A negative pressure tube type semi-solid ultra-short process noble metal wire manufacturing device and process
By using a negative pressure tubular semi-solid ultra-short process manufacturing device and technology, the problems of lengthy processes and high material loss in the preparation of precious metal wires have been solved, achieving efficient preparation of continuous fine wires, simplifying the process and reducing oxidation loss.
Patent Information
- Application Number
- CN202611635517.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, the preparation process of precious metal wires is lengthy, the surface is prone to oxidation, and the material loss is large. Negative pressure suction casting cannot directly produce continuous fine wires, and there is a lack of short-process preparation solutions that simplify the process.
The negative pressure tubular semi-solid ultra-short process manufacturing device includes an insulated tank, a vacuum pump, a booster pump, a forming tube mold, an eddy current cooling tube assembly, an anti-broken wire buffer guide mechanism, and a constant tension take-up machine. Through the overall regulation of vacuum suction, pressurized liquid delivery, zoned temperature control, rapid cooling, and tension buffering, the continuous preparation of fine wires from molten metal is achieved.
It can directly produce 0.1-2mm continuous non-ferrous metal wires, which are especially suitable for small-batch production of precious metals. It eliminates many processes, reduces oxidation loss, and improves production efficiency. The length of a single roll can reach 500-3000m.
Smart Images

Figure CN123149269A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal wire preparation technology, specifically relating to a negative pressure tubular semi-solid ultra-short process precious metal wire manufacturing device and process, which is suitable for the rapid preparation of small batches of wires of non-ferrous metals such as copper, gold, and silver, especially precious metals. Background Technology
[0002] The conventional manufacturing process for metal wire involves multiple steps, including smelting, casting, hot rolling, and cold rolling / cold drawing. It requires a large amount of equipment, such as smelting furnaces, continuous casting machines, hot rolling mills, cold rolling mills, heat treatment furnaces, and take-up machines, making it more suitable for large-scale industrial production. For small-batch production of precious metal wires such as gold and silver, existing methods commonly use small induction furnaces to produce 6-8mm diameter cast rods via upward or downward drawing, followed by multiple cold drawing passes, with some steps requiring annealing. The existing process has significant drawbacks: a long process flow and high processing time; the wire surface is prone to oxidation during high-temperature processing, requiring additional peeling to ensure product surface quality, increasing material loss and processing costs; and the need to remove the beginning and end portions of the cast billet, further wasting precious metal materials.
[0003] Existing negative pressure suction casting technologies are mainly used to prepare block or rod-shaped ingot blanks. Even if the negative pressure suction casting equipment is simply copied, it is impossible to directly obtain continuous fine metal wires, especially ultrafine metal wires. The main technical obstacles are: the mismatch between extrusion and traction speeds during semi-solid extrusion of fine wires, and the instantaneous tension fluctuations that easily cause the fine wires to break. The ingot casting process lacks continuous and effective control for tension buffering of the fine wires, and can only produce short blanks, making it impossible to achieve kilometer-scale continuous fine wire production. Therefore, existing technologies lack a short-process continuous preparation scheme for small-batch precious metal wires that can simplify the process, reduce oxidation, and reduce material loss. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of existing technologies, such as lengthy preparation processes for small batches of precious metal wires, easy surface oxidation, large material losses, and the fact that negative pressure suction casting can only produce blanks and cannot directly obtain continuous fine wires. This invention provides a negative pressure tubular semi-solid ultra-short process device and process for manufacturing precious metal wires.
[0005] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A negative pressure tubular semi-solid ultra-short process precious metal wire manufacturing device includes an insulated tank, a vacuum pump, a booster pump, a forming tube mold, an eddy current cooling tube assembly, an anti-wire breakage buffer guide mechanism, a steering roller assembly, and a constant tension take-up machine. The heat preservation tank is used to contain molten metal liquid, and the heat preservation tank is equipped with a liquid level sensor for monitoring the liquid level of the melt; the outlet of the heat preservation tank is connected to a suction pipe; the suction pipe is connected to a vacuum pump and a booster pump through pipelines and valves respectively; A vacuum pressure sensor is installed on the pipeline of the vacuum pump. The vacuum pump is used to draw negative pressure on the pipeline and the suction pipe to realize melt suction and melt degassing. The booster pump is made of high-temperature resistant nickel-based high-temperature alloy. It is equipped with a built-in pressure sensor and the output pressure can be continuously adjusted in the range of 0.05-0.6MPa. The discharge end of the booster pump is sealed and connected to the feed end of the forming tube mold. The forming tube mold is equipped with a heating wire assembly that can be divided into temperature-controlled zones. The heating wire assembly is divided into at least two temperature-controlled zones: a feeding preheating zone and a semi-solid forming zone. The discharge end of the forming tube mold is equipped with a hard graphite mold hole with a diameter of 0.1-2mm. An argon gas inlet is provided on the side wall of the forming tube mold, which can introduce high-purity argon gas to form an argon gas isolation layer that isolates air. The discharge port of the forming tube mold is equipped with a vortex cooling tube assembly; the vortex cooling tube assembly is equipped with a low-temperature argon inlet and an argon outlet; The output end of the eddy current cooling tube assembly is sequentially arranged with an anti-broken wire buffer guide mechanism, a steering roller assembly, and a constant tension take-up machine. The anti-broken wire buffer guide mechanism includes a floating swing roller, a displacement sensor and a damping cylinder; the wire is wound on the floating swing roller, the damping cylinder provides damping support for the floating swing roller, and the displacement sensor collects the displacement signal of the floating swing roller and feeds it back to the constant tension take-up machine. The device is equipped with a complete temperature control system and a pressure measurement and control unit; the constant tension take-up machine is equipped with a closed-loop control system for traction speed, and the traction speed is continuously adjustable from 0.5-15m / min.
[0006] Furthermore, the floating roller of the anti-broken yarn buffer guide mechanism moves in real time following the tension fluctuation of the yarn. The displacement sensor feeds back the signal to the constant tension take-up machine, and the traction speed is corrected in a closed loop to suppress the breakage of the nascent yarn caused by instantaneous tension changes.
[0007] Furthermore, the semi-solid forming zone of the forming tube mold is used to maintain the metal in a semi-solid region where solid and liquid coexist; the temperature of the preheating zone of the forming tube mold feed is 10-30℃ higher than the metal melting point.
[0008] Furthermore, the vortex cooling tube assembly is circulated with low-temperature argon gas as a cooling medium, which can achieve a wire cooling rate of 80-300℃ / s.
[0009] This invention also provides a negative pressure tubular semi-solid ultra-short process for manufacturing precious metal wires, using the aforementioned manufacturing apparatus, and includes the following steps: S1. Metal smelting: The non-ferrous metal raw materials to be processed are melted into molten metal using an induction furnace, resistance furnace, electric arc furnace, or electron beam furnace. The superheated temperature of the melt is 20-60°C higher than the melting point of the corresponding metal. The molten metal is then transferred into a heat preservation tank and kept at a temperature 10-40°C higher than the melting point of the metal. S2. Negative Pressure Liquid Suction Melt Purification: Close the valve, start the vacuum pump, and evacuate the pipeline system to a negative pressure range of 50-800Pa. Using vacuum suction, the molten metal inside the insulated tank is drawn into the pipeline through the suction pipe. The vacuum pump's vacuum level is adjusted in real-time based on feedback from the liquid level sensor. Under negative pressure, hydrogen and oxygen are released from the molten metal, and low-boiling-point impurities are volatilized and removed, completing the online purification of the melt. For volatile precious metals, the negative pressure of the pipeline system is selected to be 200-800Pa; for metals with low volatility, such as copper, the negative pressure of the pipeline system is selected to be 50-300Pa. S3. Boosting feeding: Turn on the booster pump and open the valve. The molten metal enters the booster pump under the combined action of gravity and the pushing pressure of the booster pump; the output pushing pressure of the booster pump is controlled at 0.05-0.6MPa. S4. Partial Temperature Controlled Semi-Solid Extrusion Molding: A booster pump forces molten metal into the forming die; the temperature of the preheating zone of the forming die is 10-30°C higher than the metal's melting point; the temperature of the semi-solid forming zone is controlled to the solid-liquid two-phase temperature window of the metal, and the volume fraction of the solid phase of the semi-solid metal is strictly controlled between 30-70%; if the solid phase fraction is below 30%, the melt has excessive fluidity and is prone to wire breakage; if the solid phase fraction is above 70%, the extrusion die resistance is too high and continuous extrusion is impossible; the semi-solid metal is extruded through the hard graphite die hole to form a continuous nascent filament; high-purity argon gas is continuously introduced into the forming die to form an argon gas isolation layer to isolate oxygen and prevent oxidation of the high-temperature melt and the nascent filament; S5. Rapid cooling: The extruded nascent filament immediately enters the vortex cooling tube group for forced rapid cooling. The cooling medium is low-temperature argon gas, and the cooling rate is controlled at 80-300℃ / s. The nascent filament quickly and completely solidifies to obtain solid metal filament. S6. Tension Buffering and Traction Take-up: The solid wire first passes through the anti-breakage buffering guide mechanism for tension buffering. The floating swing roller, combined with the displacement sensor, provides real-time feedback on the wire tension fluctuations and continuously adjusts the traction speed of the constant tension take-up machine. The constant tension take-up machine completes constant tension winding at a traction speed of 0.5-15m / min, resulting in finished metal wire with a diameter of 0.1-2mm. The entire process, from the melt entering the forming die to the wire completing eddy cooling, is conducted in an argon inert protective atmosphere. The finished wire surface is free of oxide scale, eliminating the need for subsequent peeling. The continuous length of a single roll of finished wire can reach 500-3000m.
[0010] Furthermore, the metal to be processed is elemental copper, gold, or silver; for silver, the temperature of the semi-solid forming zone is controlled at 880-940℃; for copper, the temperature of the semi-solid forming zone is controlled at 1050-1080℃; and for gold, the temperature of the semi-solid forming zone is controlled at 1040-1060℃.
[0011] Furthermore, in step S4, the solid phase volume fraction is controlled at 40-60%, which is a preferred range to adapt to continuous and stable extrusion filament production.
[0012] Furthermore, in step S6, during the filament operation, the anti-broken filament buffer guide mechanism controls the instantaneous tension fluctuation of the filament within ±15%, avoiding the breakage of the semi-solid extruded nascent filament.
[0013] While existing technologies may have separate units for negative pressure melt degassing, semi-solid forming, pressurized conveying, and argon protection, simply stacking these units cannot directly achieve continuous filament production. The nascent semi-solid extruded filaments have extremely low strength, and breakage occurs even with minor tension fluctuations during extrusion. This invention addresses this by employing a holistic approach: simultaneous negative pressure suction for melt purification, pressure-controlled booster pumping, zoned temperature-controlled semi-solid extrusion, rapid eddy current cooling, and anti-breakage tension buffering. This allows for the direct extrusion of molten metal into 0.1-2mm continuous ultrafine metal wires, eliminating the need for casting, hot rolling, multi-pass drawing, and intermediate annealing processes, shortening the processing cycle, and utilizing an inert protective atmosphere throughout to suppress oxidation and reduce precious metal loss.
[0014] The working principle of the device and process of this invention is as follows: First, a vacuum pump is used to draw molten metal under negative pressure, and the degassing and purification of low-boiling-point impurities are completed simultaneously during the drawing process. Then, the molten metal is sent into a zoned temperature-controlled forming mold by a pressure-controllable booster pump. The preheating zone of the forming mold ensures that the melt does not solidify prematurely, and the semi-solid forming zone precisely controls the ratio of the solid and liquid phases of the metal. The semi-solid material has suitable extrusion fluidity and can maintain a continuous filament shape after extrusion. The extruded filament is immediately cooled rapidly by a low-temperature argon vortex. To address the inherent technical problem of extremely low strength and easy breakage of the semi-solid extruded filament, this invention adds an anti-breakage buffer guide mechanism, which suppresses instantaneous tension impact through a closed-loop control of floating swing roller, displacement sensor, and take-up machine. Combined with argon gas isolation throughout the process, high-temperature oxidation is avoided. Continuous filament of the target specification is produced directly, eliminating multiple traditional processes such as rod casting, hot rolling, multi-pass drawing, and intermediate annealing. This invention differs from the traditional negative pressure suction casting technique for preparing ingot blanks. Traditional negative pressure suction casting can only produce short blanks and lacks effective tension buffering for fine wires, making it impossible to achieve kilometer-level continuous fine wires.
[0015] It should be noted that the anti-broken wire buffer guide mechanism of the present invention is not a direct copy of the existing mature wire winding tension buffer device; the existing tension buffer mechanism is applied to finished wire that has been completely solidified and has good mechanical properties; the tension buffer object in this application is the nascent filament that has just completed semi-solid extrusion, has undergone preliminary cooling, and has very fragile mechanical properties. This mechanism works in conjunction with the entire negative pressure-pressure-semi-solid extrusion-rapid cooling process to achieve stable preparation of kilometer-level continuous fine filaments.
[0016] The present invention has the following beneficial effects: First, it can directly prepare 0.1-2mm continuous non-ferrous metal wires, especially suitable for small-batch production of gold and silver precious metals, eliminating the entire process of casting rods, hot rolling, multi-pass drawing, and intermediate annealing, greatly improving processing efficiency compared to the traditional downward drawing method; Second, the vacuum suction stage simultaneously completes melt degassing and purification, simplifying the vacuum treatment process, eliminating the need for large-scale dedicated vacuum melting furnaces, and saving equipment space and production time; Third, argon gas protection is used throughout the forming and cooling process, resulting in no obvious oxidation on the wire surface, eliminating the need for subsequent descaling, reducing precious metal material loss, and the length of a single roll of continuous wire can reach 500-3000m; Fourth, the forming die has zoned temperature control, and the semi-solid solid phase fraction is controllable; the addition of an anti-breakage buffer guide mechanism effectively suppresses tension fluctuations, solving the technical obstacle of easy breakage of semi-solid fine wires, resulting in high process stability; Fifth, the metal melting is compatible with various melting equipment such as induction furnaces, resistance furnaces, electric arc furnaces, and electron beam furnaces, with a wide range of process adaptability. Attached Figure Description
[0017] Figure 1 This is a schematic diagram of the overall structure of the negative pressure tubular semi-solid ultra-short process precious metal wire manufacturing device of the present invention. Figure 2 This is a partially enlarged schematic diagram of the anti-broken wire buffer guide mechanism of the present invention.
[0018] in: 1-Insulated tank; 2-Liquid level sensor; 3-Suction pipe; 4-Valve; 5-Vacuum pump; 51-Vacuum pressure sensor; 6-Booster pump; 61-Booster pump built-in pressure sensor; 7-Forming mold; 71-Feeding preheating zone; 72-Semi-solid forming zone; 73-Heating wire assembly; 74-Hard graphite mold hole; 75-Argon gas inlet; 8-Edge cooling tube assembly; 81-Cryogenic argon gas inlet; 82-Argon gas outlet; 10-Anti-wire breakage buffer guide mechanism; 11-Directional roller assembly; 12-Constant tension take-up machine; 13-Temperature and pressure control unit.
[0019] 101-Floating swing roller; 102-Damping cylinder; 103-Displacement sensor; S-Metal wire; Bidirectional arrows indicate the floating direction of the floating swing roller; unidirectional arrows indicate the traveling direction of the wire. Detailed Implementation
[0020] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the embodiments.
[0021] Embodiments of the device of the present invention like Figure 1 , Figure 2As shown, a negative pressure tubular semi-solid ultra-short process precious metal wire manufacturing device includes an insulated tank 1, a vacuum pump 5, a booster pump 6, a forming tube mold 7, an eddy current cooling tube assembly 8, an anti-wire breakage buffer guide mechanism 10, a steering roller assembly 11, and a constant tension take-up machine 12.
[0022] The insulated tank 1 is used to hold molten metal. A liquid level sensor 2 is installed on the tank to collect the liquid level of the molten metal in real time. The outlet of the insulated tank is connected to a suction pipe 3, which is connected to a vacuum pump 5 and a booster pump 6 via a pipeline and a valve 4, respectively. A vacuum pressure sensor 51 is installed on the pipeline at the front end of the vacuum pump 5 to monitor the negative pressure of the pipeline in real time. The booster pump 6 is made of high-temperature resistant nickel-based high-temperature alloy, and the pump body integrates a built-in pressure sensor 61. The output pressure is continuously adjustable from 0.05 to 0.6 MPa. The outlet of the booster pump is sealed and connected to the inlet of the forming mold 7.
[0023] The forming tube mold 7 has a partially cross-sectional structure, with a heating wire assembly 73 arranged inside, dividing it into two independent temperature control zones: a feeding preheating zone 71 and a semi-solid forming zone 72. A replaceable hard graphite mold hole 74 with a diameter of 0.1-2mm is installed at the bottom of the forming tube mold. An argon gas inlet 75 is opened on the side wall of the forming tube mold to introduce high-purity argon gas, forming an argon gas isolation layer inside the tube mold that isolates oxygen.
[0024] The forming tube mold discharge end is connected to the vortex cooling tube assembly 8. The vortex cooling tube assembly is equipped with a low-temperature argon inlet 81 and an argon outlet 82, and relies on circulating low-temperature argon to achieve rapid cooling of the wire.
[0025] The output direction of the eddy current cooling tube assembly is sequentially arranged with an anti-breakage buffer guide mechanism 10, a steering roller assembly 11, and a constant tension take-up machine 12. Combined with... Figure 2 The anti-broken wire buffer guide mechanism 10 consists of a floating swing roller 101, a damping cylinder 102, and a displacement sensor 103. The metal wire S is wound around the floating swing roller 101, and the damping cylinder 102 provides elastic damping support to the floating swing roller. When the wire tension fluctuates, it drives the floating swing roller to move up and down. The displacement sensor 103 collects the swing roller displacement signal and feeds it back to the constant tension take-up machine 12. The closed-loop real-time correction of the traction speed suppresses the breakage of the nascent wire caused by instantaneous tension impact.
[0026] The entire device is equipped with a temperature and pressure control unit 13, which collects temperature measurement points, vacuum pressure, and booster pump output pressure signals in a unified manner; the constant tension take-up machine comes with a traction speed closed-loop control system, and the traction speed can be continuously adjusted from 0.5 to 15 m / min.
[0027] When this device is in operation, valve 4 is closed, and the vacuum pump draws negative pressure into the pipeline to draw the molten metal from inside the insulation tank into the pipeline, while simultaneously degassing the melt under negative pressure. Then, the booster pump is turned on and valve 4 is opened, and the melt is pressed into the forming die by the booster pump. After passing through the feeding preheating zone, it enters the semi-solid forming zone and is adjusted to a solid-liquid two-phase state. The nascent filament is extruded through the hard graphite die hole 74. The nascent filament enters the eddy cooling tube group for rapid solidification, passes through the anti-breakage buffer guide mechanism for tension adjustment, and is then guided by the steering roller group before being wound up by the constant tension take-up machine.
[0028] Example 1 of the present invention: Preparation of φ0.5mm pure silver wire (optimal implementation conditions) The following steps are taken to prepare 0.5mm pure silver wire using the apparatus of this invention: S1. Metal smelting: Pure silver raw material is melted in an induction furnace. The melt is superheated by 40°C and then transferred to a heat preservation tank. The temperature of the heat preservation tank is 25°C higher than the melting point of silver. S2. Negative pressure liquid suction melt purification: Close the valve, start the vacuum pump, and pump the pipeline to an absolute pressure of 400Pa; rely on the vacuum suction to draw the silver molten liquid in the heat preservation tank into the pipeline through the suction pipe; maintain the negative pressure according to the feedback of the liquid level sensor, and the silver molten liquid precipitates dissolved hydrogen gas under the negative pressure, and low boiling point impurities volatilize, thus completing the melt purification. S3. Boosting feeding: Start the booster pump, open the valve, the booster pump outputs a pressure of 0.2MPa, and the silver molten liquid enters the booster pump under the pushing action of gravity and the booster pump; S4. Partial Temperature Controlled Semi-Solid Extrusion Molding: A booster pump delivers molten silver into the forming die; the temperature of the preheating zone is 970℃, the temperature of the semi-solid forming zone is 910℃, and the volume fraction of the semi-solid silver phase is 50%; the die hole diameter is 0.5mm; high-purity argon gas is introduced into the die to form an argon gas isolation layer, and the semi-solid silver is extruded from the die hole to form the initial filament. S5. Rapid cooling: The nascent silver wire passes through a vortex cooling tube assembly and is cooled by low-temperature argon gas at a rate of 150℃ / s to obtain a solid silver wire; S6. Tension buffering and traction take-up: The wire passes through the anti-breakage buffering guide mechanism, and the tension fluctuation is controlled within ±12%; the constant tension take-up machine has a traction speed of 3m / min, and the silver wire is guided by the guide roller group to complete the winding, resulting in a φ0.5mm pure silver finished wire.
[0029] This embodiment produces silver wire with a bright, oxide-free surface, requiring no peeling, and a single roll length of up to 1200m; it can be produced in small batches, and the production efficiency is greatly improved compared to the traditional bottom drawing method, eliminating waste material from the beginning and end of the cast billet.
[0030] Example 2: Preparation of φ1.0mm pure copper wire (optimal implementation conditions) S1. Metal smelting: Oxygen-free copper raw material is melted in an electric resistance furnace. The melt is superheated to 35°C and the resulting molten copper is transferred to a heat preservation tank. The temperature of the heat preservation tank is 20°C higher than the melting point of copper. S2. Negative pressure liquid suction molten metal purification: Close the valve, start the vacuum pump, and pump the pipeline to an absolute pressure of 150Pa; negative pressure suction of copper molten metal, liquid level sensor monitors the liquid level in real time, under negative pressure conditions the molten metal precipitates hydrogen and oxygen gas, and low boiling point impurities volatilize and are purified. S3. Boosting feeding: Turn on the booster pump, open the valve, the booster pump outputs a pressure of 0.25MPa, and the molten copper enters the booster pump; S4. Partial temperature-controlled semi-solid extrusion forming of tube mold: The diameter of the forming tube mold hole is 1.0 mm; the temperature of the feeding preheating zone is 1090℃, the temperature of the semi-solid forming zone is 1065℃, and the volume fraction of copper semi-solid solid phase is 55%; high-purity argon gas is introduced for protection, and semi-solid copper is extruded from the die hole to form nascent filaments. S5. Rapid cooling: The vortex cooling tube assembly has a low-temperature argon cooling rate of 120℃ / s, which rapidly cools the nascent filament. S6. Tension buffer and traction take-up: The anti-breakage buffer guide mechanism controls the tension fluctuation ±10%; the constant tension take-up machine has a traction speed of 2.5m / min, guided by the steering roller group, and the take-up machine obtains φ1.0mm oxygen-free copper wire finished product.
[0031] In this embodiment, the copper wire surface is free of oxidation, eliminating the need for casting, hot rolling, and multiple drawing processes; the length of a single coil can reach 1800m, and the production efficiency is 20 times higher than that of traditional processes.
[0032] Example 3: Preparation of φ0.2mm gold wire (optimal implementation conditions) S1. Metal smelting: Gold raw materials are melted in an electron beam furnace. The melt is superheated by 30°C to obtain molten gold. The molten gold is then transferred to a heat preservation tank, where the temperature is 22°C higher than the melting point of gold. S2. Negative pressure liquid suction melt purification: Close the valve, start the vacuum pump, and pump the vacuum pipeline to an absolute pressure of 600Pa; vacuum suction of gold melt, liquid level sensor monitors the liquid level, negative pressure environment degassing of melt, low boiling point impurities volatilization purification. S3. Boosting feeding: Start the booster pump, open the valve, the booster pump outputs a pressure of 0.18MPa, and the molten gold enters the booster pump; S4. Partition temperature-controlled semi-solid extrusion forming of tube mold: The diameter of the forming tube mold hole is 0.2mm; the temperature of the feeding preheating zone is 1070℃, the temperature of the semi-solid forming zone is 1050℃, and the volume fraction of the gold semi-solid solid phase is 45%; high-purity argon gas is introduced to isolate air, and the semi-solid gold is extruded into nascent filaments. S5. Rapid cooling: The vortex cooling tube assembly uses cryogenic argon gas for rapid cooling at a rate of 200℃ / s; S6. Tension buffer and traction take-up: The anti-breakage buffer guide mechanism controls the tension fluctuation by ±13%; the constant tension take-up machine has a traction speed of 5m / min to complete the winding and obtain a φ0.2mm gold wire finished product.
[0033] This embodiment is suitable for small-batch trial production of precious metals, with low material loss and no need for peeling; the length of a single roll can reach 800m.
[0034] Example 4: Silver wire φ0.1mm (lower boundary condition) φ0.1mm silver wire was prepared; the solid fraction was 35%, the pipeline negative pressure was 200Pa, the booster pump pressure was 0.1MPa, and the traction speed was 0.8m / min; the anti-broken wire buffer mechanism was activated to obtain a single roll of 550m continuous wire; the surface of the wire was bright and free of oxidation.
[0035] Example 5: Silver wire φ2.0mm (Upper boundary condition) A φ2.0mm silver wire was prepared with a solid fraction of 65%, a pipeline negative pressure of 700Pa, a booster pump pressure of 0.5MPa, and a traction speed of 12m / min. A single roll of 2600m continuous wire with no oxide scale on the surface was obtained.
[0036] Comparative group Comparative Example 1: φ0.5mm silver wire was prepared using a traditional precious metal bottom casting rod + multi-stage drawing process; Preparation process: smelting - drawing to prepare 7mm silver casting rod - homogenization heat treatment - 9 cold drawing - 3 intermediate annealings; oxide scale removal and cutting off the head and tail waste of the casting billet are required; the maximum length of a single finished coil is 450m; frequent wire breakage, material loss exceeding 20%, production cycle up to 12 hours, and low efficiency.
[0037] Comparative Example 2: Silver billets were prepared using ordinary negative pressure suction casting without the forming tube mold zone temperature control and anti-broken wire buffer guide mechanism of the present invention; the other negative pressure and pressurization conditions were the same as in Example 1; only discontinuous short billets could be obtained, continuous fine wires could not be obtained, wire breakage occurred frequently, and finished wire materials could not be directly produced.
[0038] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. All equivalent substitutions and simple modifications made in accordance with the technical concept of the present invention shall fall within the protection scope of the present invention.
Claims
1. A negative pressure pipe type semi-solid ultra-short process precious metal wire manufacturing apparatus, characterized by, It includes an insulation tank (1), a vacuum pump (5), a booster pump (6), a forming tube mold (7), a vortex cooling tube assembly (8), an anti-broken wire buffer guide mechanism (10), a steering roller assembly (11), and a constant tension take-up machine (12); The heat preservation tank (1) is used to contain molten metal liquid. The heat preservation tank is equipped with a liquid level sensor (2) for monitoring the liquid level of the melt. The outlet of the heat preservation tank is connected to a suction pipe (3). The suction pipe (3) is connected to a vacuum pump (5) and a booster pump (6) through pipelines and valves (4). A vacuum pressure sensor (51) is installed on the pipeline of the vacuum pump (5). The vacuum pump is used to draw negative pressure on the pipeline and the suction pipe to realize melt suction and melt degassing. The booster pump (6) is made of high-temperature resistant nickel-based high-temperature alloy. The booster pump is equipped with a built-in pressure sensor (61). The output pressure of the booster pump can be continuously adjusted in the range of 0.05-0.6MPa. The discharge end of the booster pump is sealed and connected to the feed end of the forming tube mold (7). The forming tube mold (7) is internally equipped with a heating wire assembly (73) that can be divided into temperature-controlled zones. The heating wire assembly is divided into at least two temperature-controlled zones: a feeding preheating zone (71) and a semi-solid forming zone (72). The discharge end of the forming tube mold is equipped with a hard graphite mold hole (74), the diameter of which is 0.1-2mm. The side wall of the forming tube mold is provided with an argon gas inlet (75), which can be used to introduce high-purity argon gas to form an argon gas isolation layer that isolates air. The outlet of the forming tube mold (7) is equipped with a vortex cooling tube assembly (8); the vortex cooling tube assembly (8) is equipped with a low-temperature argon inlet (81) and an argon outlet (82); The output end of the eddy current cooling tube assembly (8) is sequentially arranged with an anti-broken wire buffer guide mechanism (10), a steering roller assembly (11), and a constant tension take-up machine (12); The anti-broken wire buffer guide mechanism (10) includes a floating swing roller (101), a displacement sensor (103), and a damping cylinder (102); The device is equipped with a temperature control and pressure measurement and control unit; the constant tension take-up machine (12) is equipped with a traction speed closed-loop control system, and the traction speed is continuously adjustable from 0.5 to 15 m / min.
2. The manufacturing apparatus according to claim 1, characterized by The floating roller (101) of the anti-broken yarn buffer guide mechanism (10) moves in real time following the tension fluctuation of the yarn. The displacement sensor (103) feeds back the signal to the constant tension take-up machine (12) to correct the traction speed in a closed loop and suppress the breakage of the nascent yarn caused by the instantaneous tension change.
3. The manufacturing apparatus according to claim 1, characterized by The semi-solid forming zone (72) of the forming tube mold (7) is used to maintain the metal in a semi-solid region where the solid and liquid phases coexist; the temperature of the forming tube mold feed preheating zone (71) is 10-30℃ higher than the metal melting point.
4. The manufacturing apparatus according to claim 1, characterized by The vortex cooling tube assembly (8) uses low-temperature argon gas as a cooling medium to achieve a wire cooling rate of 80-300℃ / s.
5. A negative pressure tube type semi-solid ultra-short process precious metal wire manufacturing process using the manufacturing device according to any one of claims 1 to 4, characterized by, Includes the following steps: S1. Metal smelting: The non-ferrous metal raw materials to be processed are melted into molten metal using an induction furnace, resistance furnace, electric arc furnace, or electron beam furnace. The superheated temperature of the melt is 20-60°C higher than the melting point of the corresponding metal. The molten metal is then transferred into a heat preservation tank and kept at a temperature 10-40°C higher than the melting point of the metal. S2. Negative Pressure Liquid Suction Melt Purification: Close the valve, start the vacuum pump, and evacuate the pipeline system to a negative pressure range of 50-800Pa. Using vacuum suction, the molten metal inside the insulated tank is drawn into the pipeline through the suction pipe. The vacuum level is adjusted in real-time based on feedback from the liquid level sensor. Under negative pressure, hydrogen and oxygen are released from the molten metal, and low-boiling-point impurities are volatilized and removed, completing the online purification of the melt. For volatile precious metals, the negative pressure of the pipeline system is selected to be 200-800Pa; for metals with low volatility, such as copper, the negative pressure of the pipeline system is selected to be 50-300Pa. S3. Boosting feeding: Turn on the booster pump and open the valve. The molten metal enters the booster pump under the combined action of gravity and the pushing pressure of the booster pump; the output pushing pressure of the booster pump is controlled at 0.05-0.6MPa. S4. Partial Temperature Controlled Semi-Solid Extrusion Molding: A booster pump forces molten metal into the forming die; the temperature of the preheating zone of the forming die is 10-30°C higher than the metal's melting point; the temperature of the semi-solid forming zone is controlled to the solid-liquid two-phase temperature window of the metal, and the volume fraction of the solid phase of the semi-solid metal is strictly controlled between 30-70%; if the solid phase fraction is below 30%, the melt is too fluid and prone to wire breakage; if the solid phase fraction is above 70%, the extrusion die resistance is too high and continuous extrusion is impossible; the semi-solid metal is extruded through the hard graphite die holes to form a continuous nascent filament; high-purity argon gas is continuously introduced into the forming die to form an argon gas isolation layer to isolate oxygen and prevent oxidation of the high-temperature melt and the nascent filament; S5. Rapid cooling: The extruded nascent filament immediately enters the vortex cooling tube group for forced rapid cooling. The cooling medium is low-temperature argon gas, and the cooling rate is controlled at 80-300℃ / s. The nascent filament quickly and completely solidifies to obtain solid metal filament. S6. Tension buffering and traction take-up: The solid wire first passes through the anti-breakage buffer guide mechanism for tension buffering. The floating swing roller combined with the displacement sensor provides real-time feedback on the tension fluctuation of the wire and adjusts the traction speed of the constant tension take-up machine. The constant tension take-up machine completes constant tension winding at a traction speed of 0.5-15m / min to obtain finished metal wire with a diameter of 0.1-2mm. The entire process, from the melt entering the forming mold to the wire completing eddy cooling, is conducted within an inert argon atmosphere.
6. The manufacturing process of claim 5, wherein, The metal to be processed is elemental copper, gold, or silver; for silver, the temperature of the semi-solid forming zone is controlled at 880-940℃; for copper, the temperature of the semi-solid forming zone is controlled at 1050-1080℃; and for gold, the temperature of the semi-solid forming zone is controlled at 1040-1060℃.
7. The manufacturing process of claim 5, wherein, In step S4, the solid phase volume fraction is controlled at 40-60%, which is the preferred range and suitable for continuous and stable extrusion filament production.
8. The manufacturing process of claim 5, wherein, In step S6, during the filament operation, the anti-broken filament buffer guide mechanism controls the instantaneous tension fluctuation of the filament within ±15%, avoiding the breakage of the semi-solid extruded nascent filament.