A high plasticity nickel-tungsten alloy shaped charge liner and a hot extrusion forming method thereof

By employing a one-step hot extrusion near-net-shape forming process and solution heat treatment, the problems of high-temperature processing cracking and low material utilization of nickel-tungsten alloy shaped charges have been solved, achieving high plasticity and toughness and efficient production.

CN123149268APending Publication Date: 2026-11-24西部超导材料科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611388071.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively solve the problem of high-temperature processing cracking of nickel-tungsten alloy shaped charges, and cannot achieve near-net-shape forming of complex thin-walled rotary structures, resulting in low material utilization and high production efficiency and cost.

Method used

A one-step hot extrusion near-net-shape forming process is adopted, combined with a high-temperature protective coating and a closed cavity mold. The nickel-tungsten alloy liner blank is prepared by single hot extrusion and then subjected to solution heat treatment to achieve triaxial compressive stress forming, eliminate tensile stress zone, and ensure material utilization and microstructure uniformity.

Benefits of technology

Stable plastic forming of nickel-tungsten alloy shaped charges has been achieved, with a material utilization rate of over 90%, significantly improving plasticity, toughness, and production efficiency, and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149268A_ABST
    Figure CN123149268A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of nickel-tungsten alloy hot working technology, and relates to a high-ductility and high-toughness nickel-tungsten alloy liner and its hot extrusion forming preparation method. The method includes the following steps: First, after homogenizing and annealing a nickel-tungsten alloy ingot, a high-temperature protective coating is applied to its surface, followed by heating to the hot extrusion temperature and holding at that temperature to obtain a nickel-tungsten alloy billet; second, the nickel-tungsten alloy billet is placed in a preheated extrusion die, and a one-step hot extrusion near-net-shape forming process is used to obtain a nickel-tungsten alloy liner blank; finally, the nickel-tungsten alloy liner blank is subjected to solution heat treatment, and after finishing, a nickel-tungsten alloy liner is obtained. This invention solves the problems of multiple hot forging processes, high material loss, and large machining operations associated with existing nickel-tungsten alloy liner hot forging processes. By relying on a single hot extrusion to directly achieve near-net-shape forming of the nickel-tungsten alloy liner, it not only effectively shortens the process and reduces production costs, but also produces a nickel-tungsten alloy liner with both high ductility and toughness and a uniform microstructure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nickel-tungsten alloy hot working technology, and relates to a high-ductility and high-toughness nickel-tungsten alloy liner and its hot extrusion molding preparation method. Background Technology

[0002] Nickel-tungsten alloys have a moderate density (11~13 g / cm³). 3 With excellent dynamic ductility and high sound wave propagation speed, nickel-tungsten alloy (LTA) is a promising candidate material for next-generation shaped charge liner applications. LTA applications place stringent demands on the comprehensive performance of raw materials, requiring high density, ultra-high plasticity, and high impact toughness. The formed components must also meet quality requirements such as uniform wall thickness and the absence of micropores and microcracks. However, LTA alloys have a high tungsten content, making them typical difficult-to-deform alloys. These alloys exhibit high resistance to high-temperature deformation, a narrow hot working temperature range, and are highly sensitive to tensile stress. The additional tensile stress generated by traditional hot working easily leads to corner cracking defects in the blank.

[0003] Current nickel-tungsten alloy liner manufacturing processes have significant technical shortcomings. Traditional methods primarily involve multi-stage hot forging combined with large-margin machining. While hot forging can break up coarse dendritic structures in the cast state, a single forging operation can only achieve simple deformations such as upsetting and drawing. Furthermore, the open forging process leaves the billet's sides unconstrained, inevitably creating localized tensile stress zones that easily lead to cracks on the surface and edges of the nickel-tungsten alloy billet. More importantly, hot forging can only produce solid bar or square billets, and cannot directly form thin-walled rotating liner liners with internal cavities. Subsequent machining processes such as turning, boring, and milling are required to remove a large amount of substrate for the inner and outer conical surfaces and the internal cavity, resulting in a utilization rate of less than 60% for the expensive nickel-tungsten alloy material. Simultaneously, the repeated heating process is energy-intensive, causes severe oxidation and peeling on the workpiece surface, and results in a cumbersome overall process with low production efficiency.

[0004] Existing research has also disclosed technical solutions for preparing nickel-tungsten alloy plates using rolling processes. Specifically, while multi-pass cold rolling combined with intermediate annealing can refine the alloy grains, the rolling deformation is mainly in a plane strain state, resulting in concentrated tensile stress at the edges of the plate. For nickel-tungsten alloys, which are sensitive to tensile stress, edge cracking defects are prone to occur. Moreover, the rolling process can only produce flat plates and solid bars, and cannot directly obtain the rotary thin-walled structure specifically for shaped charge covers. Furthermore, if rolled plates are used for welding and machining to form shaped charge covers, additional welding interfaces or multiple cutting processes will be introduced, making it difficult to guarantee the dimensional accuracy of the component wall thickness and the uniformity of the overall microstructure. If the internal cavity is machined by deep hole drilling and boring of rolled bars, the problems of high material loss and high manufacturing costs still exist.

[0005] In summary, neither hot forging nor rolling, two conventional plastic processing techniques, can eliminate harmful tensile stress during the forming process, making it difficult to solve the problem of cracking during high-temperature processing of nickel-tungsten alloys. Furthermore, neither of them can achieve near-net-shape forming of complex thin-walled rotary structures for shaped charges.

[0006] Therefore, there is an urgent need to provide a high-ductility and high-toughness nickel-tungsten alloy liner and its hot extrusion molding preparation method to solve the above problems. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art and to propose a high-ductility and high-toughness nickel-tungsten alloy liner and its hot extrusion molding preparation method.

[0008] To achieve the above objectives, the present invention provides the following technical solution: Firstly, such as Figure 1 As shown, this invention discloses a hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy liner, comprising the following steps: Step 1: After homogenizing and annealing the nickel-tungsten alloy ingot, a high-temperature protective coating is applied to its surface, and then it is heated to the hot extrusion temperature and held at the temperature to obtain the nickel-tungsten alloy billet. Step 2: Place the nickel-tungsten alloy billet in a preheated extrusion die and use a one-step hot extrusion near-net-shape forming process to obtain a nickel-tungsten alloy liner blank; Step 3: Perform solution heat treatment on the nickel-tungsten alloy shaped charge blank, and then perform precision machining to obtain the nickel-tungsten alloy shaped charge.

[0009] Specifically, in step 1, the homogenization annealing is carried out in an atmospheric environment at normal pressure. After the homogenization annealing is completed, the nickel-tungsten alloy ingot is cooled to room temperature in air.

[0010] Specifically, in step 2, the extrusion mold is a closed-cavity mold, and the cavity of the closed-cavity mold matches the inner cone angle and outer contour dimensions of the nickel-tungsten alloy liner.

[0011] More specifically, the nickel-tungsten alloy shaped charge blanks produced by the extrusion die have a wall thickness deviation of no more than 0.2 mm, and the blank surface is free of oxidation and cracking defects, and the interior is free of shrinkage cavities and shrinkage porosity metallurgical defects.

[0012] Furthermore, in step 1, the homogenization annealing temperature is 1150~1250℃, and the holding time is 10~20h.

[0013] Furthermore, in step 1, the hot extrusion temperature is 1150~1200℃, and the holding time is 30~90min.

[0014] Furthermore, in step 2, the preheating temperature of the extrusion die is 250~450℃, and the preheating time is ≥30min.

[0015] Furthermore, in step 2, the extrusion speed of the one-step hot extrusion near-net-shape forming process is 60~100mm / s, and the extrusion ratio is 8~25; the final extrusion temperature of the nickel-tungsten alloy liner blank is ≥1000℃.

[0016] Furthermore, in step 3, the solution heat treatment temperature is 1050~1150℃, and the holding time is 2~4h.

[0017] Specifically, after the solution heat treatment and heat preservation are completed, water cooling is used.

[0018] Furthermore, in step 1, the high-temperature protective coating is a high-temperature antioxidant coating, and the thickness of the high-temperature antioxidant coating is 50~200μm.

[0019] Specifically, the high-temperature antioxidant coating is preferably a yttrium oxide-based coating or a glass-based coating.

[0020] Secondly, this invention discloses a high-ductility and high-toughness nickel-tungsten alloy liner, which is prepared by the hot extrusion molding method for high-ductility and high-toughness nickel-tungsten alloy liners described in the first aspect above. The elongation of the nickel-tungsten alloy liner is ≥75%, and the impact toughness is ≥700 J / cm. 2 .

[0021] Specifically, the material utilization rate of the nickel-tungsten alloy liner is ≥90%.

[0022] Compared with the prior art, the present invention has the following beneficial effects: First, the present invention adopts a one-step hot extrusion near-net-shape forming process, which ensures that the nickel-tungsten alloy billet is subjected to strong triaxial compressive stress throughout the extrusion cylinder, which can significantly suppress crack nucleation and propagation, and realize the stable plastic forming of the difficult-to-deform nickel-tungsten alloy. It effectively overcomes the technical defects of traditional hot forging and rolling processes, which generate local tensile stress zones and cause cracking of billet edges and surfaces.

[0023] Meanwhile, this one-step hot extrusion near-net-shape forming process requires only a single heating and deformation to complete the main body of the shaped charge liner, avoiding the multiple temperature rises and falls caused by repeated heating in traditional hot forging. Traditional hot forging involves significant temperature drops in the billet between each heating cycle, easily causing the billet to fall into the low-temperature brittle range, leading to cracking. Furthermore, the processing temperature of nickel-tungsten alloys is 950~1200℃, with a safe hot working temperature range of only 250℃. Nickel-tungsten alloy billets are highly sensitive to temperature drops. The one-step hot extrusion near-net-shape forming process provided by this invention features a fast deformation rate and a short forming cycle, making the overall temperature drop of the nickel-tungsten alloy billet controllable. This ensures that the deformation process remains stable within the alloy's safe hot working window, fundamentally avoiding the risk of billet cracking due to excessive temperature drops.

[0024] Secondly, this invention can directly produce a nickel-tungsten alloy liner blank with an inner cavity and an outer conical surface through a single hot extrusion process, with a finished wall thickness deviation of ≤0.2 mm. This eliminates the need for large-scale machining processes such as turning and boring after hot forging or rolling. The material utilization rate of this invention exceeds 90%, far higher than that of traditional hot forging and rolling processes, significantly saving high-cost nickel-tungsten alloy raw materials and reducing manufacturing costs.

[0025] Third, this invention, through precise matching of hot extrusion process parameters, promotes full dynamic recrystallization of the nickel-tungsten alloy ingot during deformation; combined with subsequent solution heat treatment, a uniform and refined grain structure can be obtained. The nickel-tungsten alloy liner prepared by the method of this invention has an elongation after fracture ≥75% and a room temperature impact toughness ≥700 J / cm². The above-mentioned excellent comprehensive plasticity and toughness can ensure that it forms a continuous and stable high-speed metal jet under detonation load.

[0026] In summary, this invention, relying on the characteristics of hot extrusion triaxial compressive stress forming, overcomes the technical challenge of easy cracking during high-temperature plastic processing of nickel-tungsten alloys; it achieves near-net-shape forming of complex thin-walled rotary structures of shaped charges in one step; and while ensuring uniform matrix structure and obtaining ultra-fine grain and ultra-high plasticity and toughness microstructure, the material utilization rate is increased to over 90%, providing a complete and feasible technical solution for the short-process, low-cost, and high-performance industrial manufacturing of nickel-tungsten alloy shaped charges. Attached Figure Description

[0027] The accompanying drawings are incorporated in and form part of this specification, and together with the description serve to explain the principles of the invention.

[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0029] Figure 1 A flowchart of a hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner provided by the present invention; Figure 2 This is a microstructure diagram of the nickel-tungsten alloy shaped charge liner L-1 prepared in Example 1 of the present invention; Figure 3 This is a microstructure diagram of the nickel-tungsten alloy shaped charge liner L-2 prepared in Example 2 of the present invention; Figure 4 This is a microstructure diagram of the nickel-tungsten alloy shaped charge liner L-3 prepared in Example 3 of the present invention; Figure 5 This is a microstructure diagram of the nickel-tungsten alloy shaped charge liner L-4 prepared in Example 4 of the present invention; Figure 6 This is a comparison diagram of the plasticity properties of the nickel-tungsten alloy shaped charges prepared in Examples 1-4 of this invention; Figure 7 This is a comparison chart of the toughness properties of the nickel-tungsten alloy propellant liner prepared in Examples 1-4 of this invention; Figure 8 This is a comparison chart of material utilization rates between Examples 1-4 of the present invention and Comparative Example 1. Detailed Implementation

[0030] Exemplary embodiments will now be described in detail. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples consistent with some aspects of the invention as detailed in the appended claims.

[0031] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0032] Example 1 This embodiment discloses a hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy liner, including the following steps: Step 1: Place the nickel-tungsten alloy ingot in a heat treatment furnace and perform homogenization annealing at 1200℃ and atmospheric pressure for 15 hours. After holding at this temperature, remove the ingot and cool it to room temperature in air. Then, coat the surface of the nickel-tungsten alloy ingot with a 100μm thick yttrium oxide-based high-temperature anti-oxidation coating. After coating, place the ingot in a heat treatment furnace, heat it to 1180℃ and hold it for 60 minutes to obtain the nickel-tungsten alloy billet. Step 2: Select a closed-cavity die. The cavity of this extrusion die matches the inner cone angle and outer contour dimensions of the nickel-tungsten alloy liner. Preheat the closed-cavity die at 350℃ for 40 minutes. Then, remove the nickel-tungsten alloy billet from the heat treatment furnace and place it into the preheated closed-cavity die. Perform a one-step hot extrusion near-net-shape forming process to obtain the nickel-tungsten alloy liner blank. Specifically, the extrusion speed of the one-step hot extrusion near-net-shape forming process is 80 mm / s, and the extrusion ratio is 15. The final extrusion temperature of the nickel-tungsten alloy liner blank is 1050℃.

[0033] Step 3: The nickel-tungsten alloy shaped charge blank is subjected to solution heat treatment at 1100℃, held at the temperature for 3 hours, and then water-cooled. After precision machining, the nickel-tungsten alloy shaped charge L-1 is obtained.

[0034] Example 2 This embodiment discloses a hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy liner, including the following steps: Step 1: Place the nickel-tungsten alloy ingot in a heat treatment furnace and perform homogenization annealing at 1150℃ and atmospheric pressure for 20 hours. After holding at this temperature, remove the ingot and cool it to room temperature in the air. Then, coat the surface of the nickel-tungsten alloy ingot with a glass-based high-temperature anti-oxidation coating with a thickness of 150μm. After coating, place the ingot in a heat treatment furnace, heat it to 1150℃ and hold it for 90 minutes to obtain the nickel-tungsten alloy billet. Step 2: Select a closed-cavity mold. The cavity of this extrusion mold matches the inner cone angle and outer contour dimensions of the nickel-tungsten alloy liner. Preheat the closed-cavity mold at 250°C for 50 minutes. Then, remove the nickel-tungsten alloy billet from the heat treatment furnace and place it into the preheated closed-cavity mold. Perform a one-step hot extrusion near-net-shape forming process to obtain the nickel-tungsten alloy liner blank. Specifically, the extrusion speed of the one-step hot extrusion near-net-shape forming process is 60 mm / s, and the extrusion ratio is 20. The final extrusion temperature of the nickel-tungsten alloy liner blank is 1020°C.

[0035] Step 3: The nickel-tungsten alloy shaped charge blank is subjected to solution heat treatment at 1050℃, held at the temperature for 4 hours, and then water-cooled. After precision machining, the nickel-tungsten alloy shaped charge L-2 is obtained.

[0036] Example 3 This embodiment discloses a hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy liner, including the following steps: Step 1: Place the nickel-tungsten alloy ingot in a heat treatment furnace and perform homogenization annealing at 1250℃ and atmospheric pressure for 10 hours. After holding at this temperature, remove the ingot and cool it to room temperature in the air. Then, coat the surface of the nickel-tungsten alloy ingot with a 50μm thick yttrium oxide-based high-temperature anti-oxidation coating. After coating, place the ingot in a heat treatment furnace, heat it to 1200℃ and hold it for 30 minutes to obtain the nickel-tungsten alloy billet. Step 2: Select a closed-cavity mold. The cavity of this extrusion mold matches the inner cone angle and outer contour dimensions of the nickel-tungsten alloy liner. Preheat the closed-cavity mold at 450℃ for 30 minutes. Then, remove the nickel-tungsten alloy billet from the heat treatment furnace and place it into the preheated closed-cavity mold. Perform a one-step hot extrusion near-net-shape forming process to obtain the nickel-tungsten alloy liner blank. Specifically, the extrusion speed of the one-step hot extrusion near-net-shape forming process is 100 mm / s, and the extrusion ratio is 10. The final extrusion temperature of the nickel-tungsten alloy liner blank is 1080℃.

[0037] Step 3: The nickel-tungsten alloy shaped charge blank is subjected to solution heat treatment at 1150℃, held at that temperature for 2 hours, and then water-cooled. After precision machining, the nickel-tungsten alloy shaped charge L-3 is obtained.

[0038] Example 4 This embodiment discloses a hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy liner, including the following steps: Step 1: Place the nickel-tungsten alloy ingot in a heat treatment furnace and perform homogenization annealing at 1180℃ and atmospheric pressure for 18 hours. After holding at this temperature, remove the ingot and cool it to room temperature in the air. Then, coat the surface of the nickel-tungsten alloy ingot with a glass-based high-temperature anti-oxidation coating with a thickness of 200μm. After coating, place the ingot in a heat treatment furnace, heat it to 1160℃ and hold it for 75 minutes to obtain the nickel-tungsten alloy billet. Step 2: Select a closed-cavity die. The cavity of this extrusion die matches the inner cone angle and outer contour dimensions of the nickel-tungsten alloy liner. Preheat the closed-cavity die at 300℃ for 60 minutes. Then, remove the nickel-tungsten alloy billet from the heat treatment furnace and place it into the preheated closed-cavity die. Perform a one-step hot extrusion near-net-shape forming process to obtain the nickel-tungsten alloy liner blank. Specifically, the extrusion speed of the one-step hot extrusion near-net-shape forming process is 70 mm / s, and the extrusion ratio is 25. The final extrusion temperature of the nickel-tungsten alloy liner blank is 1000℃.

[0039] Step 3: The nickel-tungsten alloy shaped charge blank is subjected to solution heat treatment at 1080℃, held at that temperature for 3.5h, and then water-cooled. After precision machining, the nickel-tungsten alloy shaped charge L-4 is obtained.

[0040] Comparative Example 1 This comparative example provides a method for preparing a nickel-tungsten alloy, which employs a traditional multi-fire forging process and includes the following steps: Step 1: Place the nickel-tungsten alloy ingot in a heat treatment furnace and perform homogenization annealing at 1200℃ and atmospheric pressure. After holding at this temperature for 15 hours, remove the ingot and cool it to room temperature in the air. Step 2: The homogenized annealed nickel-tungsten alloy ingot is clad, then heated to 1180℃ and held for 4 hours. After holding, it is forged into an open billet. The open billet forging adopts the upsetting and drawing deformation method, with the upsetting ratio controlled at 1.5, the drawing deformation controlled at 30%, and the final forging temperature not lower than 1050℃. After forging, it is cooled in air to obtain an intermediate billet. Step 3: The intermediate billet is treated with a soft sleeve, heated to 1100℃ and held for 3 hours, and then subjected to 6 intermediate forgings. During each forging, upsetting and drawing deformation is carried out first, followed by alternating face forging, and finally octagonal reversal deformation. The upsetting ratio is controlled at 1.7, the drawing deformation is controlled at 40%, and the final forging temperature is not lower than 900℃. After forging, it is cooled in air to obtain a bar billet.

[0041] Step 4: The billet is solution treated at 1100℃ and held at that temperature for 3 hours, then removed from the furnace and water-cooled.

[0042] Step 5: Perform multiple machining operations on the water-cooled billet, including but not limited to turning, boring, and milling, to obtain the inner cavity and outer conical surface structure, and finally obtain the nickel-tungsten alloy shaped charge cover DB-1.

[0043] To verify the effectiveness of the hot extrusion molding method for preparing high-ductility nickel-tungsten alloy liner of the present invention, the material utilization rate, microstructure uniformity, elongation and impact toughness of the nickel-tungsten alloy liners prepared in Examples 1-3 and Comparative Example 1 were tested respectively, and the specific analysis is as follows.

[0044] See Figures 2-5 It can be seen that this invention, through a one-step hot extrusion near-net-shape forming process and supporting process parameters, can effectively eliminate the problems of original dendrites, casting porosity, and compositional segregation inside nickel-tungsten alloy ingots; all samples formed complete recrystallized grain structures, with a dense and intact overall structure, and no casting defects remained. From the microstructure diagrams of the various nickel-tungsten alloy liner casings, it can be seen that this process can stably achieve controllable grain refinement of nickel-tungsten alloys. The uniform and dense microstructure can fully coordinate plastic deformation, significantly improving the elongation and impact toughness of the alloy, meeting the requirements for the preparation and use of high-ductility and high-toughness nickel-tungsten alloy liner casings.

[0045] Further, see Figure 6 As shown, the elongation of the nickel-tungsten alloy shaped charge liner L-1 is 76%, that of the nickel-tungsten alloy shaped charge liner L-2 is 78%, that of the nickel-tungsten alloy shaped charge liner L-3 is 75%, and that of the nickel-tungsten alloy shaped charge liner L-4 is 80%. See also... Figure 7 As shown, the impact toughness of the nickel-tungsten alloy liner L-1 is 716 J / cm². 2 The impact toughness of the nickel-tungsten alloy liner L-2 is 723 J / cm². 2 The impact toughness of the nickel-tungsten alloy liner L-3 is 705 J / cm². 2 The impact toughness of the nickel-tungsten alloy liner L-4 is 738 J / cm². 2 The above data fully demonstrates that the one-step hot extrusion near-net-shape forming process of the present invention, combined with the matching solution heat treatment process, can significantly improve the plasticity and toughness of nickel-tungsten alloy liner, and can meet the application requirements of high plasticity and toughness nickel-tungsten alloy liner.

[0046] Figure 8 The material utilization rate test results, as shown in the figure, indicate that the material utilization rate of nickel-tungsten alloy shaped charge liner L-1 is 91%, that of nickel-tungsten alloy shaped charge liner L-2 is 92%, that of nickel-tungsten alloy shaped charge liner L-3 is 90%, that of nickel-tungsten alloy shaped charge liner L-4 is 93%, while that of nickel-tungsten alloy shaped charge liner DB-1 is only 55%. In terms of material utilization rate, this invention has a significant advantage over the traditional multi-fire forging process.

[0047] In summary, compared with the embodiments of the present invention, Comparative Example 1 adopts the traditional multi-fire hot forging combined with multi-cutting process, which has obvious shortcomings: (1) The process flow is long, the ingot needs to be reheated in the furnace and repeatedly forged, resulting in low production efficiency; (2) The material loss is large, the material utilization rate is only about 55%, which greatly increases the raw material production cost; (3) The overall energy consumption is high, and the billet will be severely oxidized on its surface due to repeated high-temperature heating.

[0048] Accordingly, the present invention adopts a one-step hot extrusion near-net-shape forming process, which can directly form a liner blank with an inner cavity and an outer conical surface, and has multiple outstanding advantages: (1) Forming can be completed in only one heat, greatly simplifying the process flow; the material utilization rate can reach more than 90%, greatly saving high-value nickel-tungsten alloy raw materials; (2) The overall energy consumption is lower, and the production process is green and environmentally friendly; (3) The microstructure of the nickel-tungsten alloy liner is uniform and dense, the elongation after fracture is not less than 75%, and the impact toughness is not less than 700J / cm. 2 Therefore, it is evident that the present invention represents a significant technological advancement compared to traditional processes.

[0049] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.

[0050] It should be understood that the present invention is not limited to the content already described above, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner by hot extrusion molding, characterized in that, Includes the following steps: Step 1: After homogenizing and annealing the nickel-tungsten alloy ingot, a high-temperature protective coating is applied to its surface, and then it is heated to the hot extrusion temperature and held at the temperature to obtain the nickel-tungsten alloy billet. Step 2: Place the nickel-tungsten alloy billet in a preheated extrusion die and use a one-step hot extrusion near-net-shape forming process to obtain a nickel-tungsten alloy liner blank; Step 3: Perform solution heat treatment on the nickel-tungsten alloy shaped charge blank, and then perform precision machining to obtain the nickel-tungsten alloy shaped charge.

2. The hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner according to claim 1, characterized in that, In step 1, the homogenization annealing temperature is 1150~1250℃, and the holding time is 10~20h.

3. The hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner according to claim 1, characterized in that, In step 1, the hot extrusion temperature is 1150~1200℃, and the holding time is 30~90min.

4. The hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner according to claim 1, characterized in that, In step 2, the preheating temperature of the extrusion die is 250~450℃, and the preheating time is ≥30min.

5. The hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner according to claim 1, characterized in that, In step 2, the extrusion speed of the one-step hot extrusion near-net-shape forming process is 60~100mm / s, and the extrusion ratio is 8~25; the final extrusion temperature of the nickel-tungsten alloy liner blank is ≥1000℃.

6. The hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner according to claim 1, characterized in that, In step 3, the solution heat treatment temperature is 1050~1150℃, and the holding time is 2~4h.

7. The hot extrusion molding method for preparing a high-ductility and high-toughness nickel-tungsten alloy propellant liner according to claim 1, characterized in that, In step 1, the high-temperature protective coating is a high-temperature antioxidant coating, and the thickness of the high-temperature antioxidant coating is 50~200μm.

8. A high-ductility and high-toughness nickel-tungsten alloy shaped charge liner, characterized in that, The nickel-tungsten alloy liner is prepared by the hot extrusion molding method for high-ductility and high-toughness nickel-tungsten alloy liners as described in any one of claims 1 to 7, wherein the elongation of the nickel-tungsten alloy liner is ≥75% and the impact toughness is ≥700 J / cm. 2 .