shearing parameter settings: disc shear blade gap 0.05-0.15mm, blade overlap 0.5-1.0mm, shearing speed 60-80m / min; During the shearing process, a pressure of 5-10kN is applied to the edge of the strip steel through an edge compaction device to reduce shear stress concentration; Burr and microcrack passivation: Immediately after shearing, use a rotating wire brush to clean the burrs on the edge, and at the same time use a special roller polishing device to perform micro-polishing on the sheared edge to passivate the tips of the microcracks generated by shearing and reduce the risk of crack propagation. Step 4: Edge reinforcement and quality inspection after cutting After pre-shearing, the strip edge is subjected to low-temperature induction strengthening treatment. The induction heating temperature is 250-300℃ and the heating time is 1-2s, which causes slight plastic deformation of the edge metal, releases residual shear stress, and improves the plasticity and toughness of the edge. An online visual inspection system is used to perform full-surface inspection on the sheared edge with an accuracy of 0.1mm. Microcracks with a depth of ≥0.2mm are identified and marked. The marked defects are locally polished to ensure that there are no microcracks visible to the naked eye before proceeding to the pickling and cold rolling processes. Step 5: Connection with subsequent processes After processing, the strip steel is pickled to remove the surface iron oxide scale, and then enters the 18-roll 6-stand rolling mill for cold rolling. During the cold rolling process, the edge tension is controlled at 100-130 N / mm² to avoid excessive tension causing edge crack propagation.

2. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 1, characterized in that: The wire brush has a wire diameter of 0.1-0.3 mm and a rotation speed of 1000-1500 r / min.

3. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 1, characterized in that: The pickling process involves using hydrochloric acid at a concentration of 15%-20% and a temperature of 75-85℃.

4. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 1, characterized in that: Chemical composition by mass percentage: C 0.002%, Si 3.5%, Al 0.8%, Mn 0.35%, P 0.01%, S 0.002%, N 0.0025%, Sn 0.05%, balance Fe and impurities.

5. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 1, characterized in that: Chemical composition by mass percentage: C 0.0025%, Si 4.0%, Al 1.0%, Mn 0.3%, P 0.012%, S 0.0022%, N 0.002%, Sn 0.055%, balance Fe and impurities.

6. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 1, characterized in that: Chemical composition by mass percentage: C 0.0022%, Si 4.5%, Al 1.1%, Mn 0.25%, P 0.013%, S 0.0025%, N 0.002%, Sn 0.045%, balance Fe and impurities.

7. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 4, characterized in that: The hot-rolled coil has a width of 1000 mm, a final rolling temperature of 870℃, an edge grain size of 50 μm, and a core grain size of 60 μm. Normalization control: Non-oxidizing preheating section 650℃, speed 90m / min, the edge is 25℃ lower than the center; radiant tube heating section 880℃, hold for 50s, edge 850℃, center 890℃; cooling section slowly cools to 720℃, then quickly cools to 350℃; after normalization, the edge grain size is 65μm, and the center grain size is 85μm. Pre-shearing: strip temperature 180℃, single-sided shearing amount 8mm; blade gap 0.1mm, overlap 0.8mm, shearing speed 70m / min; wire brush speed 1200r / min, and microcrack tips are blunted after polishing. Edge strengthening and inspection: Induction heating to 280℃ for 1.5s; online inspection revealed no microcracks ≥0.2mm. Results: Pre-sheared edge microcrack rate 1.2%, cold rolling strip breakage rate 0.2 times / 10,000 tons, yield 96.8%, finished product B50=1.76T, P1.5 / 50=3.7W / kg.

8. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 5, characterized in that: The hot-rolled coil has a width of 900 mm, a final rolling temperature of 865℃, an edge grain size of 45 μm, and a core grain size of 55 μm. Normalization control: Non-oxidizing preheating section 680℃, speed 85m / min, the edge is 28℃ lower than the center; radiant tube heating section 900℃, hold for 45s, edge 860℃, center 910℃; cooling section slow cooling to 730℃, fast cooling to 380℃; after normalization, the edge grain size is 68μm, and the center grain size is 90μm; Pre-shearing: strip temperature 160℃, single-sided shearing amount 10mm; blade gap 0.12mm, overlap 0.9mm, shearing speed 65m / min; wire brush speed 1300r / min, and microcrack tips are blunted after polishing. Edge strengthening and inspection: Induction heating to 260℃ for 2 seconds; online inspection revealed no microcracks ≥0.2mm. Results: Pre-shearing edge microcrack rate 0.8%, cold rolling strip breakage rate 0.15 times / 10,000 tons, yield 97.2%, finished product B50=1.77T, P1.5 / 50=3.6W / kg.

9. The method for controlling and reducing edge cracking during normalizing pre-shearing of hot-rolled raw materials for new energy non-oriented silicon steel according to claim 6, characterized in that: The hot-rolled coil has a width of 1250mm, a final rolling temperature of 875℃, an edge grain size of 55μm, and a core grain size of 65μm. Normalization control: Non-oxidizing preheating section 620℃, speed 95m / min, the edge is 22℃ lower than the center; radiant tube heating section 910℃, hold for 55s, edge 870℃, center 920℃; cooling section slow cooling to 710℃, fast cooling to 320℃; after normalization, the edge grain size is 70μm, and the center grain size is 95μm; Pre-shearing: strip temperature 190℃, single-sided shearing amount 12mm; blade gap 0.15mm, overlap 1.0mm, shearing speed 75m / min; wire brush speed 1400r / min, and microcrack tips are blunted after polishing. Edge strengthening and inspection: Induction heating to 290℃ for 1.2s; online inspection revealed no microcracks ≥0.2mm. Results: Pre-shearing edge microcrack rate 1.5%, cold rolling strip breakage rate 0.25 times / 10,000 tons, yield 96.5%, finished product B50=1.78T, P1.5 / 50=3.5W / kg.

Citation Information

Patent Citations

  • A production method for reducing edge crack defects in hot-rolled non-oriented silicon steel

    CN110586657B

  • A method for improving the control of strip breakage in cold-rolled high-grade non-oriented silicon steel

    CN113751517B

  • Edge defect treatment method for non-oriented silicon steel produced by cold tandem mill

    CN116921433A