One-step drawing process for constant outer diameter variable wall thickness steel tube

By employing a one-time drawing process for steel pipes with constant outer diameter and variable wall thickness, and utilizing axial gradient preheating and online heating quenching technologies, the problems of plastic strain differences and grain boundary corrosion in the drawing process of super austenitic corrosion-resistant stainless steel pipes with variable wall thickness were solved, achieving uniformity and high performance of the microstructure throughout the entire length.

CN123149265APending Publication Date: 2026-11-24JIANGSU JIUJUN STEEL PIPE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611367129.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the process of drawing super austenitic corrosion-resistant stainless steel pipes with varying wall thickness, there are differences in plastic strain and deformation energy storage in the axial position, which increases the risk of grain boundary corrosion. Furthermore, the existing technology of multiple segmented drawing and offline annealing methods leads to abnormal grain growth and uneven microstructure and properties.

Method used

A one-time drawing process for steel pipes with constant outer diameter and variable wall thickness is adopted. Through axial gradient preheating, sizing outer mold and follower mandrel cooperation, online medium frequency induction heating and high pressure annular spray quenching, uniform deformation and rapid quenching of each section are achieved, which promotes discontinuous static recrystallization and deformation energy storage utilization.

Benefits of technology

This method achieves a uniform single-phase austenitic equiaxed grain structure along the entire length of the pipe, reducing the risk of intergranular corrosion, improving forming stability and mechanical properties, and reducing surface damage and fluctuations in microstructure properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149265A_ABST
    Figure CN123149265A_ABST
Patent Text Reader

Abstract

This invention relates to the field of plastic processing and online deformation heat treatment microstructure control technology for super austenitic corrosion-resistant stainless steel pipes. It discloses a one-time drawing process for steel pipes with constant outer diameter and variable wall thickness, comprising: axial gradient preheating based on the wall thickness reduction rate of the billet's axial section; axial movement of the mandrel while constraining the outer diameter with a sizing die to adjust the deformation gap, completing a single-pass drawing of the pipe; continuous introduction into a medium-frequency induction heating zone with dynamically adjusted power for rapid heating and solution treatment, utilizing deformation energy storage to induce discontinuous static recrystallization; and subsequent introduction into a high-pressure annular spray zone for rapid quenching with a collision jet. This invention balances axial flow stress through gradient preheating, eliminating the risk of local hardening and cracking. Combined with online transient solution treatment and strong quenching, it suppresses the precipitation of brittle intermetallic phases, achieving full-length grain refinement and uniform matching of corrosion resistance and load-bearing properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of plastic processing and online deformation heat treatment microstructure control technology of super austenitic corrosion-resistant stainless steel pipes, and particularly relates to a one-time drawing process for steel pipes with constant outer diameter and variable wall thickness. Background Technology

[0002] Super austenitic corrosion-resistant stainless steel contains high mass fractions of chromium, nickel, molybdenum, and nitrogen, exhibiting excellent resistance to pitting and crevice corrosion. It is commonly used in the manufacture of deep-sea oil production umbilicals and corrosion-resistant pipeline systems. Under such conditions, the internal pressure and bending stress borne by the pipe along the axial direction are not the same, but rather exhibit a certain gradient. Using pipes with a constant outer diameter and a stepped or gradually changing wall thickness along the axial direction can reduce unnecessary load-bearing margins while maintaining a uniform external assembly standard.

[0003] Super austenitic corrosion-resistant stainless steel exhibits low stacking fault energy and a strong tendency for work hardening. During variable wall thickness plastic drawing, the thin-walled region experiences greater wall reduction, more severe material deformation, a significant increase in internal dislocation density, and the accumulation of high deformation energy. Conversely, the thick-walled region shows less deformation and relatively lower deformation energy. Significant differences exist in plastic strain and deformation energy at different axial positions within the tube. Furthermore, this material is prone to phase precipitation within a specific intermediate-temperature sensitization range. The precipitation of chromium- and molybdenum-rich intermetallic phases at grain boundaries leads to chromium and molybdenum depletion in the austenitic matrix. This increases the risk of intergranular corrosion. Existing technologies typically employ multiple segmented drawing processes, combined with offline resistance furnace static annealing at each stage. During the offline annealing heating process, due to the limited heat transfer rate of the furnace, the time required for the tube to pass through the sensitization temperature zone is relatively long, making it easy for a second phase to precipitate. At the same time, due to the large deformation and high deformation energy storage in the thin-walled region, abnormal grain growth and mixed crystals are prone to occur during the heat preservation process; while due to the small deformation and low deformation energy storage in the thick-walled region, incomplete solid solution may occur due to insufficient recrystallization and solid solution driving force.

[0004] Therefore, how to reduce the difference in rheological stress at different axial positions during single-pass drawing with variable wall thickness, and how to use deformation energy storage after forming to achieve grain refinement and phase precipitation suppression along the entire length of the tube, has become the technical problem to be solved by this invention. Summary of the Invention

[0005] To address the problems in the background art, the technical solution of the present invention is as follows: A one-time drawing process for steel pipes with constant outer diameter and variable wall thickness, comprising the following steps: Step S1: Based on the axially preset wall thickness reduction rate distribution of the super austenitic corrosion-resistant stainless steel billet tube from 0.15 to 0.55, axial gradient preheating is carried out on the super austenitic corrosion-resistant stainless steel billet tube. The preheating temperature of the small deformation thick wall section is controlled at 180°C to 250°C, and the preheating temperature of the large deformation thin wall section is controlled at 300°C to 380°C, so that the initial deformation resistance of the high reduction rate section is lower than that of the low reduction rate section. Step S2: The outer diameter of the super austenitic corrosion-resistant stainless steel billet is constrained by the sizing outer die. The follower mandrel is driven to move axially to adjust the annular deformation gap between the inner hole of the sizing outer die and the outer circumference of the follower mandrel. The billet is drawn at a drawing speed of 15 mm / s to 45 mm / s to form a variable wall thickness tube with a constant outer diameter and a gradient change in inner diameter in a single pass. Step S3: After drawing and demolding, the variable wall thickness tube is continuously introduced into the multi-segment medium-frequency induction heating zone. The output power of the medium-frequency induction heating coils of each segment is dynamically adjusted according to the real-time tube wall thickness and drawing speed measured at the sizing die outlet, so that the tube is heated to 1160℃ to 1200℃ within 2.0s to 5.0s. The axial residence time in the 1160℃ to 1200℃ range is 8s to 20s, so that the austenite undergoes discontinuous static recrystallization and the deformation-induced carbonitrides are completely dissolved. Step S4: The tube material removed from the medium-frequency induction heating zone is introduced into the high-pressure annular spray zone within 0.8s, and rapid quenching is performed by applying a collision impact jet. The average cooling rate of the tube wall from 1160℃ to below 400℃ is controlled to be greater than 90℃ / s, thereby blocking the precipitation of intermetallic phases in the sensitization temperature range of 650℃ to 1000℃.

[0006] Preferably, the chemical composition of the super austenitic corrosion-resistant stainless steel billet tube, by mass percentage, includes: C 0.020%, Si 0.60%, Mn 1.00%, Cr 19.5% to 21.0%, Ni 17.5% to 18.5%, Mo 6.0% to 6.8%, N 0.18% to 0.25%, Cu 0.50% to 1.00%, P 0.030%, S 0.010%, with the balance being Fe and impurity elements; and the pitting resistance equivalent constant PREN is calculated by the sum of 3.3 times the mass percentage of Cr and Mo and 16 times the mass percentage of N, and is greater than or equal to 43.0.

[0007] Preferably, before performing axial gradient preheating on the super austenitic corrosion-resistant stainless steel billet in step S1, the method further includes: step S11, sandblasting to remove oxide scale and pickling passivation of the inner and outer surfaces of the super austenitic corrosion-resistant stainless steel billet with mixed acid, and depositing an oxalate conversion film with a thickness of 3μm to 8μm on the inner and outer surfaces of the billet; step S12, coating the outer surface of the oxalate conversion film with a composite lubricant and drying and curing it, wherein the composite lubricant contains 15% to 25% by mass of molybdenum disulfide micro powder, 5% to 10% by mass of polytetrafluoroethylene micro powder, and the balance being modified waterborne acrylic resin.

[0008] Preferably, in step S1, the axial gradient preheating of the super austenitic corrosion-resistant stainless steel billet tube specifically includes: step S13, controlling the preheating temperature of the thick-walled section with a cross-sectional wall thickness reduction rate of 0.15 to 0.25 to be 180°C to 250°C, and controlling the preheating temperature of the thin-walled section with a cross-sectional wall thickness reduction rate of 0.45 to 0.55 to be 300°C to 380°C; step S14, in the variable wall thickness transition section, continuously and smoothly adjusting the induction heating power within the range of 180°C to 380°C based on the axial displacement monitoring signal, so that the target preheating temperature increases linearly with the increase of the cross-sectional wall thickness reduction rate.

[0009] Preferably, in step S2, the sizing outer die is a cemented carbide die, the inner diameter of the die hole sizing zone is constant, and the working cone angle at the die inlet is 12°; the drawing process specifically includes: step S21, when drawing the thin-walled section, driving the follower mandrel to the front limit position to form the minimum deformation gap; step S22, when drawing the variable wall thickness transition section, controlling the follower mandrel to retract at a controlled speed; step S23, when drawing the thick-walled section, controlling the follower mandrel to retract to the rear stable position and keep it stationary to form the maximum deformation gap, and keeping the drawing force in the range of 120kN to 210kN.

[0010] Preferably, in step S3, the total heating length of the multi-segment medium-frequency induction heating zone along the axial direction is 450mm, specifically including: step S31, the instantaneous linear power density of each segment of the medium-frequency induction heating coil applied at the axial position increases linearly with the increase of the real-time pipe wall thickness, so that the pipe material is heated from the demold surface temperature of 120°C to the target solid solution temperature of 1180°C, and the induction output power is matched in the thin-walled section and the thick-walled section respectively, and the heating time is controlled to be 2.0s to 5.0s.

[0011] Preferably, step S3 further includes: step S32, in the multi-segment medium-frequency induction heating zone, in the temperature range of 1160°C to 1200°C, the austenitic equiaxed crystals are regenerated and the carbonitrides are completely dissolved, so as to obtain a single-phase austenitic equiaxed crystal structure with an average grain size of ASTM 7.0 to 8.0 grade over the entire length.

[0012] Preferably, in step S4, the high-pressure annular spray zone includes four sets of annular water spray manifolds arranged axially in a staggered manner, with 16 pressure atomizing nozzles evenly distributed around the circumference of each manifold. Specifically, step S41 involves controlling the axial distance between two adjacent sets of annular water spray manifolds to be 40mm to 60mm, tilting the nozzle axis 15° to 30° in the opposite direction to the pipe discharge to form a reverse impact water curtain, and applying jet flushing with deionized water at a pressure of 0.8MPa to 1.5MPa.

[0013] Preferably, after the pipe exits the high-pressure annular spray zone, the surface moisture is dried online. Through the coordinated processes of axial gradient preheating in step S1, follower mandrel drawing in step S2, online medium-frequency induction heating in step S3, and high-pressure annular spray quenching in step S4, a σ-free surface is obtained across the entire cross-section of the pipe. The single-phase austenitic structure precipitated by the χ phase results in a critical pitting temperature greater than or equal to 75.0℃, an intergranular corrosion rate less than or equal to 0.13mm / a, a yield strength of 330MPa to 380MPa, a tensile strength of 680MPa to 760MPa, and an elongation after fracture greater than or equal to 45% for all sections of the finished variable wall thickness pipe.

[0014] Compared with existing technologies, the one-time drawing process for steel pipes with constant outer diameter and variable wall thickness of the present invention has the following advantages: 1. In a one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness, the deformation resistance of the large deformation thin-walled region is reduced by axial gradient preheating. Combined with the axial movement of the follower mandrel, the difference in plastic flow between the thin-walled and thick-walled regions during the drawing process can be reduced, making the deformation of the pipe along the axial direction more uniform. This can reduce local strain concentration, reduce the risk of necking and cracking, and improve the forming stability of single-pass drawing of variable wall thickness pipe. At the same time, it can reduce surface damage and microstructure fluctuations caused by traditional multi-pass cold drawing and frequent inter-pass annealing.

[0015] 2. By continuously connecting sizing drawing with online medium-frequency induction heating, the deformation energy retained after drawing can be directly utilized to promote discontinuous static recrystallization of austenite. The heating intensity can be adjusted according to the real-time tube wall thickness and drawing speed, so that different wall thickness sections can obtain heating conditions adapted to their own heat capacity. This is beneficial for each section to complete discontinuous static recrystallization and solidification in a shorter time, and can also reduce grain coarsening caused by long-term heat preservation. This results in a fine, uniform, and non-mixed-crystal single-phase austenite equiaxed grain structure along the entire length of the tube, improving the problem of abnormal grain growth in thin-walled areas during offline static annealing.

[0016] 3. High-pressure annular spray quenching after high-temperature solution treatment allows the pipe to quickly pass through the temperature range where intermetallic phases easily precipitate, reducing the precipitation of brittle second phases rich in chromium and molybdenum at the austenite grain boundaries. The impact jet can also promptly destroy the vapor film on the pipe wall surface, making the cooling of the pipe more uniform in the circumferential and axial directions. This ensures that the thin-walled section, the transition section with varying wall thickness, and the thick-walled section maintain a relatively consistent grain boundary state, which is beneficial for the finished pipe to obtain uniform resistance to intergranular corrosion and pitting corrosion along its entire length. Attached Figure Description

[0017] Figure 1 This is a flowchart of the single-pass drawing and online deformation heat treatment process for variable wall thickness steel pipes according to the present invention. Figure 2 This is an exploded diagram of the tubing forming control and microstructure regulation technology elements of the present invention. Detailed Implementation

[0018] The technical solutions of the embodiments of this application will be clearly described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this application are within the scope of protection of this application.

[0019] A one-time drawing process for steel pipes with constant outer diameter and variable wall thickness includes the following steps: Step S1: Based on the axially preset wall thickness reduction rate distribution of the super austenitic corrosion-resistant stainless steel billet tube from 0.15 to 0.55, axial gradient preheating is carried out on the super austenitic corrosion-resistant stainless steel billet tube. The preheating temperature of the small deformation thick wall section is controlled at 180°C to 250°C, and the preheating temperature of the large deformation thin wall section is controlled at 300°C to 380°C, so that the initial deformation resistance of the high reduction rate section is lower than that of the low reduction rate section. Step S2: The outer diameter of the super austenitic corrosion-resistant stainless steel billet is constrained by the sizing outer die. The follower mandrel is driven to move axially to adjust the annular deformation gap between the inner hole of the sizing outer die and the outer circumference of the follower mandrel. The billet is drawn at a drawing speed of 15 mm / s to 45 mm / s to form a variable wall thickness tube with a constant outer diameter and a gradient change in inner diameter in a single pass. Step S3: After drawing and demolding, the variable wall thickness tube is continuously introduced into the multi-segment medium-frequency induction heating zone. The output power of the medium-frequency induction heating coils of each segment is dynamically adjusted according to the real-time tube wall thickness and drawing speed measured at the sizing die outlet, so that the tube is heated to 1160℃ to 1200℃ within 2.0s to 5.0s. The axial residence time in the 1160℃ to 1200℃ range is 8s to 20s, so that the austenite undergoes discontinuous static recrystallization and the deformation-induced carbonitrides are completely dissolved. Step S4: The tube material removed from the medium-frequency induction heating zone is introduced into the high-pressure annular spray zone within 0.8s, and rapid quenching is performed by applying a collision impact jet. The average cooling rate of the tube wall from 1160℃ to below 400℃ is controlled to be greater than 90℃ / s, thereby blocking the precipitation of intermetallic phases in the sensitization temperature range of 650℃ to 1000℃.

[0020] Preferably, the chemical composition of the super austenitic corrosion-resistant stainless steel billet tube, by mass percentage, includes: C 0.020%, Si 0.60%, Mn 1.00%, Cr 19.5% to 21.0%, Ni 17.5% to 18.5%, Mo 6.0% to 6.8%, N 0.18% to 0.25%, Cu 0.50% to 1.00%, P 0.030%, S 0.010%, with the balance being Fe and impurity elements; and the pitting resistance equivalent constant PREN is calculated by the sum of 3.3 times the mass percentage of Cr and Mo and 16 times the mass percentage of N, and is greater than or equal to 43.0.

[0021] Preferably, before performing axial gradient preheating on the super austenitic corrosion-resistant stainless steel billet in step S1, the method further includes: step S11, sandblasting to remove oxide scale and pickling passivation of the inner and outer surfaces of the super austenitic corrosion-resistant stainless steel billet with mixed acid, and depositing an oxalate conversion film with a thickness of 3μm to 8μm on the inner and outer surfaces of the billet; step S12, coating the outer surface of the oxalate conversion film with a composite lubricant and drying and curing it, wherein the composite lubricant contains 15% to 25% by mass of molybdenum disulfide micro powder, 5% to 10% by mass of polytetrafluoroethylene micro powder, and the balance being modified waterborne acrylic resin.

[0022] Preferably, in step S1, the axial gradient preheating of the super austenitic corrosion-resistant stainless steel billet tube specifically includes: step S13, controlling the preheating temperature of the thick-walled section with a cross-sectional wall thickness reduction rate of 0.15 to 0.25 to be 180°C to 250°C, and controlling the preheating temperature of the thin-walled section with a cross-sectional wall thickness reduction rate of 0.45 to 0.55 to be 300°C to 380°C; step S14, in the variable wall thickness transition section, continuously and smoothly adjusting the induction heating power within the range of 180°C to 380°C based on the axial displacement monitoring signal, so that the target preheating temperature increases linearly with the increase of the cross-sectional wall thickness reduction rate.

[0023] Preferably, in step S2, the sizing outer die is a cemented carbide die, the inner diameter of the die hole sizing zone is constant, and the working cone angle at the die inlet is 12°; the drawing process specifically includes: step S21, when drawing the thin-walled section, driving the follower mandrel to the front limit position to form the minimum deformation gap; step S22, when drawing the variable wall thickness transition section, controlling the follower mandrel to retract at a controlled speed; step S23, when drawing the thick-walled section, controlling the follower mandrel to retract to the rear stable position and keep it stationary to form the maximum deformation gap, and keeping the drawing force in the range of 120kN to 210kN.

[0024] Preferably, in step S3, the total heating length of the multi-segment medium-frequency induction heating zone along the axial direction is 450mm, specifically including: step S31, the instantaneous linear power density of each segment of the medium-frequency induction heating coil applied at the axial position increases linearly with the increase of the real-time pipe wall thickness, so that the pipe material is heated from the demold surface temperature of 120°C to the target solid solution temperature of 1180°C, and the induction output power is matched in the thin-walled section and the thick-walled section respectively, and the heating time is controlled to be 2.0s to 5.0s.

[0025] Preferably, step S3 further includes: step S32, in the multi-segment medium-frequency induction heating zone, in the temperature range of 1160°C to 1200°C, the austenitic equiaxed crystals are regenerated and the carbonitrides are completely dissolved, so as to obtain a single-phase austenitic equiaxed crystal structure with an average grain size of ASTM 7.0 to 8.0 grade over the entire length.

[0026] Preferably, in step S4, the high-pressure annular spray zone includes four sets of annular water spray manifolds arranged axially in a staggered manner, with 16 pressure atomizing nozzles evenly distributed around the circumference of each manifold. Specifically, step S41 involves controlling the axial distance between two adjacent sets of annular water spray manifolds to be 40mm to 60mm, tilting the nozzle axis 15° to 30° in the opposite direction to the pipe discharge to form a reverse impact water curtain, and applying jet flushing with deionized water at a pressure of 0.8MPa to 1.5MPa.

[0027] Preferably, after the pipe exits the high-pressure annular spray zone, the surface moisture is dried online. Through the coordinated processes of axial gradient preheating in step S1, follower mandrel drawing in step S2, online medium-frequency induction heating in step S3, and high-pressure annular spray quenching in step S4, a σ-free surface is obtained across the entire cross-section of the pipe. The single-phase austenitic structure precipitated by the χ phase results in a critical pitting temperature greater than or equal to 75.0℃, an intergranular corrosion rate less than or equal to 0.13mm / a, a yield strength of 330MPa to 380MPa, a tensile strength of 680MPa to 760MPa, and an elongation after fracture greater than or equal to 45% for all sections of the finished variable wall thickness pipe.

[0028] Example 1: In the engineering deployment of deep-sea oil production umbilicals and high-temperature, high-acid oil and gas transmission pipelines, the pipe body is subjected to a load gradient along the axial direction, consisting of ocean current, wave, suspension, bending stress, and the self-weight load of the end connection joints. S31254 super austenitic alloy was selected, containing, by mass percentage, 0.015% carbon, 0.42% silicon, 0.65% manganese, 20.12% chromium, 18.05% nickel, 6.18% molybdenum, 0.212% nitrogen, 0.75% copper, 0.018% phosphorus, 0.002% sulfur, and the balance iron. The corrosion-resistant stainless steel billet tube has a pitting resistance equivalent constant PREN of 43.91. To achieve structural weight reduction and load-bearing gradient matching, the wall thickness needs to be smoothly increased axially from a 3.50mm thin-walled load-bearing section through a 1000mm linear variable wall thickness transition section to a 7.00mm thick-walled reinforced section while maintaining a constant outer diameter of 60mm. This is based on the inherent physical characteristics of this super austenitic corrosion-resistant stainless steel, namely low stacking fault energy and high work hardening rate, and the presence of chromium- and molybdenum-rich elements in the 650℃ to 1000℃ temperature range. phase and The rapid precipitation of the sensitized phase kinetics leads to a strong axial strain gradient distribution in conventional cold drawing due to the significant difference in deformation between the thin-walled large deformation zone and the thick-walled small deformation zone. If the formed material is sent to a resistance furnace for static heating and annealing, the heating process takes a long time to traverse the precipitation temperature zone, resulting in chromium and molybdenum depletion at the grain boundaries. Furthermore, the thin-walled high-energy storage zone is prone to grain coarsening and mixed crystal formation during static heat preservation, while the thick-walled low-energy storage zone suffers from insufficient thermodynamic driving force, resulting in incomplete solid dissolution of carbonitrides. This leads to a stepwise dispersion in the corrosion resistance and mechanical strength of the pipe along its entire length.

[0029] A solution-treated S31254 super austenitic corrosion-resistant stainless steel billet with an initial outer diameter of 68 mm and an initial wall thickness of 8 mm was selected. First, the entire surface of the billet was sandblasted with quartz sand to remove the hot-rolled oxide scale. Then, it was pickled in a mixed pickling solution of 18% nitric acid and 3% hydrofluoric acid at 35°C for 15 min to clean the surface. After rinsing with water, it was immersed in an oxalate bath at 75°C for 10 min. A 5.2 μm thick porous crystalline anchoring morphology was deposited on both the inner and outer surfaces of the billet. The oxalate conversion membrane is then uniformly roll-coated on the outer layer of the oxalate conversion membrane with a composite lubricant comprising 20% ​​molybdenum disulfide micro powder, 8% polytetrafluoroethylene micro powder, and 72% modified waterborne acrylic resin by mass. The lubricant is then dried and cured in a hot air environment at 140℃ for 20 minutes to form a solid lubricating film layer that is tightly attached to the micropores of the oxalate conversion membrane and is resistant to high temperature and high shear stress. This eliminates interface seizing and scratch defects in the billet tube during the subsequent variable cross-section drawing process.

[0030] A blank tube coated with a solid lubricating film is loaded onto the servo drawing and pushing end, so that the front end of the blank tube passes through a high-frequency induction preheating coil of a single-turn hollow copper tube, and the basic preheating temperature is set. The temperature is 160℃, and the temperature compensation coefficient is... The temperature is 320℃, depending on the axial position of the billet tube. Section wall thickness reduction rate ,in, The initial wall thickness is 8mm. Indicates the axial position after drawing. The pipe wall thickness at that location is used as the target pipe wall thickness when setting the axial gradient preheating temperature, derived from the axial gradient preheating formula. The target preheating temperature for each deformation section was determined. The basis for this preheating temperature calculation is as follows: by calibrating the hot compressive rheological stress curve of solution-treated super austenitic corrosion-resistant stainless steel in the temperature range of 150℃ to 400℃, the work hardening rate of this material at room temperature is approximately 620 MPa per unit true strain. Within the 150℃ to 400℃ range, the material's rheological stress exhibits a linear softening decay with increasing temperature, and the temperature softening sensitivity coefficient is 1.12 MPa per degree Celsius. Setting the base preheating temperature to 160℃ ensures that the material is removed from the room temperature embrittlement sensitivity zone and maintains lubrication. Adhesion activity: Setting the temperature compensation coefficient to 320℃ results in a 128℃ temperature rise increment when the shrinkage rate increases from 0.15 to 0.55, providing approximately 143MPa of thermal softening stress compensation. This precisely offsets the work hardening increment caused by the increased shrinkage, ensuring that the initial equivalent stress in all sections entering the outer mold deformation zone remains stable within a balanced range of 410MPa to 435MPa. For a large deformation thin-walled section with a wall thickness of 3.50mm and a cross-sectional wall thickness reduction rate of 0.5625, high-frequency induction power heating raises the preheating temperature of the pipe wall to 340℃. For a wall thickness of 7... For the small deformation thick-walled section with a wall thickness reduction rate of 0.1250 and a diameter of 0.00mm, the induction heating power is reduced to maintain the preheating temperature of the tube wall at 200℃. In the transition section with varying wall thickness, the preheating temperature is controlled to smoothly transition continuously between 200℃ and 340℃ based on the axial displacement monitoring signal. The thermal softening effect induced by the temperature rise dynamically offsets the high work hardening tendency in the large wall reduction area, so that different deformation sections of the billet tube obtain mutually balanced initial deformation resistance and plastic flow stress before entering the die deformation zone. It should be noted that during the continuous drawing process of the tube, the main body of the finished tube has The wall thickness of the effective bearing section gradually changes between 3.60 mm and 6.80 mm, and the corresponding main shrinkage rate range is within the controlled process window of 0.15 to 0.55. In the embodiment, the wall thickness shrinkage rates of 0.1250 and 0.5625 correspond to the process transition chamfer limit margin of the tube blank head drawing clamping end and the tail demolding transition zone, respectively. After entering the effective forming section, the system controls the wall thickness shrinkage rate to quickly converge and stabilize in the main process range of 0.15 to 0.55, ensuring complete self-consistency between the embodiment and the process parameter design range in terms of theoretical boundaries and actual forming state.

[0031] The preheated billet is fed into a YG8 cemented carbide sizing die with an inlet working cone angle of 12°. The inner diameter of the outer die is constant at 60mm. At the same time, the working half-cone angle is coaxially matched inside the billet. Set the drawing speed for a 3° follower mandrel. The speed is 30 mm / s. In actual assembly and transmission control, the follower mandrel is rigidly and coaxially locked to the piston rod of the electro-hydraulic servo actuator cylinder at the rear end of the frame via a high-strength heat-resistant alloy tie rod that passes through the inner hole at the tail of the billet tube. A set of guide centering slides with self-lubricating wear-resistant copper sleeves is set every 800 mm along the axial direction of the tie rod. The outer diameter of each guide centering slide maintains a 0.5 mm single-sided sliding gap with the inner wall of the undeformed billet tube. During the continuous feeding of the billet, radial constraint is applied to the tie rod to eliminate long suspension. The axial bending and radial sway of the boom under high tensile loads ranging from 120kN to 210kN ensure that the coaxiality of the working cone surface of the follower mandrel and the inner hole of the sizing outer die remains stable within 0.02mm, guaranteeing that the annular deformation gap is uniformly symmetrical in the circumferential direction. When forming a thin-walled section with a wall thickness of 3.50mm, the servo push-pull mechanism drives the follower mandrel to be positioned at the front limit position, maintaining the annular deformation gap at 3.50mm. When entering the linear variable wall thickness transition section, the wall thickness gradually changes according to the slope. and linkage relationship ,in, To control the axial displacement rate of the mandrel, the servo mechanism is controlled at a displacement rate of 2.00 mm / s. The driven follower mandrel retracts and, upon reaching the thick-walled section, controls the follower mandrel to remain in a stable position at the rear end, ensuring that the annular deformation gap remains constant at 7.00 mm. The traction and pulling force remains stable between 120 kN and 210 kN throughout the process. Under the synergistic effect of the constant diameter constraint of the outer mold and the continuous displacement of the mandrel's conical surface, a variable-walled thick tube with a constant outer diameter and a gradually changing thickness of the inner wall is formed in a single pass.

[0032] The measured surface temperature of the pipe exiting the sizing mold was 120℃. After demolding, the pipe continuously passed through a coaxially arranged multi-segment medium-frequency induction heating zone. This heating zone consisted of four multi-channel medium-frequency induction heating coils, with a total heating length of 450mm. The target solution treatment temperature was set. The overall efficiency constant of induction electrothermal conversion is 1180℃. Set to 0.75, theoretical material density The value is taken as 8000 kg per cubic meter, and the average isobaric specific heat capacity at high temperature is also considered. The value is 550 joules per kilogram Kelvin, and the pipe has a constant outer diameter. The thickness is 0.060m, based on the pipe wall thickness measured in real time at the outlet of the sizing mold. With drawing line speed Determine instantaneous linear power density ,in, Instantaneous linear power density, To ensure a measured surface temperature of 120℃ upon demolding, the instantaneous linear power density corresponding to the thin-walled and thick-walled sections was used as the two endpoints in the actual power adjustment. Linear interpolation was performed based on the real-time pipe wall thickness during the transition section with varying wall thickness, ensuring that the instantaneous linear power density at each axial position increased linearly with the real-time pipe wall thickness. The total heating power of the intermediate frequency induction heating coils in each section was calculated by converting the corresponding instantaneous linear power density into the effective operating length of that section. The total heating power output was 52.25kW in the thin-walled section and dynamically increased to [a higher value] in the thick-walled section. With a total heating power of 97.84kW, the power is linearly and smoothly adjusted between 52.25kW and 97.84kW in the transition section, allowing the thin-walled section, transition section, and thick-walled section to rapidly heat to the 1180℃ single-phase austenite solution temperature range within 3.2s. To maintain the axial residence time of the tube in the 1160℃ to 1180℃ range for 15s, a high-temperature insulating and heat-soaking sleeve is coaxially connected to the outlet of the multi-segment medium-frequency induction heating zone, and the heating is adjusted according to the drawing speed of 30mm / s. The effective heat preservation length is adjusted to ensure that the tube body, after rapid heating, remains continuously within the temperature range of 1160℃ to 1180℃. Within this high-temperature range, the tube body utilizes the high-density dislocation energy accumulated from a single-pass drawing as the driving force for discontinuous static recrystallization nucleation, enabling the deformation substructure to complete strain relaxation and equiaxed crystal recrystallization nucleation. Simultaneously, the deformation-induced transient carbonitrides dissociate and dissolve back into the austenite matrix. After the tube undergoes drastic diameter and wall reduction plastic deformation within the mold, it is demolded, and the deformation-induced high-density dislocation entanglement and lattice... The distortion energy is completely and transiently retained within the crystal. During the rapid heating of the tube wall to 1160°C to 1180°C and the axial high-temperature residence process, the high-density deformation energy storage continuously drives the recrystallization nucleation and grain boundary migration of austenite, causing discontinuous static recrystallization and strain relaxation of austenite. Within the 15s axial residence time, the newly recrystallized equiaxed grains grow uniformly to ASTM 7.1 to 7.5 grade, and at the same time, the fine carbonitrides precipitated during the deformation process are completely dissolved back into the austenite matrix lattice.

[0033] After the tube body, having completed online solution heating, is removed from the intermediate frequency induction coil, a high-pressure annular spray zone containing four sets of annular water spray manifolds with an axial spacing of 50 mm is introduced within 0.6 seconds. Sixteen pressure atomizing nozzles, evenly distributed circumferentially within each manifold, spray deionized water at a pressure of 1.2 MPa. The spray direction is tilted at a 20° angle to the opposite direction of the tube's travel axis towards the tube's discharge direction to form a reverse impact water curtain. This breaks through the vapor film heat-insulating layer on the tube wall surface, controlling the average cooling rate of the tube wall from 1180℃ to 350℃ to reach 106.4℃ / s, thus exceeding the temperature range of 650℃ to 1000℃. The single-phase austenite microstructure is frozen at a temperature sensitive to intermetallic phase precipitation at ℃. Four sets of annular water spray manifolds are staggered along the pipe discharge axis at 50mm axial intervals. Each set of annular water spray manifolds is coaxially set, and 16 pressure atomizing nozzles on the inner circumference of each manifold are evenly distributed at a circumferential angle of 22.5°. The nozzles between adjacent sets of manifolds are staggered by 11.25° in the circumferential direction and arranged in an alternating top-to-bottom arrangement. The radial spray distance from the nozzle outlet to the outer surface of the pipe is constant at 35mm. The high-pressure jet forms an overlapping and enveloping 360° annular closed water curtain on the outer circumferential surface of the pipe, in conjunction with the reverse... The 20° angled scouring kinetic energy rapidly strips away the vaporized gas film, and a 65mm inner diameter annular air knife structure is coaxially connected at the outlet of the spray zone. 0.6MPa compressed air performs annular shearing and blowing on the residual water film on the pipe surface, achieving efficient and uniform heat exchange and surface drying without visual blind spots. The discharged material is then dried by the annular compressed air air knife to remove residual moisture. The resulting finished pipe exhibits a clean single-phase austenitic equiaxed grain structure across the entire cross-section, including thin-walled sections, transitional sections, and thick-walled sections. The average grain size is consistently between ASTM 7.1 and 7.5, and the axial sections show consistent grain size. The yield strength is maintained between 342 MPa and 368 MPa, the tensile strength between 715 MPa and 742 MPa, and the elongation after fracture between 48.5% and 52.0%. The critical pitting temperature (CPT) of the entire cross section, measured according to ASTM G48 Method E, is between 75.0℃ and 77.5℃. The intergranular corrosion rate, measured according to ASTM A262 Method C, is between 0.112 mm / a and 0.125 mm / a. This achieves a uniform match between geometric dimensional gradient accuracy, high strength and toughness mechanical load-bearing capacity, and resistance to localized corrosion in all sections of the entire length.

[0034] Example 2: In this example, seamless billets of S31254 super austenitic corrosion-resistant stainless steel, smelted in the same batch and solution-treated, were used for parameter boundary and control tests. The chemical composition of the billet, by mass percentage, included 0.015% carbon, 0.42% silicon, 0.65% manganese, 20.12% chromium, 18.05% nickel, 6.18% molybdenum, 0.212% nitrogen, 0.75% copper, 0.018% phosphorus, 0.002% sulfur, and the balance iron. The pitting corrosion resistance equivalent constant... The initial blank tube specifications were 68 mm outer diameter and 8 mm wall thickness, with a diameter of 43.91. The test platform was equipped with a hydraulic servo cold drawing machine with a maximum drawing load of 500 kN and a displacement control accuracy of 0.01 mm, a high-frequency induction preheating coil with a working frequency of 100 kHz to 300 kHz and continuously adjustable power, a multi-segment medium-frequency induction heating zone with a working frequency of 1 kHz to 10 kHz and a temperature control accuracy of ±2 ℃, an annular cooling water tank with 16 high-pressure atomizing nozzles and a water supply pressure adjustable from 0.8 MPa to 2.5 MPa, and a coaxial infrared temperature sensor with a sampling frequency of 50 Hz. The annular cooling water tank was used to form a high-pressure annular spray zone to simultaneously monitor the axial temperature field, drawing load, and geometric dimensional accuracy after forming during the continuous drawing process of the tube body.

[0035] The experiment was conducted under three test groups: lower limit condition, standard median condition, and upper limit condition. A partial missing control group (removing key processes), an out-of-range control group (parameters deviating from the specified range), and a comparison group using traditional multi-pass cold drawing and annealing were also included. All samples were designed with a finished tube outer diameter of 60 mm, a thin-walled load-bearing section wall thickness of 3.50 mm, and a thick-walled reinforcing section wall thickness of 7.00 mm as the forming target. The test groups were determined based on axial position. Section wall thickness reduction rate Determine the deformation at different axial positions, and then apply the axial gradient preheating relationship. Determine the preheating temperature for each section, among which, The initial wall thickness is 8mm. Indicates axial position The wall thickness of the tube after drawing; when setting the axial gradient preheating temperature. The target thickness at that location is determined during power adjustment after drawing and demolding. The wall thickness of the tube after demolding is measured in real time at this location. After demolding, the instantaneous linear power density formula is applied based on the wall thickness and drawing speed. Adjust the output power of each section of the intermediate frequency induction heating coil, among which, The theoretical density of the material is 8000 kg per cubic meter. The high-temperature average isobaric specific heat capacity is 550 joules per kilogram Kelvin. With a constant outer diameter of 0.060m, For the drawing speed, The target complete solution temperature is 1180℃. The actual measured surface temperature after demolding was 120℃. To determine the overall efficiency constant of induction electrothermal conversion, in actual control, the instantaneous linear power density at both ends is first determined based on the real-time wall thickness of the thin-walled and thick-walled sections. The variable wall thickness transition section is linearly adjusted between the two ends according to the real-time wall thickness, so that the instantaneous linear power density increases linearly with the increase of the real-time wall thickness. The output power of each section of the medium-frequency induction heating coil is determined according to the corresponding instantaneous linear power density and the effective heating length. In order to make the axial residence time at different drawing speeds correspond to the process settings of each group, the multi-segment medium-frequency induction heating zone and the subsequent continuous high-temperature heat preservation section together form a high-temperature action zone. The effective high-temperature action length is adjusted according to the drawing speed, so that the tube maintains the set axial residence time in the temperature range of 1160℃ to 1200℃. After completing the online solution heating, the tube continuously enters the high-pressure annular spray zone, where it is rapidly quenched by forming a reverse impact water curtain through the collision impact jet.

[0036] Under the lower limit conditions, the basic preheating temperature of test group 1 was set to 150℃ and the temperature compensation coefficient was set to 280℃, so that the axial preheating temperature was between 180℃ and 300℃, and the drawing speed was 15mm / s. The drawn tube was heated online to 1160℃ and held axially for 8s, and then rapidly quenched with a spray pressure of 0.8MPa. The measured cooling rate was 92.4℃ / s. Under the process parameters of this group, the drawing force was between 135kN and 188kN. The microstructure of the finished product was a single-phase austenitic equiaxed grain structure without brittle phase precipitation, with an average grain size of ASTM 7.8 grade. The yield strength was 374MPa, the tensile strength was 751MPa, the elongation after fracture was 47.5%, the critical pitting temperature was 76.0℃, and the intergranular corrosion rate was 0.115mm / a.

[0037] Under standard median conditions, test group 2 used a base preheating temperature of 160℃ and a temperature compensation coefficient of 320℃ to control the axial preheating temperature between 200℃ and 340℃, with a drawing speed of 30mm / s; the online solution treatment temperature was 1180℃, the axial residence time was 15s, the spray pressure was 1.2MPa, the measured cooling rate was 106.4℃ / s, and the corresponding drawing force was 120kN to 210kN. The finished product maintained a single-phase austenitic equiaxed grain structure without brittle phase precipitation, with an average grain size of ASTM 7.4 grade; the yield strength was 358MPa, the tensile strength was 732MPa, the elongation after fracture was 49.8%, the critical pitting temperature was 77.0℃, and the intergranular corrosion rate was 0.118mm / a.

[0038] Under the upper limit conditions, the basic preheating temperature of test group 3 was increased to 180℃, the temperature compensation coefficient was increased to 360℃, the axial preheating temperature was controlled between 250℃ and 380℃, and the drawing speed was 45mm / s; the online solution temperature was 1200℃, the axial residence time was 20s, and quenching was carried out with a spray pressure of 1.5MPa. The measured cooling rate reached 118.2℃ / s. The drawing force of this group was between 112kN and 195kN. The resulting microstructure was still a single-phase austenitic equiaxed grain structure without brittle phase precipitation, with an average grain size of ASTM 7.1 grade; the yield strength was 345MPa, the tensile strength was 718MPa, the elongation after fracture was 51.5%, the critical pitting temperature was 75.5℃, and the intergranular corrosion rate was 0.122mm / a.

[0039] After covering the lower, median, and upper limits of the above-mentioned working conditions, the three test groups generally had a drawing force ranging from 112kN to 210kN. Axial gradient preheating enabled the large deformation thin-walled section to achieve thermal softening corresponding to the wall reduction rate. After the pipe was demolded, online temperature compensation was performed based on the instantaneous linear power density, raising the temperature to 1160℃ to 1200℃ within 2.0s to 5.0s. The high-density dislocation pile-up and deformation energy storage formed during the drawing process caused the austenite to undergo submicron-level discontinuous static recrystallization. Subsequently, it passed through the sensitization temperature range of 650℃ to 1000℃ at a cooling rate greater than 90℃ / s. The average grain size finally obtained by the three test groups was between ASTM 7.1 and 7.8, the yield strength was between 345MPa and 374MPa, the elongation after fracture was between 47.5% and 51.5%, the critical pitting temperature was between 75.5℃ and 77.0℃, and the intergranular corrosion rate was less than 0.125mm / a.

[0040] Control group 1 eliminated axial gradient preheating and performed room temperature cold drawing at 25℃, with other parameters set as in test group 2. After losing axial temperature compensation, work hardening in the thin-walled section caused an increase in deformation resistance, with the drawing force increasing from 198kN to 285kN. Microcracks and surface scratches appeared in the transition zone of varying wall thickness. Its average grain size was ASTM 7.3 grade, yield strength was 362MPa, tensile strength was 738MPa, elongation after fracture was 44.0%, critical pitting temperature was 76.5℃, intergranular corrosion rate was 0.120mm / a, and the microstructure was mainly austenitic matrix.

[0041] Control group 2 retained the forming process but eliminated online solution treatment. Instead, it involved forming the tube and then holding it at 1180℃ for 30 minutes in an offline resistance furnace followed by water quenching. All other parameters were the same as in control group 2, with the pull-out force remaining between 120kN and 210kN. During the offline heating process, the tube was kept in a sensitization temperature range of 650℃ to 1000℃ to enrich the chromium and molybdenum content. phase and The phase is continuously distributed along the austenite grain boundaries, while the grains coarsen in the thin-walled high-energy-storage region, eventually forming a mixed crystal of ASTM 4.0 grade; the yield strength drops to 295 MPa, the tensile strength is 642 MPa, the elongation after fracture is 38.5%, the critical pitting temperature drops to 55.0℃, and the intergranular corrosion rate increases to 0.462 mm / a.

[0042] Control group 3 maintained the other parameters of test group 2, except that the high-pressure annular spray quenching was replaced with conventional water bath immersion cooling, with a cooling rate of 42.5℃ / s and a drawing force of 120kN to 210kN. During the cooling process, when the tube wall passed through the intermetallic phase precipitation temperature zone, austenite matrix grain boundaries precipitated and dispersed. Phase; average grain size is ASTM 7.4 grade, yield strength is 338 MPa, tensile strength is 695 MPa, elongation after fracture is 43.0%, critical pitting temperature is 61.5℃, and intergranular corrosion rate is 0.385 mm / a.

[0043] Control group 4 used a solution temperature of 1120℃ and an axial residence time of 5s, with other parameters set as in test group 2. The pull-out force ranged from 120kN to 210kN. Due to the solution temperature being lower than 1160℃ and the residence time being insufficient, the austenitic matrix still retained deformed substructures and undissolved carbonitrides. The average grain size was ASTM 8.5 grade, the yield strength was 392MPa, the tensile strength was 758MPa, the elongation after fracture was 36.5%, the critical pitting temperature was 63.0℃, and the intergranular corrosion rate was 0.295mm / a.

[0044] Control group 5 increased the solution temperature to 1240℃ and extended the axial residence time to 30s, while using the same parameters as test group 2. The pull-out force ranged from 120kN to 210kN. After the solution temperature exceeded 1200℃ and the residence time increased, the austenite grains became significantly coarser, forming ASTM 4.5 grade coarse grains, and the grain boundary bonding strength weakened. The yield strength was 288MPa, the tensile strength was 635MPa, the elongation after fracture was 41.0%, the critical pitting temperature was 68.0℃, and the intergranular corrosion rate was 0.210mm / a.

[0045] Control group 6 eliminated axial gradient preheating and applied uniform 120℃ preheating along the axial direction. The remaining parameters were the same as those of test group 2. Due to the preheating temperature being below 150℃, the rheological stress compensation in different wall reduction sections was insufficient, and the pull-out force increased to 165kN to 248kN. The wall thickness tolerance of the variable wall thickness transition section exceeded ±0.08mm. Its microstructure was an austenitic matrix with an average grain size of ASTM 7.4 grade, a yield strength of 360MPa, a tensile strength of 735MPa, an elongation after fracture of 46.0%, a critical pitting temperature of 76.5℃, and an intergranular corrosion rate of 0.121mm / a.

[0046] Control group 7 used traditional three-pass cold drawing, with annealing at 1050℃ between passes, and the finished product was then subjected to offline solution treatment at 1180℃ for 30 minutes followed by water quenching. The drawing force under this process was between 140kN and 230kN. The resulting microstructure was an austenitic matrix with localized second-phase precipitation and uneven grain size. The average grain size was ASTM 5.5 grade mixed grain. The yield strength was 308MPa, the tensile strength was 662MPa, the elongation after fracture was 42.0%, the critical pitting temperature was 58.5℃, and the intergranular corrosion rate was 0.335mm / a.

[0047] As can be seen from the corresponding changes between the experimental and control groups, axial gradient preheating directly affects the differences in rheological stress in different wall reduction sections. The online medium-frequency induction heating after demolding utilizes the deformation energy stored in the single-pass drawing to cause discontinuous static recrystallization of austenite and solidify the deformation-induced carbonitrides. Subsequently, the high-pressure annular spray zone applies a collision impact jet for rapid cooling, limiting the precipitation of harmful second phases at grain boundaries. The above continuous process enables the variable wall thickness super austenitic corrosion-resistant stainless steel tube to maintain the corresponding consistency of wall thickness gradient dimensions, mechanical properties, and resistance to pitting and intergranular corrosion in all sections of the entire length after single-pass drawing.

[0048] Example 3: This example is used for the transition section between a deep-sea suspended oil production pipeline and a special marine riser. The pipe material is simultaneously subjected to self-weight tension, wave bending, and alternating fluid pulsation loads along the axial direction, forming a large stress gradient in the transition section. An S31254 super austenitic corrosion-resistant stainless steel billet was selected, containing, by mass percentage, 0.015% carbon, 0.42% silicon, 0.65% manganese, 20.12% chromium, 18.05% nickel, 6.18% molybdenum, 0.212% nitrogen, 0.75% copper, 0.018% phosphorus, 0.002% sulfur, and the balance iron. Its pitting resistance equivalent constant PREN is 43.91. Maintaining a constant outer diameter of 60mm... Under the premise of dimensional constraints, the wall thickness along the axial direction is increased from a 3.60mm thin-walled bearing section through an 80mm variable-thickness transition section to a 6.80mm thick-walled reinforcing section. This condition corresponds to the deformation boundary where the wall thickness reduction rate increases from 0.15 to 0.55, and the wall thickness gradient slope reaches 0.040. Due to the short transition section, the wall reduction amount and the axial displacement of the mandrel change rapidly in this section, and the local frictional heat and deformation hardening are more concentrated. The subsequent high-temperature treatment also needs to take into account the precipitation of sensitized phase and grain growth. Therefore, the parameters of wall reduction flow resistance, induced energy input and cooling heat flow are calibrated to control the forming structure and properties under the conditions of high wall reduction rate and large wall thickness gradient slope.

[0049] A solution-treated S31254 super austenitic corrosion-resistant stainless steel billet with an initial outer diameter of 68 mm and an initial wall thickness of 8 mm was selected. First, the entire surface of the billet was sandblasted with quartz sand to remove the hot-rolled oxide scale. Then, it was pickled in a mixed pickling solution of 18% nitric acid and 3% hydrofluoric acid at 35°C for 15 min. After washing with water, it was immersed in an oxalate bath at 75°C for 10 min, resulting in the deposition of a 7.2 μm thick oxalate deposit with a porous, anchored microstructure on both the inner and outer surfaces of the billet. Oxalate conversion film is formed, and then a composite lubricant is uniformly rolled onto the outer surface of the oxalate conversion film. The composite lubricant contains 25% molybdenum disulfide micro powder, 10% polytetrafluoroethylene micro powder, and 65% modified waterborne acrylic resin by mass. It is cured and kept at 140℃ hot air oven for 20 minutes. After curing, a solid lubricating film layer is formed to withstand the interfacial shearing action during the drawing process with large wall reduction and high wall thickness gradient slope, and to reduce the adhesive wear between the metal and the mold surface.

[0050] A blank tube coated with a solid lubricating film is loaded onto the servo-drawing feed end, and the front end of the blank tube passes through a high-frequency induction preheating coil. The basic preheating temperature is... Set to 175℃, temperature compensation coefficient Set at 350℃, based on the shrinkage rate of the cross-sectional wall thickness. The target preheating temperature for each deformation section is determined by the relationship with the axial gradient preheating. The wall thickness input used for preheating setting is the target wall thickness of the tube after drawing at the corresponding axial position. For the thin-walled section with a wall thickness of 3.60 mm and a cross-sectional wall thickness reduction rate of 0.55, the high-frequency induction power is adjusted to make the tube wall preheating temperature reach 367.5℃. For the thick-walled section with a wall thickness of 6.80 mm and a cross-sectional wall thickness reduction rate of 0.15, the tube wall preheating temperature is stabilized at 227.5℃. In the transition section with varying wall thickness, based on the axial displacement monitoring signal, the preheating temperature is linearly and smoothly adjusted along the axial displacement between 227.5℃ and 367.5℃ as the cross-sectional wall thickness reduction rate changes. The thermal softening effect generated by the temperature increase compensates for the deformation resistance of the section with large wall thickness reduction, so that each section of the tube maintains a continuous plastic rheological state before entering the sizing mold.

[0051] The preheated billet is fed into a YG8 cemented carbide sizing die with an inlet working cone angle of 12°. The inner diameter of the outer die is constant at 60mm. A working half-cone angle is coaxially set inside the billet. The drawing line speed is 4.5° with a follower mandrel. Set at 40 mm / s, when forming a thin-walled section with a wall thickness of 3.60 mm, the servo push-pull mechanism positions the follower mandrel at its front limit position, maintaining the annular deformation gap at 3.60 mm. After entering the variable wall thickness transition section with a length of 80 mm and a wall thickness gradient slope of 0.040, according to the linkage relationship between the wall thickness gradient slope and the axial displacement rate of the follower mandrel, the follower mandrel is controlled to move at a displacement rate of 20.33 mm / s. Retract backward; after reaching the thick-walled section, keep the follower mandrel in a stable position at the rear end, stabilize the annular deformation gap at 6.80mm, and the traction pulling force is between 135kN and 225kN throughout the drawing process. Under the combined action of the constant diameter constraint of the sizing outer mold and the continuous axial movement of the follower mandrel conical surface, a variable wall thick tube with a constant outer diameter and a rapidly changing inner diameter along the 80mm transition section is formed in a single pass.

[0052] When the pipe is removed from the sizing mold, the measured surface temperature is 120℃. It then continuously enters a four-segment, multi-channel medium-frequency induction heating zone with a total heating length of 450mm, arranged coaxially. In this embodiment, the target solution temperature is... Set at 1180℃, the overall efficiency constant of induction electrothermal conversion. Set to 0.78, theoretical density of the material Take 8000 kg / m³, high temperature average isobaric specific heat capacity Take 550 joules per kilogram of Kelvin, with a constant outer diameter The diameter is set to 0.060m, and the power control is based on the real-time measured pipe wall thickness and drawing speed at the outlet of the sizing die. Determine instantaneous linear power density The measured wall thickness used here is different from the target wall thickness used during axial gradient preheating. First, the instantaneous linear power density at both ends is determined based on the measured wall thickness of the thin-walled and thick-walled sections. Then, in the variable wall thickness transition section, the instantaneous linear power density is linearly adjusted between the two ends according to the real-time wall thickness, so that the instantaneous linear power density increases linearly with the real-time wall thickness. The total heating power of the intermediate frequency induction heating coils in each section is determined according to the corresponding instantaneous linear power density and effective operating length. The total heating power of the thin-walled section is 68.65kW, and the total heating power of the thick-walled section dynamically increases to 122.33kW. The power in the variable wall thickness transition section is linearly and smoothly adjusted between 68.65kW and 122.33kW with the displacement of the tube body, so that the thin-walled section, transition section, and thick-walled section all heat up to the 1180℃ single-phase austenite solution temperature range within 2.8s.

[0053] In the axial arrangement of the heating and insulation sections, a 360mm long high-temperature ceramic fiber insulation and heat-spreading sleeve is coaxially connected to the outlet of a 450mm four-segment medium-frequency induction heating coil. The total axial span of the heating and insulation mechanism is 810mm. At a drawing speed of 40mm / s, the time for the pipe to pass through the 450mm induction coil is 11.25s, with the first 2.8s completing the heating and the subsequent 8.45s maintaining the temperature within the solution temperature range. After entering the insulation and heat-spreading sleeve, the axial residence time is calculated based on the time the actual pipe wall temperature is between 1160℃ and 1180℃, with the 2.75s mark being the optimal time for axial residence. Within this temperature range, the axial residence time of the pipe in the 1160℃ to 1180℃ range is 11.2s. Through this high-temperature residence process, the high-density dislocation energy accumulated by the drawing deformation is directly utilized to cause discontinuous static recrystallization of austenite. At the same time, the deformation-induced fine carbonitrides are dissolved in the austenite matrix. Within the drawing speed range of 15mm / s to 45mm / s, by adjusting the effective axial extension and retraction length of the heat-insulating and heat-spreading sleeve and the output power of the medium-frequency induction heating coils in each section, the axial residence time of each section in the 1160℃ to 1200℃ range is maintained between 8s and 20s.

[0054] After online solution heating, the tube exits the medium-frequency induction heating zone and enters the high-pressure annular spray zone within 0.5 seconds. The high-pressure annular spray zone is equipped with four sets of axially staggered annular water spray manifolds, with an axial spacing of 40 mm between adjacent sets. Each manifold contains 16 pressure atomizing nozzles evenly distributed around its circumference. Deionized water at 1.5 MPa is used to apply a counter-impact jet, with the nozzle axis tilted 30° in the opposite direction to the tube's discharge, forming a reverse impact water curtain. This breaks through the vapor film heat-insulating layer on the tube wall surface, achieving an average cooling rate of 123.5℃ / s from 1180℃ to 340℃. The tube rapidly passes through the sensitization temperature zone of 650℃ to 1000℃. After exiting the high-pressure annular spray zone, residual moisture on the surface is dried online by an annular compressed air knife. The resulting finished tube exhibits a single-phase austenitic equiaxed crystal structure across the entire cross-section of the thin-walled section, the transition section with a gradually changing slope for large wall thickness, and the thick-walled section. No other abnormalities were observed. phase and The phase precipitation has an average grain size level of ASTM 7.2 to 7.6, a full-section yield strength of 352 MPa to 370 MPa, a tensile strength of 725 MPa to 748 MPa, an elongation after fracture of 48.0% to 51.2%, a critical pitting temperature (CPT) of 76.0℃ to 77.5℃ as measured by ASTM G48 Method E, and an intergranular corrosion rate of 0.115 mm / a to 0.122 mm / a as measured by ASTM A262 Method C. The pipe maintains its corresponding dimensions, mechanical properties, and resistance to pitting and intergranular corrosion under conditions of large wall reduction and large wall thickness gradient.

[0055] Example 4: This example combines Figures 1 to 2 This paper describes a one-time drawing process for a steel pipe with a constant outer diameter and variable wall thickness. Figure 1 As shown, in step S1, based on the pre-set wall thickness reduction rate distribution of the super austenitic corrosion-resistant stainless steel billet tube along the axial direction of 0.15 to 0.55, axial gradient preheating is implemented on the super austenitic corrosion-resistant stainless steel billet tube. The preheating temperature of the small deformation thick-walled section is controlled at 180℃ to 250℃, and the preheating temperature of the large deformation thin-walled section is controlled at 300℃ to 380℃, so that the initial deformation resistance of the high reduction rate section is lower than that of the low reduction rate section. In step S2, a sizing die is used to impose a constant constraint on the outer diameter of the super austenitic corrosion-resistant stainless steel billet tube. The follower mandrel is synchronously driven to move axially to adjust the annular deformation gap between the inner hole of the sizing die and the outer circumference of the follower mandrel. The billet tube is drawn at a drawing speed of 15mm / s to 45mm / s, forming a variable wall thickness tube with a constant outer diameter and a gradient change in inner diameter in a single pass. In step S3, the variable wall thickness tube after drawing and demolding is continuously introduced into a multi-segment medium-frequency induction heating zone. The output power of each segment of the medium-frequency induction heating coil is dynamically adjusted according to the real-time tube wall thickness measured at the sizing die outlet and the drawing speed, so that the tube heats up to 1160℃ to 1200℃ within 2.0s to 5.0s. The axial residence time in the 1160℃ to 1200℃ range is 8s to 20s, which causes discontinuous static recrystallization of austenite and complete solidification of deformation-induced carbonitrides. In step S4, the tube that has been removed from the medium-frequency induction heating zone is introduced into a high-pressure annular spray zone within 0.8s, where a collision impact jet is applied for rapid quenching. The average cooling rate of the tube wall from 1160℃ to below 400℃ is controlled to be greater than 90℃ / s, blocking the precipitation of intermetallic phases in the sensitization temperature range of 650℃ to 1000℃.

[0056] like Figure 2 As shown, a one-time drawing process for steel pipe with constant outer diameter and variable wall thickness includes axial gradient preheating, single-pass drawing of billet, multi-stage medium-frequency induction heating, and high-pressure annular spray quenching. In axial gradient preheating, oxalate conversion film is deposited and composite lubricant is coated, and preheating is controlled according to the distribution of cross-sectional wall thickness reduction rate. In single-pass drawing of billet, the outer diameter is constantly constrained by the sizing die, and the annular deformation gap is adjusted in coordination, resulting in a gradient change in the inner diameter. In multi-stage medium-frequency induction heating, the output power is dynamically adjusted to cause discontinuous static recrystallization of austenite and complete solid solution of carbonitrides. In high-pressure annular spray quenching, an impact jet is applied to control the average cooling rate and block the precipitation of intermetallic phases.

[0057] Example 5: Before batch clamping and machining S31254 super austenitic corrosion-resistant stainless steel pipes with an outer diameter of 60mm and a wall thickness ranging from 3.50mm to 7.00mm, the mechanical backlash and displacement zero-point drift formed by the long-term reciprocating motion of the hydraulic servo system are calibrated. A contact-type grating displacement sensor is used to detect the sizing zone at the inlet of the sizing die and the working half-cone angle. The servo push-pull mechanism is driven to fine-tune the axial position of the follower mandrel at a 3° starting reference position on the conical surface, with a step size of 0.02 mm. This ensures that the initial alignment deviation between the annular deformation gap and the target wall thickness of 3.50 mm in the thin-walled section is controlled within 0.01 mm. Subsequently, a calibrated high-frequency current is applied to the high-frequency induction preheating coil under no-load propulsion conditions in the cold drawing machine. The surface temperature rise curve is collected along the axial travel path of the billet tube using an infrared temperature sensor. The basic preheating temperature is then corrected based on the measured temperature rise slope. 160℃, temperature compensation coefficient The table shows the induction power distribution at 320℃. During the process of increasing the wall thickness reduction rate of the billet tube section from 0.1250 to 0.5625, the tube wall preheating temperature changes monotonically and smoothly within the range of 200℃ to 340℃ to compensate for the changes in rheological stress caused by the fluctuations in the electrical and thermal conductivity of the billet tube batches.

[0058] The tube is drawn at a linear speed of 30 mm / s. As the tube continuously exits the sizing mold and enters the multi-segment medium-frequency induction heating zone with a total heating length of 450mm, the mold exit temperature measuring device monitors the measured temperature of the tube surface in real time at a sampling frequency of 50Hz. When the local surface temperature fluctuates between 115°C and 125°C due to ambient airflow disturbances, the power regulation unit adjusts the instantaneous linear power density formula. Power adjustment is performed, including real-time pipe wall thickness. Take the pipe wall thickness measured at the outlet of the sizing mold; substitute it into the theoretical material density. 8000 kg / m³, high temperature average isobaric specific heat capacity 550 joules per kilogram Kelvin, outer diameter 0.060m, target complete solution temperature The temperature is 1180℃ and the overall efficiency constant of induction electrothermal conversion is... The power adjustment unit has a response period of 0.75 and a response period of 0.02s. It determines the output values ​​at both ends based on the instantaneous linear power density corresponding to the thin-walled and thick-walled sections, and makes linear adjustments between the two ends when the real-time tube wall thickness changes, so that the instantaneous linear power density increases linearly with the increase of the real-time tube wall thickness. The output power of the medium frequency induction heating coil of each section is determined by the corresponding instantaneous linear power density and the effective working length, so that the heating power of the thin-walled section is stabilized at 52.25kW and the heating power of the thick-walled section is stabilized at 97.84kW. It also compensates for the actual heat capacity deviation of the furnace and controls the temperature of each section of the entire tube to rise to 1180℃ within 3.2s.

[0059] The multi-segment medium-frequency induction heating zone is divided into four independent induction coils along the axial direction. Each segment is 112.5 mm long, with a total heating length of 450 mm. The power adjustment unit distributes the total heating power, which varies with the real-time pipe wall thickness, to the four coils according to the axial heating stage. The first coil bears 40% of the total output power for rapid heating; the second coil bears 30% to bring the pipe wall temperature to 1160°C; the third coil bears 18% to adjust the pipe wall temperature to the solution temperature of 1180°C; and the fourth coil bears 12% to compensate for end heat radiation loss and maintain uniform heating. Each of the four coils is driven by an independent inverter power supply module. Under the unified clock trigger of the main controller, the output power of each segment is synchronously adjusted according to the real-time pipe wall thickness. The outlet of the multi-segment medium-frequency induction heating zone is connected to a high-temperature insulation and uniform heating section. By adjusting its effective working length, the pipe after rapid heating is kept in the axial residence time of 15 seconds in the range of 1160°C to 1200°C.

[0060] After online solution heating, the high-temperature tube enters the high-pressure annular spray zone within 0.6 seconds. Four sets of annular water spray manifolds apply impact jets at 1.2 MPa pressure, forming a reverse impact water curtain for rapid quenching. The measured average cooling rate of the tube wall from 1180℃ to 350℃ remains above 106.4℃ / s, rapidly passing through the sensitization temperature zone of 650℃ to 1000℃, blocking… phase and Phase precipitation occurs; the resulting tube body forms a single-phase austenitic structure with an average grain size of ASTM 7.1 to 7.5 across its entire cross-section, with a full-length yield strength stable at 342 MPa to 368 MPa and a critical pitting temperature maintained above 75°C.

[0061] Example 6: This example selects S31254 super austenitic corrosion-resistant stainless steel variable wall thickness tubes for deep-sea extreme corrosion and high-pressure alternating load conditions. The dimensional dynamic response characteristics during its continuous forming process are controlled. A solution-treated billet tube with the following chemical composition by mass percentage: carbon 0.015%, silicon 0.42%, manganese 0.65%, chromium 20.12%, nickel 18.05%, molybdenum 6.18%, nitrogen 0.212%, copper 0.75%, phosphorus 0.018%, sulfur 0.002%, and balance iron, has a pitting resistance equivalent constant PREN of 43.91. The initial outer diameter of the billet tube is 68 mm, and the wall thickness is 8 mm. The target constant outer diameter of the tube is 60 mm. The designed wall thickness for the thin-walled load-bearing section is 3.50 mm, the designed wall thickness for the thick-walled reinforcing section is 7 mm, the length of the variable wall thickness transition section is 1000 mm, and the wall thickness gradient slope is... The thickness of the surface conversion film and solid lubricating film was measured using an eddy current thickness gauge along the inner and outer circumferences and the entire length of the billet tube before clamping it on the line. The oxalate conversion film deposition thickness was controlled between 4.8 μm and 5.6 μm. A composite lubricant containing 20% ​​molybdenum disulfide micro powder, 8% polytetrafluoroethylene micro powder, and the remainder modified waterborne acrylic resin was dried and cured to form a solid lubricating film layer with a thickness between 8.0 μm and 12.0 μm. Subsequently, a dynamic tension sensor was installed on the drawing chuck, and a drawing speed of 15 mm / s to 45 mm / s was used. The traction tube passes through a cemented carbide sizing die with an inner diameter of 60mm, and the drawing load signal is collected in real time, with the drawing force control range being 120kN to 210kN. When the force sensor detects that the drawing load exceeds 210kN and continues to rise, the servo fluid supply circuit adjusts the hydrostatic compensation of the lubricating fluid in the working area of ​​the die inlet. The servo fluid supply circuit includes a high-pressure micro-plunger pump, a proportional overflow pressure regulating valve, and four sets of micro-hole oil injection channels opened on the circumference of the cone surface at the inlet of the sizing die. The fluid lubricating medium is a high-temperature fully synthetic polyalphaolefin-based drawing oil with a flash point higher than 320℃. A micro-lubricating oil is pulsedly injected between the working cone surface at the inlet of the sizing die and the oxalate conversion film on the outer surface of the tube at a supply pressure of 8MPa to 15MPa, forming a dynamic pressure micro-oil pad at the metal deformation interface to supplement the lubrication of the local solid lubricating film shear damage area. The temperature of the working area at the die inlet is maintained below 200℃, so that the solid composite lubricating film and the micro-fluid hydrostatic lubrication form transient complementarity during the rising stage of the drawing load.

[0062] During the mandrel drawing process, to address the time lag in the displacement response of the servo push-pull mechanism caused by the compressibility of hydraulic oil and the mechanical transmission clearance, a dynamic feedforward lag compensation algorithm is employed in the mandrel servo control system to adjust the drawing linear speed. Set to 30mm / s, working half-cone angle of the follower mandrel Set to 3°, based on the position of the transition point of the variable cross-section, output the axial retraction command of the follower mandrel 0.05s in advance, and follow the linkage relationship. The servo push-pull mechanism is controlled to move at a displacement rate of 2.00 mm / s. The driven mandrel retracts, and the laser ultrasonic online thickness sensor installed at the outlet of the sizing mold monitors the wall thickness gradient trajectory in real time at a sampling frequency of 100Hz. The deviation between the measured wall thickness change rate and the preset wall thickness gradient slope of 0.0035 is fed back to the servo controller. By fine-tuning the displacement rate of the driven mandrel in a closed loop, the linearity deviation of the wall thickness in the transition section is controlled within ±0.02mm. The main controller calculates the current target wall thickness of the variable cross-section and the ideal retraction position in real time based on the pipe traction displacement encoder signal, and outputs a feedforward control command 0.05s in advance to compensate for the 40ms electro-hydraulic response lag of the hydraulic servo valve and the 0.015mm transmission dead zone of the mechanical screw. The real-time wall thickness difference fed back by the online thickness sensor is input to the proportional-integral-derivative controller after being filtered by a first-order low-pass filter. The displacement rate correction gain is calculated at an adjustment frequency of 50 times per second and superimposed on the basic retraction displacement command, so that the axial tracking error of the driven mandrel within the 1000mm transition stroke is kept within 0.01mm.

[0063] After the pipe is removed from the sizing mold, the actual surface temperature is used as the reference. A multi-segment medium-frequency induction heating zone with a total heating length of 450mm and continuous heating at 120℃ is introduced. The power control module is based on the instantaneous linear power density formula. Power control is performed, including real-time pipe wall thickness. The pipe wall thickness was measured at the outlet of the sizing mold; the theoretical density of the material was also measured. Take 8000 kg / m³, high temperature average isobaric specific heat capacity Take 550 joules per kilogram of Kelvin, outer diameter Take 0.060m as the target complete solution temperature. Take 1180℃ as the overall efficiency constant of induction electrothermal conversion. The power control module uses a value of 0.75 to determine the control values ​​at both ends based on the instantaneous linear power density corresponding to the thin-walled and thick-walled sections. In the transition section with varying wall thickness, it linearly adjusts the control values ​​between the two ends based on the real-time pipe wall thickness, so that the instantaneous linear power density increases linearly with the increase of the real-time pipe wall thickness. The output power is determined in combination with the effective working length of the medium-frequency induction heating coils in each section, so that the heating power from the thin-walled section to the thick-walled section is dynamically adjusted between 52.25kW and 97.84kW. The pipe body heats up to 1180℃ within 3.2s. In the subsequent high-temperature section of the medium-frequency induction heating zone and in the high-temperature ceramic fiber insulation and heat-spreading sleeve coaxially connected to its outlet, the solid solution temperature is maintained, so that the axial residence time of the pipe body in the range of 1160℃ to 1200℃ reaches 15s, causing discontinuous static recrystallization of austenite and complete solid solution of deformation-induced carbonitrides.

[0064] After online solution heating is completed, the pipe is introduced into a high-pressure annular spray zone within 0.6 seconds. This zone comprises four sets of axially staggered annular water spray manifolds, with an axial spacing of 50 mm between adjacent sets. Each manifold contains 16 pressure atomizing nozzles evenly distributed around its circumference. These nozzles use 1.2 MPa deionized water and apply a 45° angled impact jet along the outer circumference of the pipe, simultaneously tilting the nozzle axis 20° in the opposite direction to the pipe's discharge direction, creating a reverse impact water curtain. The average cooling rate of the pipe wall from 1180°C to 350°C reaches 106.4°C / s, rapidly passing through the sensitization temperature range of 650°C to 1000°C, thus blocking... phase and Phase precipitation occurs; the resulting finished pipe has a single-phase austenitic equiaxed grain structure with an average grain size of ASTM 7.1 to 7.5 across all cross sections along its entire length, with a yield strength stable at 342 MPa to 368 MPa, elongation after fracture maintained at 48.5% to 52.0%, and critical pitting temperature maintained above 75℃.

[0065] The embodiments of this application have been described above with reference to the accompanying drawings. Unless otherwise specified, the embodiments and features in the embodiments of this application can be combined with each other. This application is not limited to the specific implementation methods described above. The specific implementation methods described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of this application without departing from the spirit and essence of this application, and all of these forms are within the protection scope of this application.

Claims

1. A one-step drawing process for constant outer diameter variable wall thickness steel tube, characterized in that, Includes the following steps: Step S1: Based on the axially preset wall thickness reduction rate distribution of the super austenitic corrosion-resistant stainless steel billet tube from 0.15 to 0.55, axial gradient preheating is carried out on the super austenitic corrosion-resistant stainless steel billet tube. The preheating temperature of the small deformation thick wall section is controlled at 180°C to 250°C, and the preheating temperature of the large deformation thin wall section is controlled at 300°C to 380°C, so that the initial deformation resistance of the high reduction rate section is lower than that of the low reduction rate section. Step S2: The outer diameter of the super austenitic corrosion-resistant stainless steel billet is constrained by the sizing outer die. The follower mandrel is driven to move axially to adjust the annular deformation gap between the inner hole of the sizing outer die and the outer circumference of the follower mandrel. The billet is drawn at a drawing speed of 15 mm / s to 45 mm / s to form a variable wall thickness tube with a constant outer diameter and a gradient change in inner diameter in a single pass. Step S3: After drawing and demolding, the variable wall thickness tube is continuously introduced into the multi-segment medium-frequency induction heating zone. The output power of the medium-frequency induction heating coils of each segment is dynamically adjusted according to the real-time tube wall thickness and drawing speed measured at the sizing die outlet, so that the tube is heated to 1160℃ to 1200℃ within 2.0s to 5.0s. The axial residence time in the 1160℃ to 1200℃ range is 8s to 20s, so that the austenite undergoes discontinuous static recrystallization and the deformation-induced carbonitrides are completely dissolved. Step S4: The tube material removed from the medium-frequency induction heating zone is introduced into the high-pressure annular spray zone within 0.8s, and rapid quenching is performed by applying a collision impact jet. The average cooling rate of the tube wall from 1160℃ to below 400℃ is controlled to be greater than 90℃ / s, thereby blocking the precipitation of intermetallic phases in the sensitization temperature range of 650℃ to 1000℃.

2. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, The chemical composition of the super-austenitic corrosion-resistant stainless steel pipe blank contains, by mass percent: C 0.020%, 0.60%, 1.00%, Cr 19.5% to 21.0%, Ni 17.5% to 18.5%, Mo 6.0% to 6.8%, N 0.18% to 0.25%, Cu 0.50% to 1.00%, 0.030%, 0.010%, with the balance being Fe and impurities; and a pitting resistance equivalent number PREN is calculated by the sum of the Cr mass percent, 3.3 times the Mo mass percent, and 16 times the N mass percent and is greater than or equal to 43.

0.

3. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, Before performing axial gradient preheating on the super austenitic corrosion-resistant stainless steel billet in step S1, the process further includes: step S11, sandblasting to remove oxide scale and pickling passivation of the inner and outer surfaces of the super austenitic corrosion-resistant stainless steel billet with mixed acid, depositing an oxalate conversion film with a thickness of 3μm to 8μm on the inner and outer surfaces of the billet; step S12, coating the outer surface of the oxalate conversion film with a composite lubricant and drying and curing it, wherein the composite lubricant contains 15% to 25% by mass of molybdenum disulfide micro powder, 5% to 10% by mass of polytetrafluoroethylene micro powder, and the balance being modified waterborne acrylic resin.

4. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, In step S1, the axial gradient preheating of the super austenitic corrosion-resistant stainless steel billet tube specifically includes: step S13, controlling the preheating temperature of the thick-walled section with a wall thickness reduction rate of 0.15 to 0.25 to be 180℃ to 250℃, and controlling the preheating temperature of the thin-walled section with a wall thickness reduction rate of 0.45 to 0.55 to be 300℃ to 380℃; step S14, in the variable wall thickness transition section, continuously and smoothly adjusting the induction heating power within the range of 180℃ to 380℃ based on the axial displacement monitoring signal, so that the target preheating temperature increases linearly with the increase of the wall thickness reduction rate.

5. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, In step S2, the sizing die is made of cemented carbide, the inner diameter of the sizing zone of the die hole is constant, and the working cone angle of the die inlet is 12°. The drawing process specifically includes: step S21, when drawing the thin-walled section, driving the follower mandrel to the front limit position to form the minimum deformation gap; step S22, when drawing the variable wall thickness transition section, controlling the follower mandrel to retract at a controlled speed; step S23, when drawing the thick-walled section, controlling the follower mandrel to retract to the rear stable position and keep it stationary to form the maximum deformation gap, and keeping the drawing force in the range of 120kN to 210kN.

6. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, In step S3, the total heating length of the multi-segment medium-frequency induction heating zone along the axial direction is 450mm. Specifically, it includes: step S31, where the instantaneous linear power density of the medium-frequency induction heating coils applied to the axial position of each segment increases linearly with the increase of the real-time pipe wall thickness, so that the pipe material is heated from the demold surface temperature of 120℃ to the target solid solution temperature of 1180℃. The induction output power is matched in the thin-walled section and the thick-walled section respectively, and the heating time is controlled to be 2.0s to 5.0s.

7. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, Step S3 further includes: Step S32, in the multi-segment medium-frequency induction heating zone, the austenitic equiaxed grains are regenerated and the carbonitrides are completely dissolved in the temperature range of 1160℃ to 1200℃, so as to obtain a single-phase austenitic equiaxed grain structure with an average grain size level of ASTM 7.0 to 8.0 over the entire length.

8. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, In step S4, the high-pressure annular spray zone includes four sets of annular water spray manifolds arranged axially in a staggered manner. Each manifold has 16 pressure atomizing nozzles evenly distributed around its circumference. Specifically, step S41 involves controlling the axial distance between two adjacent sets of annular water spray manifolds to be 40mm to 60mm, tilting the nozzle axis 15° to 30° in the opposite direction of the pipe discharge to form a reverse impact water curtain, and applying jet flushing with deionized water at a pressure of 0.8MPa to 1.5MPa.

9. The one-time drawing process for a steel pipe with constant outer diameter and variable wall thickness according to claim 1, characterized in that, After the pipe is removed from the high-pressure annular spray zone, its surface moisture is dried online. Through the coordinated processes of axial gradient preheating in step S1, follower mandrel drawing in step S2, online medium-frequency induction heating in step S3, and high-pressure annular spray quenching in step S4, a σ-free surface is obtained across the entire cross-section of the pipe. The single-phase austenitic structure precipitated by the χ phase results in a critical pitting temperature greater than or equal to 75.0℃, an intergranular corrosion rate less than or equal to 0.13mm / a, a yield strength of 330MPa to 380MPa, a tensile strength of 680MPa to 760MPa, and an elongation after fracture greater than or equal to 45% for all sections of the finished variable wall thickness pipe.