Superfine tungsten-cerium alloy wire and method for manufacturing the same

By using a composite lubrication method of graphite emulsion and vegetable oil, and dynamically controlling the lubrication layer, the problems of high wire breakage rate and high friction in the cold drawing process of ultrafine tungsten-cerium alloy wire were solved, improving production efficiency and wire quality, and realizing the efficient preparation of ultrafine tungsten-cerium alloy wire.

CN123149274APending Publication Date: 2026-11-24CHONGYI ZHANGYUAN TUNGSTEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611686135.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-29
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies for cold drawing ultrafine tungsten-cerium alloy wires suffer from problems such as high wire breakage rate, high friction, severe die wear, poor wire surface quality, and unsatisfactory mechanical properties. In particular, the lubrication effect decreases when drawing fine wires, affecting production efficiency and product quality.

Method used

A composite lubrication method using graphite emulsion and vegetable oil is adopted. By dynamically and synergistically controlling the thickness of the graphite emulsion coating, the drawing speed, and the compression ratio, a stable composite boundary lubrication layer is formed. Combining the fluidity of vegetable oil and the fixing effect of graphite particles, the lubrication performance is optimized.

Benefits of technology

It improved production efficiency, reduced mold wear, ensured the surface quality and mechanical properties of the wire, reduced the wire breakage rate, and achieved efficient preparation of ultrafine tungsten-cerium alloy wire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149274A_ABST
    Figure CN123149274A_ABST
Patent Text Reader

Abstract

This application belongs to the field of tungsten-cerium alloy wire manufacturing, specifically relating to an ultrafine tungsten-cerium alloy wire and its preparation method. The preparation method includes the following steps: S1, obtaining a first tungsten-cerium alloy wire, wherein, by mass percentage, the composition of the first tungsten-cerium alloy wire is: cerium: 1.2%-1.6%, with the remainder being tungsten and unavoidable impurities, and the wire diameter of the first tungsten-cerium alloy wire is 50-55 μm; S2, coating the surface of the first tungsten-cerium alloy wire with graphite emulsion to obtain a second tungsten-cerium alloy wire, and drying the second tungsten-cerium alloy wire to obtain a third tungsten-cerium alloy wire; S3, immersing the third tungsten-cerium alloy wire in vegetable oil and drawing it; S4, repeating steps S2 and S3 until an ultrafine tungsten-cerium alloy wire with a wire diameter ≤28 μm is obtained. This application adopts a scheme of dynamic synergistic control as the wire diameter decreases, and introduces a composite lubrication of graphite emulsion and vegetable oil to mitigate the adverse effects of graphite emulsion coating peeling on lubrication performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of tungsten-cerium alloy wire manufacturing, specifically relating to an ultrafine tungsten-cerium alloy wire and its preparation method. Background Technology

[0002] Diamond wire, as an essential consumable for cutting and manufacturing silicon wafers, directly affects the quality of the wafers and the efficiency of the cells. Diamond wire needs to be developed towards thinner and higher strength. Due to the high strength and ease of drawing of ultrafine tungsten-cerium alloy wire, it is chosen as the primary processing material for diamond wire. Ultrafine tungsten-cerium alloy wire uses cerium oxide as a dispersed reinforcing phase. Cerium oxide particles provide dispersion reinforcement while also improving the surface electronic structure of the material. Compared to the tungsten-cerium system, cerium oxide has a certain promoting effect on plastic deformation during cold drawing, which helps reduce the probability of wire breakage when drawing fine-gauge wires.

[0003] Current cold-drawn ultrafine tungsten-cerium alloy wires suffer from high friction during drawing, severe die wear, poor wire surface quality, high breakage rate, and unsatisfactory mechanical properties. Existing technologies mainly improve lubrication by modifying the composition of graphite emulsion. Graphite emulsion is an essential high-temperature lubricant for drawing refractory metal wires such as tungsten and molybdenum wires, possessing good lubricity and high-temperature coating properties, and does not peel off or burn between 600℃ and 1200℃. However, the performance of graphite emulsion is affected by multiple factors, including graphite powder particle size, viscosity, and dispersion stability. Graphite emulsion coatings are prone to cracking and peeling during drawing; coarse-particle graphite emulsion is easily extruded and detaches from the wire surface in the form of flakes and strips, causing lubrication failure, forming longitudinal grooves on the wire surface, and exacerbating matrix oxidation, which is detrimental to subsequent processing. For small-diameter ultrafine tungsten-cerium alloy wires, the adhesion and retention of the graphite emulsion coating are more difficult due to the increased wire surface area, making the reduced lubrication effect caused by coating peeling particularly prominent. Furthermore, the modified graphite emulsion has a complex composition, and deviations in pH and viscosity can affect the lubrication effect, thereby impacting the fiber breakage rate, surface quality, and mechanical properties. Due to its complex composition, the production conditions for preparing graphite emulsions also become stringent, posing a significant technical challenge in the production process.

[0004] Therefore, under the condition of low wire breakage rate, the production of ultra-long, continuous cold-drawing of ultra-fine tungsten-cerium alloy wires using conventional graphite emulsion is currently the main challenge. To address the problems of low drawing efficiency, high energy consumption, high wire breakage rate, poor wire diameter uniformity, and poor mechanical properties in the preparation process of ultra-fine tungsten-cerium alloy wires, a novel ultra-fine tungsten-cerium alloy wire and its preparation method are urgently needed. Summary of the Invention

[0005] To solve the above-mentioned technical problems, this application provides a method for preparing ultrafine tungsten-cerium alloy wire, comprising the following steps: S1, obtaining a first tungsten-cerium alloy wire, wherein, by mass percentage, the composition of the first tungsten-cerium alloy wire is: cerium: 1.2%-1.6%, the remainder being tungsten and unavoidable impurities, and the wire diameter of the first tungsten-cerium alloy wire is 50-55 μm; S2, coating the surface of the first tungsten-cerium alloy wire with graphite emulsion to obtain a second tungsten-cerium alloy wire, and drying the second tungsten-cerium alloy wire to obtain a third tungsten-cerium alloy wire; S3, immersing the third tungsten-cerium alloy wire in vegetable oil and drawing it; S4, repeating steps S2 and S3 until an ultrafine tungsten-cerium alloy wire with a wire diameter ≤28 μm is obtained.

[0006] As a preferred embodiment of the preparation method of the ultrafine tungsten-cerium alloy wire described in this application, the method of obtaining the first tungsten-cerium alloy wire in step S1 is specifically as follows: obtaining a tungsten-cerium alloy rod, and then forging and drawing the tungsten-cerium alloy rod to obtain the first tungsten-cerium alloy wire.

[0007] In a preferred embodiment of the method for preparing ultrafine tungsten-cerium alloy wire described in this application, in step S2, the specific gravity of the graphite emulsion is 1.010-1.013, and the viscosity of the graphite emulsion is 3.8-4.0 cP; the drying treatment is carried out in a multi-die hot drawing and drying furnace, wherein the length of the multi-die hot drawing and drying furnace is 50-60 cm, the speed of the multi-die hot drawing and drying furnace is 57-62 m / min, and the heating temperature of the multi-die hot drawing and drying furnace is 460-500℃.

[0008] In a preferred embodiment of the method for preparing an ultrafine tungsten-cerium alloy wire as described in this application, the temperature of the vegetable oil in step S3 is 50-55°C.

[0009] As a preferred embodiment of the preparation method of the ultrafine tungsten-cerium alloy wire described in this application, when the wire diameter of the tungsten-cerium alloy wire is ≥45μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is ≥1.8μm and ≤2.3μm, the drawing entry speed is ≥95m / min and ≤135m / min, and the drawing compression rate is ≥20% and ≤25%.

[0010] As a preferred embodiment of the preparation method of the ultrafine tungsten-cerium alloy wire described in this application, when the wire diameter of the tungsten-cerium alloy wire is >35μm and <45μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is >1.3μm and <1.8μm, the drawing inlet speed is >135m / min and <235m / min, and the drawing compression rate is >17% and <20%.

[0011] As a preferred embodiment of the preparation method of the ultrafine tungsten-cerium alloy wire described in this application, when the wire diameter of the tungsten-cerium alloy wire is ≤35μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is ≥0.8μm and ≤1.3μm, the drawing entry speed is ≥235m / min and ≤420m / min, and the drawing compression rate is ≥15% and ≤17%.

[0012] This application also provides an ultrafine tungsten-cerium alloy wire, which is prepared using the above-described method for preparing ultrafine tungsten-cerium alloy wire.

[0013] As a preferred embodiment of the ultrafine tungsten-cerium alloy wire described in this application, the diameter difference of the ultrafine tungsten-cerium alloy wire is ≤0.04μm.

[0014] As a preferred embodiment of the ultrafine tungsten-cerium alloy wire described in this application, the ultrafine tungsten-cerium alloy wire has a tensile strength ≥6400MPa, a coil diameter ≥120mm, and an average of ≤7 wire breaks per 100,000 kilometers.

[0015] This study found that when the diameter of the tungsten-cerium alloy wire is greater than 55 μm, a small amount of peeling off the graphite emulsion coating does not significantly weaken the lubrication performance; however, when the wire diameter is less than 50 μm, a small amount of peeling off the graphite emulsion coating significantly affects the lubrication effect. During the cold drawing process of tungsten-cerium alloy wire, as the wire diameter gradually decreases, the degree of hardening increases, the plasticity reserve decreases, and the probability of wire breakage increases. Simultaneously, problems such as accumulated frictional heat, unstable lubrication film, and fluctuations in drawing load also occur. In the coarse-gauge stage, the single-pass compression degree is high, requiring a large drawing load to offset friction and complete plastic forming, resulting in significant frictional heat accumulation, which easily leads to die wear and localized damage to the lubrication film. In the fine-gauge stage, due to insufficient strength margin and difficulty in ensuring the uniformity of the lubrication film thickness, fluctuations in drawing load are more likely to cause wire breakage. Especially under fine wire diameter conditions, the uniformity and continuity of the carbon layer on the tungsten wire surface are easily damaged, leading to peeling off of the graphite emulsion coating, decreased lubrication performance, further fluctuations in friction and drawing load, and an increased risk of wire breakage.

[0016] The beneficial effects of this application are as follows: This application proposes an ultrafine tungsten-cerium alloy wire and its preparation method. The method employs a dynamic synergistic control scheme as the wire diameter decreases, and introduces a composite lubrication system of graphite emulsion and vegetable oil to mitigate the adverse effects of graphite emulsion coating peeling on lubrication performance. Graphite, being a solid powder, has limited adhesion to metal surfaces; when used alone, the lubricating film is prone to peeling and exhibits poor uniformity. Vegetable oil contains natural polar molecules, and its fatty acid molecules have a strong adsorption effect on metal surfaces, forming a robust adsorption film that fixes graphite particles to the tungsten wire surface. Graphite nanoparticles can deposit at the friction interface to form a physical film, which, when superimposed with the vegetable oil adsorption film, constitutes a stable and dense composite boundary lubrication layer. Simultaneously, the fluidity of the vegetable oil can supplement the fluid lubrication layer between the friction pairs, further reducing the coefficient of friction. Even if localized peeling of the graphite emulsion occurs, the vegetable oil adsorption film can still provide effective lubrication, thereby mitigating the decline in lubrication performance.

[0017] Building upon this foundation, the coarse-gauge stage employs a higher compression ratio to improve efficiency, coupled with a thicker graphite emulsion coating to enhance lubrication and isolation, while simultaneously using a lower drawing speed to suppress heat accumulation. The medium-gauge stage gradually transitions between compression ratio, coating thickness, and drawing speed. The fine-gauge stage reduces the compression ratio to mitigate work hardening and lower the probability of wire breakage, thins the coating, and emphasizes uniformity to stabilize the drawing load, while increasing the drawing speed to compensate for efficiency and promote stable lubricant film formation. Through the coordinated convergence of compression ratio, coating thickness, and drawing speed, and with the continuous suppression of friction and heat through dual lubrication of graphite emulsion and vegetable oil, a balance is ultimately achieved between drawing stability, wire quality, and production efficiency.

[0018] This application employs a dual lubrication system of graphite emulsion and vegetable oil, which can improve production efficiency and reduce production costs. The method has high drawing efficiency, good lubrication performance, and low die wear. The tungsten-cerium alloy wires prepared have uniform diameter, excellent surface quality, and good mechanical properties. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0020] Figure 1 This is a SEM image of the ultrafine tungsten-cerium alloy wire prepared in Example 1 of this application; Figure 2 SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 1 of this application; Figure 3This is a SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 2 of this application; Figure 4 SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 3 of this application; Figure 5 This is a SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 4 of this application; Figure 6 This is a SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 5 of this application.

[0021] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0022] The technical solutions in the embodiments will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0023] This application provides a method for preparing ultrafine tungsten-cerium alloy wire, comprising the following steps: S1. Obtain a first tungsten-cerium alloy wire, wherein, by mass percentage, the composition of the first tungsten-cerium alloy wire is: cerium: 1.2%-1.6%, the remainder being tungsten and unavoidable impurities, and the wire diameter of the first tungsten-cerium alloy wire is 50-55μm; The specific method for obtaining the first tungsten-cerium alloy wire is as follows: obtain a tungsten-cerium alloy rod, and perform spin forging and drawing on the tungsten-cerium alloy rod to obtain the first tungsten-cerium alloy wire; S2. The surface of the first tungsten-cerium alloy wire is coated with graphite emulsion to obtain the second tungsten-cerium alloy wire, and the second tungsten-cerium alloy wire is dried to obtain the third tungsten-cerium alloy wire. The graphite emulsion has a specific gravity of 1.010-1.013 and a viscosity of 3.8-4.0 cP; the drying process is carried out in a multi-mold hot drawing heating and drying oven, wherein the length of the multi-mold hot drawing heating and drying oven is 50-60 cm, the speed of the multi-mold hot drawing heating and drying oven is 57-62 m / min, and the heating temperature of the multi-mold hot drawing heating and drying oven is 460-500℃; S3. The third tungsten-cerium alloy wire is immersed in vegetable oil and then drawn; the temperature of the vegetable oil is 50-55℃; the vegetable oil is industrial rapeseed oil or industrial soybean oil. S4. Repeat steps S2 and S3 until an ultrafine tungsten-cerium alloy wire with a diameter ≤28μm is obtained; When the diameter of the tungsten-cerium alloy wire is ≥45μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is ≥1.8μm and ≤2.3μm, the drawing inlet speed is ≥95m / min and ≤135m / min, and the drawing compression ratio is ≥20% and ≤25%. When the diameter of the tungsten-cerium alloy wire is >35μm and <45μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is >1.3μm and <1.8μm, the drawing inlet speed is >135m / min and <235m / min, and the drawing compression rate is >17% and <20%. When the diameter of the tungsten-cerium alloy wire is ≤35μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is ≥0.8μm and ≤1.3μm, the drawing inlet speed is ≥235m / min and ≤420m / min, and the drawing compression rate is ≥15% and ≤17%.

[0024] This application also provides an ultrafine tungsten-cerium alloy wire, comprising: a wire diameter difference ≤0.04μm; a tensile strength ≥6400MPa; a coil diameter ≥120mm; and an average wire breakage frequency ≤7 times per 100,000 kilometers.

[0025] The technical solution of this application will be further described below with reference to specific embodiments.

[0026] Example 1

[0027] A method for preparing ultrafine tungsten-cerium alloy wire, the method comprising the following steps: S1. Obtain a first tungsten-cerium alloy wire, wherein, by mass percentage, the composition of the first tungsten-cerium alloy wire is: cerium: 1.4%, the remainder being tungsten and unavoidable impurities, and the wire diameter of the first tungsten-cerium alloy wire is 53.0 μm; The specific method for obtaining the first tungsten-cerium alloy wire is as follows: obtain a tungsten-cerium alloy rod, and then perform spin forging and drawing on the tungsten-cerium alloy rod to obtain the first tungsten-cerium alloy wire. S2. The surface of the first tungsten-cerium alloy wire is coated with graphite emulsion to obtain the second tungsten-cerium alloy wire, and the second tungsten-cerium alloy wire is dried to obtain the third tungsten-cerium alloy wire. The graphite emulsion has a specific gravity of 1.012 and a viscosity of 3.8 cP. The drying process is carried out in a multi-mold hot drawing heating and drying oven, which has a length of 55 cm, a speed of 57 m / min, and a heating temperature of 460 ℃. S3. The third tungsten-cerium alloy wire is immersed in vegetable oil and then drawn; the temperature of the vegetable oil is 50℃; the vegetable oil is industrial rapeseed oil. S4. Repeat steps S2 and S3 until an ultrafine tungsten-cerium alloy wire with a diameter of 27 μm is obtained; The specific pulling process is as follows: The tungsten-cerium alloy wire has a diameter of 53.0 μm, a graphite emulsion coating thickness of 2.2 μm, a drawing inlet speed of 101.1 m / min, and a drawing compression rate of 23.0%. The tungsten-cerium alloy wire has a diameter of 46.5 μm, a graphite emulsion coating thickness of 2.0 μm, a drawing inlet speed of 131.3 m / min, and a drawing compression rate of 20.0%. The tungsten-cerium alloy wire has a diameter of 41.6 μm, a graphite emulsion coating thickness of 1.6 μm, a drawing inlet speed of 164.1 m / min, and a drawing compression rate of 17.1%. The tungsten-cerium alloy wire has a diameter of 37.9 μm, a graphite emulsion coating thickness of 1.5 μm, a drawing inlet speed of 198.0 m / min, and a drawing compression rate of 17.2%. The tungsten-cerium alloy wire has a diameter of 34.5 μm, a graphite emulsion coating thickness of 1.2 μm, a drawing inlet speed of 239.1 m / min, and a drawing compression rate of 15.1%. The tungsten-cerium alloy wire has a diameter of 31.8 μm, a graphite emulsion coating thickness of 1.0 μm, a drawing inlet speed of 281.6 m / min, and a drawing compression rate of 15.1%. The tungsten-cerium alloy wire has a diameter of 29.3 μm, a graphite emulsion coating thickness of 0.9 μm, a drawing inlet speed of 331.7 m / min, and a drawing compression rate of 15.1%. Please refer to the test results. Figure 1 , Figure 1 The image shows an SEM image of the ultrafine tungsten-cerium alloy wire prepared in Example 1 of this application. The ultrafine tungsten-cerium alloy wire has a smooth surface, shallow drawing marks, and a wire diameter range of 0.03 μm. The tensile strength is 6586 MPa, the coil diameter is 123 mm, and the average number of wire breaks is 5 per 100,000 kilometers.

[0028] Example 2

[0029] A method for preparing ultrafine tungsten-cerium alloy wire, the method comprising the following steps: S1. Obtain a first tungsten-cerium alloy wire, wherein, by mass percentage, the composition of the first tungsten-cerium alloy wire is: cerium: 1.2%, the remainder being tungsten and unavoidable impurities, and the wire diameter of the first tungsten-cerium alloy wire is 55μm; The specific method for obtaining the first tungsten-cerium alloy wire is as follows: obtain a tungsten-cerium alloy rod, and then perform spin forging and drawing on the tungsten-cerium alloy rod to obtain the first tungsten-cerium alloy wire. S2. The surface of the first tungsten-cerium alloy wire is coated with graphite emulsion to obtain the second tungsten-cerium alloy wire, and the second tungsten-cerium alloy wire is dried to obtain the third tungsten-cerium alloy wire. The graphite emulsion has a specific gravity of 1.010 and a viscosity of 4.0 cP. The drying process is carried out in a multi-mold hot drawing heating and drying oven, which has a length of 60 cm, a speed of 60 m / min, and a heating temperature of 480 ℃. S3. The third tungsten-cerium alloy wire is immersed in vegetable oil and then drawn; the temperature of the vegetable oil is 52℃; the vegetable oil is industrial rapeseed oil. S4. Repeat steps S2 and S3 until an ultrafine tungsten-cerium alloy wire with a diameter of 28 μm is obtained; The specific pulling process is as follows: The tungsten-cerium alloy wire has a diameter of 55.0 μm, a graphite emulsion coating thickness of 2.2 μm, a drawing inlet speed of 96.4 m / min, and a drawing compression rate of 20.7%. The tungsten-cerium alloy wire has a diameter of 49.0 μm, a graphite emulsion coating thickness of 2.0 μm, a drawing inlet speed of 121.6 m / min, and a drawing compression rate of 20.0%. The tungsten-cerium alloy wire has a diameter of 43.8 μm, a graphite emulsion coating thickness of 1.6 μm, a drawing inlet speed of 152.0 m / min, and a drawing compression rate of 17.1%. The tungsten-cerium alloy wire has a diameter of 39.9 μm, a graphite emulsion coating thickness of 1.5 μm, a drawing inlet speed of 183.4 m / min, and a drawing compression rate of 17.1%. The tungsten-cerium alloy wire has a diameter of 36.3 μm, a graphite emulsion coating thickness of 1.4 μm, a drawing inlet speed of 221.2 m / min, and a drawing compression rate of 17.1%. The tungsten-cerium alloy wire has a diameter of 33.1 μm, a graphite emulsion coating thickness of 1.2 μm, a drawing inlet speed of 266.8 m / min, and a drawing compression rate of 15.7%. The tungsten-cerium alloy wire has a diameter of 30.4 μm, a graphite emulsion coating thickness of 1.0 μm, a drawing inlet speed of 316.5 m / min, and a drawing compression rate of 15.2%. Testing revealed that the ultrafine tungsten-cerium alloy wire has a smooth surface, shallow drawing marks, and a wire diameter range of 0.04 μm; its tensile strength is 6642 MPa, its coil diameter is 125 mm, and it breaks on average 4 times per 100,000 kilometers.

[0030] Example 3

[0031] A method for preparing ultrafine tungsten-cerium alloy wire, the method comprising the following steps: S1. Obtain a first tungsten-cerium alloy wire, wherein, by mass percentage, the composition of the first tungsten-cerium alloy wire is: cerium: 1.6%, the remainder being tungsten and unavoidable impurities, and the wire diameter of the first tungsten-cerium alloy wire is 50 μm; The specific method for obtaining the first tungsten-cerium alloy wire is as follows: obtain a tungsten-cerium alloy rod, and then perform spin forging and drawing on the tungsten-cerium alloy rod to obtain the first tungsten-cerium alloy wire. S2. The surface of the first tungsten-cerium alloy wire is coated with graphite emulsion to obtain the second tungsten-cerium alloy wire, and the second tungsten-cerium alloy wire is dried to obtain the third tungsten-cerium alloy wire. The graphite emulsion has a specific gravity of 1.013 and a viscosity of 3.9 cP. The drying process is carried out in a multi-mold hot drawing heating and drying oven, which has a length of 55 cm, a speed of 62 m / min, and a heating temperature of 500 ℃. S3. The third tungsten-cerium alloy wire is immersed in vegetable oil and then drawn; the temperature of the vegetable oil is 55℃; the vegetable oil is industrial rapeseed oil. S4. Repeat steps S2 and S3 until an ultrafine tungsten-cerium alloy wire with a diameter of 26 μm is obtained; The specific pulling process is as follows: The tungsten-cerium alloy wire has a diameter of 50.0 μm, a graphite emulsion coating thickness of 2.0 μm, a drawing inlet speed of 110.0 m / min, and a drawing compression rate of 20.0%. The tungsten-cerium alloy wire has a diameter of 44.7 μm, a graphite emulsion coating thickness of 1.7 μm, a drawing inlet speed of 137.5 m / min, and a drawing compression rate of 17.1%. The tungsten-cerium alloy wire has a diameter of 40.7 μm, a graphite emulsion coating thickness of 1.5 μm, a drawing inlet speed of 165.9 m / min, and a drawing compression rate of 17.1%. The tungsten-cerium alloy wire has a diameter of 37.1 μm, a graphite emulsion coating thickness of 1.4 μm, a drawing inlet speed of 200.1 m / min, and a drawing compression rate of 18.5%. The tungsten-cerium alloy wire has a diameter of 33.5 μm, a graphite emulsion coating thickness of 1.2 μm, a drawing inlet speed of 245.5 m / min, and a drawing compression rate of 15.5%. The tungsten-cerium alloy wire has a diameter of 30.8 μm, a graphite emulsion coating thickness of 1.0 μm, a drawing inlet speed of 290.5 m / min, and a drawing compression rate of 15.1%. The tungsten-cerium alloy wire has a diameter of 28.4 μm, a graphite emulsion coating thickness of 0.9 μm, a drawing inlet speed of 342.2 m / min, and a drawing compression rate of 16.2%. Testing revealed that the ultrafine tungsten-cerium alloy wire has a smooth surface, shallow drawing marks, and a wire diameter range of 0.03 μm; its tensile strength is 6486 MPa, its coil diameter is 125 mm, and it breaks on average 7 times per 100,000 kilometers.

[0032] Comparative Example 1 The difference between this comparative example and Example 1 is that the specific gravity of the graphite emulsion is 1.020 and the viscosity of the graphite emulsion is 4.5 cP. All other steps are the same as in Example 1.

[0033] Please refer to the test results. Figure 2 , Figure 2 The image shows an SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 1 of this application. The surface lubrication layer of the ultrafine tungsten-cerium alloy wire has poor lubrication effect, with many and deep drawing marks. The wire diameter range of the ultrafine tungsten-cerium alloy wire is 0.08 μm. The tensile strength is 6283 MPa, the coil diameter is 98 mm, and the average number of wire breaks is 42 times per 100,000 kilometers.

[0034] Comparative Example 2 The difference between this comparative example and Example 1 is that the specific gravity of the graphite emulsion is 1.005 and the viscosity of the graphite emulsion is 3.5 cP. All other steps are the same as in Example 1.

[0035] Please refer to the test results. Figure 3 , Figure 3 The image shows an SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 2 of this application. The surface lubrication layer of the ultrafine tungsten-cerium alloy wire is uneven, with slight cracks and drawing marks. The wire diameter difference is 0.10 μm. The tensile strength is 5979 MPa, the coil diameter is 54 mm, and the average number of wire breaks is 65 times per 100,000 kilometers.

[0036] Comparative Example 3 The difference between this comparative example and Example 1 is that the third tungsten-cerium alloy wire is not immersed in vegetable oil during drawing, i.e., there is no vegetable oil lubrication. All other steps are the same as in Example 1.

[0037] Please refer to the test results. Figure 4, Figure 4 The image shows an SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 3 of this application. The ultrafine tungsten-cerium alloy wire has many and deep drawing marks on its surface, and the wire diameter range is 0.14 μm. The tensile strength is 6041 MPa, the coil diameter is 110 mm, and the average number of wire breaks is 106 per 100,000 kilometers.

[0038] Comparative Example 4 The difference between this comparative example and Example 1 is that the third tungsten-cerium alloy wire was immersed in mineral oil and then drawn; the mineral oil was light mineral oil. All other steps were the same as in Example 1.

[0039] Please refer to the test results. Figure 5 , Figure 5 The image shows an SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 4 of this application. The surface of the ultrafine tungsten-cerium alloy wire has a small number of deep drawing marks, the wire diameter range is 0.09 μm, the tensile strength is 6358 MPa, the coil diameter is 102 mm, and the average number of wire breaks is 56 per 100,000 kilometers.

[0040] Comparative Example 5 The difference between this comparative example and Example 1 is that the thickness of the graphite emulsion coating is 1.5 μm, which remains constant throughout. All other steps are the same as in Example 1.

[0041] Please refer to the test results. Figure 6 , Figure 6 The image shows an SEM image of the ultrafine tungsten-cerium alloy wire prepared in Comparative Example 5 of this application. The graphite emulsion in the surface lubricating layer of the ultrafine tungsten-cerium alloy wire has partially fallen off, and there are obvious drawing marks and slight cracks. The wire diameter range of the ultrafine tungsten-cerium alloy wire is 0.11 μm; the tensile strength is 6166 MPa, the coil diameter is 92 mm, and the average number of wire breaks is 60 times per 100,000 kilometers.

[0042] A comparison of the performance data of the above embodiments and comparative examples shows that: Example 1, in conjunction with Comparative Example 1, shows that when the viscosity of graphite emulsion is too high, the coating is difficult to spread into a uniform and dense lubricating film on the surface of the wire. During the drawing process, the direct contact area between the metal and the die increases, and the frictional heat and drawing stress increase accordingly, which in turn leads to an increase in surface cracks and internal defects in the wire.

[0043] Example 1, combined with Comparative Example 2, shows that when the viscosity of graphite emulsion is low, the coating is not easy to maintain continuity and integrity on the surface of the wire. During the drawing process, dry or semi-dry friction is likely to occur between the die and the wire, which increases the coefficient of friction and the drawing force, leading to an increase in internal defects and a decrease in mechanical properties of the wire.

[0044] Example 1, combined with Comparative Example 3, shows that vegetable oil can play a role in cooling and auxiliary lubrication during the drawing process, which can reduce the drawing temperature, reduce the accumulation of frictional heat, and form a composite lubricating film in synergy with graphite emulsion. Without vegetable oil lubrication, the defects in the graphite emulsion coating are difficult to compensate for, and lubrication failure and frequent wire breakage are likely to occur.

[0045] Example 1, combined with Comparative Example 4, shows that polar molecules such as fatty acids in vegetable oil are more easily adsorbed onto the surface of tungsten-cerium alloy wire and mold, forming a boundary lubrication film, which has a better friction-reducing and wear-resistant effect than mineral oil. At the same time, the viscosity and fluidity of vegetable oil at 50-55℃ are more suitable for the lubrication requirements of drawing ultra-fine tungsten-cerium alloy wire.

[0046] Example 1, in conjunction with Comparative Example 5, shows that as the wire diameter decreases, the ratio of the wire surface area to its volume increases, making the friction and heat generation problems during the drawing process more prominent. Therefore, it is necessary to optimize the thickness of the graphite emulsion coating according to the wire diameter. If the coating is too thick or too thin, it will disrupt the balance between the lubricating film and the drawing stress, resulting in a decrease in mechanical properties and surface quality.

[0047] The above description is only a preferred embodiment of this application and does not limit the patent scope of this application. All equivalent structural transformations made using the content of this application's specification under the inventive concept of this application, or direct / indirect applications in other related technical fields, are included within the patent protection scope of this application.

Claims

1. A method for preparing ultrafine tungsten-cerium alloy wire, characterized in that, Includes the following steps: S1. Obtain a first tungsten-cerium alloy wire, wherein, by mass percentage, the composition of the first tungsten-cerium alloy wire is: cerium: 1.2%-1.6%, the remainder being tungsten and unavoidable impurities, and the wire diameter of the first tungsten-cerium alloy wire is 50-55μm; S2. The surface of the first tungsten-cerium alloy wire is coated with graphite emulsion to obtain the second tungsten-cerium alloy wire, and the second tungsten-cerium alloy wire is dried to obtain the third tungsten-cerium alloy wire. S3. Immerse the third tungsten-cerium alloy wire in vegetable oil and then draw it. S4. Repeat steps S2 and S3 until an ultrafine tungsten-cerium alloy wire with a diameter ≤28μm is obtained.

2. The method for preparing an ultrafine tungsten-cerium alloy wire according to claim 1, characterized in that, In step S1, the method of obtaining the first tungsten-cerium alloy wire is as follows: obtain a tungsten-cerium alloy rod, and perform spin forging and drawing on the tungsten-cerium alloy rod to obtain the first tungsten-cerium alloy wire.

3. The method for preparing an ultrafine tungsten-cerium alloy wire according to claim 1, characterized in that, In step S2, the specific gravity of the graphite emulsion is 1.010-1.013, and the viscosity of the graphite emulsion is 3.8-4.0 cP. The drying process is carried out in a multi-mold hot drawing heating and drying oven, wherein the length of the multi-mold hot drawing heating and drying oven is 50-60 cm, the speed of the multi-mold hot drawing heating and drying oven is 57-62 m / min, and the heating temperature of the multi-mold hot drawing heating and drying oven is 460-500℃.

4. The method for preparing an ultrafine tungsten-cerium alloy wire according to claim 1, characterized in that, In step S3, the temperature of the vegetable oil is 50-55℃.

5. The method for preparing an ultrafine tungsten-cerium alloy wire according to claim 1, characterized in that, When the diameter of the tungsten-cerium alloy wire is ≥45μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is ≥1.8μm and ≤2.3μm, the drawing inlet speed is ≥95m / min and ≤135m / min, and the drawing compression rate is ≥20% and ≤25%.

6. The method for preparing an ultrafine tungsten-cerium alloy wire according to claim 1, characterized in that, When the diameter of the tungsten-cerium alloy wire is greater than 35 μm and less than 45 μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is greater than 1.3 μm and less than 1.8 μm, the drawing inlet speed is greater than 135 m / min and less than 235 m / min, and the drawing compression rate is greater than 17% and less than 20%.

7. The method for preparing an ultrafine tungsten-cerium alloy wire according to claim 1, characterized in that, When the diameter of the tungsten-cerium alloy wire is ≤35μm, the thickness of the graphite emulsion coating on the surface of the tungsten-cerium alloy wire is ≥0.8μm and ≤1.3μm, the drawing inlet speed is ≥235m / min and ≤420m / min, and the drawing compression rate is ≥15% and ≤17%.

8. An ultrafine tungsten-cerium alloy wire, characterized in that, It is prepared by the method described in any one of claims 1-7 for the preparation of an ultrafine tungsten-cerium alloy wire.

9. The ultrafine tungsten-cerium alloy wire according to claim 8, characterized in that, The diameter difference of the ultrafine tungsten-cerium alloy wire is ≤0.04μm.

10. The ultrafine tungsten-cerium alloy wire according to claim 8, characterized in that, The ultrafine tungsten-cerium alloy wire has a tensile strength ≥6400MPa, a coil diameter ≥120mm, and an average of ≤7 wire breaks per 100,000 kilometers.