Production apparatus for aluminum-aluminum composite pipe for heat exchange and production method thereof

By combining a semi-molten hot extrusion composite process with synchronous internal thread forming, the problems of low interfacial bonding strength and poor forming accuracy in the production of aluminum-aluminum composite pipes have been solved, achieving efficient and stable production of aluminum-aluminum composite pipes suitable for heat exchangers in air conditioning, refrigeration, petrochemical and other fields.

CN123149276APending Publication Date: 2026-11-24JIANGSU RUIBANG COMPOSITE MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611387063.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The current aluminum-aluminum composite pipe production process suffers from low interfacial bonding strength, and the separate processing of internal threads and composite processes leads to low production efficiency and poor thread forming accuracy for long-length pipes, making it difficult to meet the accuracy requirements of large-scale continuous production.

Method used

The semi-molten hot extrusion composite process is adopted. By simultaneously forming internal threads during hot extrusion composite, the atomic diffusion of aluminum-aluminum homogeneous materials is used to form a metallurgical bonding interface. Combined with the internal thread forming module and the configuration of a circumferential anti-rotation positioning structure, the continuous production of aluminum-aluminum composite pipes is realized.

Benefits of technology

It improves the bonding strength of the interface, enhances the forming accuracy of the internal thread and the consistency of the long dimension, reduces the production cost and the weight of the device, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149276A_ABST
    Figure CN123149276A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of metal material processing technology and discloses a production equipment and method for aluminum-aluminum composite tubes used for heat exchange. The method uses an inner layer of 6-series solid aluminum alloy tube as the substrate, and an outer layer of 4-series semi-molten aluminum alloy is hot-extruded onto the outer wall of the inner tube to form an aluminum-aluminum metallurgical interface. Simultaneously, an internal thread is processed through an internal thread extrusion module integrated into the mold. By controlling the preheating temperature of the inner layer to 400-500℃, the semi-molten temperature of the outer layer to be 5-15℃ higher than its solidus, and the temperature of the outer layer to be 80-120℃ higher than the inner layer, along with a circumferential anti-rotation structure of the module, the composite quality and thread forming accuracy are ensured. The composite tube prepared by this invention has both good corrosion resistance and heat exchange efficiency. Compared with pure copper tubes, it is lighter, lower in cost, and has a high degree of continuous production, making it suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal material processing technology, specifically relating to a production equipment and method for aluminum-aluminum composite pipes used for heat exchange. Background Technology

[0002] Heat exchangers are core equipment in air conditioning and refrigeration, petrochemical, and energy industries. Heat transfer tubes, as the core component carrying the working medium, directly determine the heat exchanger's heat exchange efficiency, service life, and manufacturing cost. Internally threaded tubes, through their internal thread structure, increase the heat exchange area and enhance medium turbulence, resulting in significantly higher heat exchange efficiency than smooth tubes. They are widely used in equipment such as evaporators, condensers, and oil coolers.

[0003] Currently, heat transfer tubes are mostly made of pure copper or copper-aluminum composite materials. Pure copper tubes have excellent thermal conductivity and formability, but their density is about 8.9 g / cm³, resulting in a large overall weight. Furthermore, copper resources are expensive and their prices fluctuate greatly. Additionally, pure copper tubes have insufficient corrosion resistance under alkaline conditions and are prone to corrosion perforation. Copper-aluminum composite tubes reduce cost and weight by coating the outer wall of the copper tube with an aluminum layer. However, the copper-aluminum interface is mostly mechanically bonded, with a bonding strength typically only 20-30 MPa, making them prone to delamination under long-term thermal cycling or vibration. Moreover, the large potential difference between copper and aluminum makes them susceptible to electrochemical corrosion in humid, alkaline environments, accelerating the failure of the inner copper layer.

[0004] Current aluminum tube production primarily employs cold-working processes such as drawing and rolling to create internal threads, followed by a coating process to form a composite layer. These steps are carried out in stages, resulting in an overall production speed of only around 2 m / min, leading to low efficiency and difficulty in guaranteeing interface bonding quality. Existing hot extrusion composite processes are mostly designed for dissimilar metals such as copper-aluminum and steel-aluminum. A mature industrialized solution for continuous production of homogeneous aluminum-aluminum composites with simultaneous internal thread forming has not yet been developed, making it difficult to simultaneously achieve high-quality interface metallurgical bonding and precise internal thread forming. Furthermore, the built-in thread die in the simultaneous forming process is susceptible to circumferential movement due to axial friction of the tube, resulting in poor thread profile consistency in long tubes and a yield rate typically below 90%, failing to meet the precision requirements of large-scale continuous production. Summary of the Invention

[0005] This invention addresses the shortcomings of existing technologies by solving the problems of low interfacial bonding strength, low production efficiency due to the separate processing of internal threads and the composite process, and poor thread forming accuracy of long-length pipes in the production of aluminum-aluminum composite pipes. It provides a production equipment and method for aluminum-aluminum composite pipes used for heat exchange, realizing continuous production of aluminum-aluminum composite pipes. The internal threads are formed simultaneously during hot extrusion composite, ensuring the metallurgical bonding strength of the interface, improving the forming accuracy of the internal threads and the consistency of the long dimensions, while also improving the corrosion resistance and heat exchange efficiency of the pipe, and reducing production costs and device weight.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a method for producing an aluminum-aluminum composite tube for heat exchange. Using an inner solid tubular aluminum alloy tube as the base, an outer semi-molten aluminum alloy layer is hot-extruded and bonded to the outer wall of the inner solid tubular aluminum alloy tube to form an aluminum-aluminum composite tube. Internal threads are simultaneously machined during the bonding process. The inner layer uses a 6-series wrought aluminum alloy with a preheating temperature of 400-500°C; the outer layer uses a 4-series cast aluminum alloy with its semi-molten state temperature controlled within a range 5-15°C above its solidus temperature, and the temperature of the outer semi-molten aluminum alloy is 80-120°C higher than the preheating temperature of the inner layer.

[0007] When the inner layer preheating temperature is below 400℃, the pipe lacks plasticity, and tooth tip cracking is prone to occur during thread forming; when it is above 500℃, the inner tube strength decreases excessively, and radial instability deformation is prone to occur during extrusion. When the temperature difference between the inner and outer layers is below 80℃, the driving force for atomic diffusion at the interface is insufficient, making it difficult to form a continuous metallurgical bonding layer; when it is above 120℃, local melting damage is prone to occur on the outer wall of the inner tube, affecting the dimensional accuracy of the pipe.

[0008] The production method includes the following steps: S1 Inner Aluminum Tube Unwinding and Feeding: 6-series aluminum alloy tubes in coil form are used as the inner tube material and are continuously fed into the production line through an unwinding device and a feeding device. S2 Inner tube surface pretreatment: sequentially soaked in hot alkaline solution, rinsed with clean water, mechanically ground or polished, neutralized with acid solution, cleaned and dried to remove the original oxide film on the outer wall of the inner tube and activate the surface to prevent secondary oxidation; S3 Preheating treatment: The preheated inner tube is heated to 400~500℃ using an induction heating device or a resistance preheating furnace; S4 outer layer aluminum melt melting and heat preservation: After the 4 series aluminum alloy is melted in the melting furnace, it is introduced into the heat preservation intermediate ladle, and the temperature is controlled in the semi-molten range of 5~15℃ above its solidus line; S5 Hot Extrusion Composite and Synchronous Internal Thread Forming: The outer semi-molten aluminum alloy is wrapped around the outer wall of the inner tube under pressure of 100~800MPa through an annular extrusion die, forming an aluminum-aluminum metallurgical interface through atomic diffusion; at the same time, the internal thread extrusion module integrated in the extrusion die cooperates with the hot inner wall of the inner tube to synchronously extrude and form a continuous internal thread; during the extrusion process, the circumferential rotation of the internal thread extrusion module is restricted by a circumferential anti-rotation positioning structure; S6 Cooling and Shaping: The composite pipe is rapidly cooled and shaped using a combination of water cooling and air cooling. S7 Traction and Rewinding Cutting: The composite pipe is smoothly led out by the traction device and wound into rolls or cut to length as needed.

[0009] When the extrusion pressure is below 100 MPa, the aluminum liquid does not adhere sufficiently to the surface of the inner tube, resulting in a decrease in interfacial bonding strength. When the pressure is above 800 MPa, the deformation of the inner tube is too large, making it difficult to control the thread dimensional accuracy. The production line traction speed is 5~20 m / min. When the traction speed is above 20 m / min, the interfacial atomic diffusion time is insufficient, and the bonding strength is significantly reduced. When the speed is below 5 m / min, the production efficiency is too low, and it does not have industrial value.

[0010] On the other hand, the present invention provides a production equipment for aluminum-aluminum composite tubes for heat exchange, wherein each unit is arranged in sequence along the horizontal direction to form a horizontal continuous production line, including an inner tube unwinding and feeding unit, a surface pretreatment unit, a preheating unit, an outer layer aluminum liquid supply unit, a hot extrusion composite unit, a cooling and shaping unit, a traction unit, a winding and cutting unit, and a control system.

[0011] The system comprises several components: an inner tube unwinding and feeding unit for releasing and conveying the inner aluminum alloy tube in coil form; a surface pretreatment unit consisting of a hot alkaline immersion tank, a clean water rinsing tank, a mechanical grinding device, an acid neutralization tank, and a cleaning and drying device, used to remove and activate the oxide film on the inner tube surface; a preheating unit using induction heating or resistance preheating to heat the inner tube to a preset process temperature; an outer aluminum liquid supply unit including a melting furnace and an insulated tundish for preparing and storing a semi-molten outer aluminum alloy; a hot extrusion composite unit including an annular extrusion die and an integrated internal thread forming module, simultaneously completing the outer layer coating and internal thread forming; an internal thread forming module equipped with a circumferential anti-rotation positioning structure to prevent circumferential movement of the module during continuous production; a cooling and shaping unit using a two-stage cooling structure of water cooling and air cooling; a traction unit providing continuous conveying power for the composite tube; a winding and cutting unit that can switch between winding and fixed-length cutting modes; and a control system that coordinates and regulates the preheating temperature, aluminum liquid temperature, extrusion pressure, and traction speed to ensure matching of parameters for each process.

[0012] Furthermore, the inner aluminum alloy is a wrought aluminum alloy of 6063 or 6061, and the outer aluminum alloy is a cast aluminum alloy of 4045 or 4047; the semi-molten temperature of the outer aluminum alloy is controlled at 575~585℃.

[0013] Further, the surface pretreatment in step S2 is as follows: the hot alkaline solution uses a sodium hydroxide or sodium carbonate solution with a mass concentration of 5%~15%, the temperature is 60~90℃, and the immersion time is 3~10s; the water rinsing pressure is 0.3~0.5MPa, and the rinsing time is 2~5s; the mechanical grinding roller speed is 1000~3000r / min, and the polishing wheel speed is 500~1500r / min; the acid solution uses a dilute phosphoric acid or dilute acetic acid with a mass concentration of 1%~5%, and the neutralization time is 2~5s; the drying hot air temperature is 80~120℃, and the drying time is 3~8s.

[0014] Furthermore, the extrusion process requires no additional protective atmosphere, and a dense alumina protective film naturally forms on the surface of the outer aluminum alloy. The formed internal thread profile is triangular or trapezoidal, with a pitch of 0.5~2.0mm and a tooth depth of 0.1~0.5mm.

[0015] Furthermore, the cooling and shaping process first involves annular spray water cooling at 15~30℃ and 0.2~0.4MPa, followed by air cooling at a wind speed of 10~20m / s, which reduces the surface temperature of the composite pipe to below 100℃.

[0016] Furthermore, the traction force of the traction device is 100~2000N; the diameter of the finished coil is 500~800mm, and the weight of a single coil is 50~200kg; the fixed-length cutting adopts a flying saw structure with a cutting accuracy of ±1mm.

[0017] Furthermore, the annular extrusion die includes an outer die sleeve, an inner die core, and a die base, with an annular forming cavity formed between the outer die sleeve and the inner die core; a heating structure is installed on the outside of the die, maintaining the working temperature at 200~350℃. The internal thread forming module is installed on the end of the inner die core through a detachable fixing mechanism, and is circumferentially fixed in conjunction with a circumferential anti-rotation positioning structure, allowing for the replacement of dies with different thread parameters according to product requirements.

[0018] This invention employs a semi-molten hot extrusion composite process, utilizing atomic diffusion of homogeneous aluminum materials to form a metallurgical bonding interface. The bonding strength is far superior to conventional mechanical coating processes, making the pipe less prone to delamination under long-term thermal cycling and vibration conditions. The outer layer uses a 4-series aluminum alloy with a lower potential, which can act as a sacrificial anode to protect the inner 6-series aluminum alloy in humid, oxygen-alkaline environments. Combined with the naturally formed alumina film on the outer surface, this significantly improves the overall corrosion resistance life of the pipe.

[0019] This invention integrates an internal thread forming module inside a hot extrusion die, enabling simultaneous internal thread processing during composite operations without the need for subsequent cold working. Utilizing the hot plasticity of the tube for thread extrusion forming avoids damage to the composite interface caused by secondary processing. The internal thread forming module is equipped with a circumferential anti-rotation positioning structure, which counteracts the circumferential force generated by the axial friction of the tube during continuous production, preventing circumferential movement of the module, ensuring the consistency and coaxiality of the thread profile in long tubes, and improving product yield. The internal thread structure increases the heat exchange area inside the tube, enhances the turbulence effect of the medium, and improves the heat transfer coefficient.

[0020] The all-aluminum composite tube prepared by this invention has a significantly reduced weight and lower material cost compared to pure copper tubes, and boasts a high recyclability rate, meeting the requirements of lightweight and green manufacturing. The production line adopts a horizontal continuous layout, with continuous operation throughout the entire process of unwinding, pretreatment, lamination, forming, cooling, and rewinding, resulting in a high degree of process integration. Through precise matching and linkage control of the inner and outer layer temperatures, it can be ensured that the outer layer fully wets the surface of the inner tube while the inner tube remains solid and does not melt, exhibiting good process stability and suitability for large-scale industrial production. Attached Figure Description

[0021] Figure 1 This is a schematic diagram of the functional module layout of the continuous production line for aluminum-aluminum composite pipes of the present invention. Figure 2 A cross-sectional schematic diagram of the structure for hot extrusion composite and synchronous internal thread forming; Figure 3 This is a schematic diagram of the cross-sectional structure of an aluminum-aluminum composite pipe. In the diagram: 1-Inner tube unwinding and feeding unit; 2-Surface pretreatment unit; 3-Preheating unit; 4-Outer aluminum liquid supply unit; 5-Hot extrusion composite unit; 6-Cooling and shaping unit; 7-Traction unit; 8-Rewinding and cutting unit; 9-Control system; 10-Inner aluminum alloy tube; 11-Outer aluminum alloy layer; 12-Internal thread; 51-Outer mold sleeve; 52-Inner mold core; 53-Annular forming cavity; 54-Semi-molten aluminum liquid; 55-Internal thread forming module; 56-Circumferential anti-rotation positioning structure; 57-Locking pressure cap. Detailed Implementation

[0022] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention.

[0023] Example 1 This embodiment provides a production equipment and method for aluminum-aluminum composite tubes used for heat exchange, which prepares an internally threaded composite tube with an inner layer of 6063 aluminum alloy and an outer layer of 4045 aluminum alloy. The product is used in air conditioner evaporators.

[0024] As shown in Figure 1, the production equipment adopts a horizontal continuous layout. Along the pipe conveying direction, the following units are arranged in sequence: inner tube unwinding and feeding unit 1, surface pretreatment unit 2, preheating unit 3, outer aluminum liquid supply unit 4, hot extrusion composite unit 5, cooling and shaping unit 6, traction unit 7, and winding and cutting unit 8. Each unit is connected by conveyor rollers and is equipped with a control system 9 to realize the linkage control of parameters throughout the entire process.

[0025] The inner tube unwinding and feeding unit 1 includes an unwinding bracket, an air-expansion shaft winding device, a tension control mechanism, and a guide roller assembly. The unwinding bracket carries the inner aluminum tube in the form of a coil. After the air-expansion shaft is inflated, it secures the coil. The tension control mechanism achieves constant tension unwinding through a tension sensor and a servo motor, with tension fluctuations controlled within ±5N. The guide roller assembly is made of polished stainless steel to guide the aluminum tube smoothly into subsequent processes, and is equipped with an anti-deviation and correction mechanism.

[0026] Surface pretreatment unit 2 consists of five stations arranged sequentially along the conveying direction: a hot alkaline immersion tank (stainless steel welded structure, with built-in heating pipes and temperature sensors, containing a 10% sodium hydroxide solution, maintaining a working temperature of 75℃); a clean water rinsing tank equipped with a high-pressure spray device and a water circulation filtration system, with a spray water pressure of 0.4MPa; a mechanical polishing device with three sets of rotating polishing rollers and two sets of wool polishing wheels, the polishing rollers rotating at 2000r / min and the polishing wheels at 1000r / min, and equipped with a dust collection system; an acid neutralization tank containing a 3% dilute phosphoric acid solution; and a cleaning and drying device divided into a clean water rinsing section and a hot air drying section, with a hot air temperature of 100℃. Splash-proof partitions and waste liquid collection tanks are installed between each station.

[0027] Preheating unit 3 adopts a high-frequency induction heating device, which consists of a high-frequency induction coil and a power frequency converter. The coil is arranged around the pipe, and the frequency converter operates at a frequency of 20kHz. It is equipped with an infrared thermometer to monitor the surface temperature of the pipe in real time, with a temperature measurement accuracy of ±5℃.

[0028] The outer aluminum melt supply unit 4 includes a crucible-type electromagnetic induction melting furnace and a heat-insulating tundish. The melting furnace crucible is made of graphite and has a rated melting temperature of 650℃. The heat-insulating tundish has a built-in heating and temperature control system, an electromagnetic stirring device, and a float-type level gauge. A flow regulating valve is installed at the outlet to precisely control the aluminum melt supply flow. The electromagnetic stirring device is set to a stirring frequency of 15Hz and uses an intermittent stirring mode, stirring for 1 minute every 10 minutes to ensure uniform aluminum melt temperature and solid fraction. In the semi-molten state, precise temperature control is primarily achieved through thermocouples, supplemented by sampling and testing of the solid fraction every shift to ensure the solid fraction remains stable within the 30%~40% range.

[0029] like Figure 2 As shown, the hot extrusion composite unit 5 is the core station of the production line, including a frame, a hydraulic extrusion main cylinder, an annular extrusion die, and an internal thread forming module 55. The frame is a welded steel plate frame structure, and the maximum pushing force of the extrusion main cylinder is 2000kN. The annular extrusion die includes an outer die sleeve 51, an inner die core 52, and a die seat. An annular forming cavity 53 is formed between the outer die sleeve 51 and the inner die core 52. The aluminum liquid flow channel of the heat-insulating tundish is connected to the cavity inlet. The die is surrounded by a resistance heating coil, and the die working temperature is maintained at 300℃.

[0030] The internal thread forming module 55 is installed at the discharge end of the inner mold core 52. The two are assembled using a shaft-hole clearance fit. The circumferential anti-rotation positioning structure 56 adopts a flat key structure. The specific assembly relationship is as follows: The center of the discharge end of the inner mold core 52 has an axially extending circular mounting hole, and a rectangular keyway is formed along the axial direction on the inner wall of the mounting hole; the left end of the internal thread forming module 55 is provided with a coaxial mounting shaft section, and a rectangular keyway of matching size is formed at the corresponding position on the outer wall of the mounting shaft section; the flat key is simultaneously embedded in the keyways of both the inner mold core 52 and the internal thread forming module 55, and its two sides are respectively in contact with the sidewalls of the keyways to restrict the relative circumferential rotation of the two. The right end of the internal thread forming module 55 is provided with an annular locking cover 57, which is connected to the end face of the inner mold core 52 by fixing screws, pressing the shoulder of the internal thread forming module 55 to achieve axial fixation and prevent axial movement caused by friction of the tube; this detachable structure allows for quick replacement of internal thread forming modules with different tooth profiles and pitches according to the product thread parameter requirements.

[0031] During the production process, when the inner aluminum alloy tube 10 is fed axially, its hot inner wall is in close contact with the helical tooth profile of the outer wall of the internal thread forming module 55. The relative friction will generate a circumferential torque acting on the internal thread forming module 55. This circumferential torque is transmitted to the flat key through the keyway sidewall, and then to the inner mold core 52 through the flat key. Since the inner mold core 52 is fixedly installed on the mold base and has no circumferential rotational freedom, it can completely offset the circumferential force, avoid circumferential displacement of the internal thread forming module 55, ensure the circumferential consistency of the tooth profile of the internal thread 12 during long-size continuous production, eliminate defects such as thread misalignment and disordered teeth, and improve the thread forming accuracy and product yield.

[0032] The internal thread is formed by extrusion using a fixed spiral mandrel. When the tube is fed axially, the inner wall rotates circumferentially along the spiral tooth profile of the module. The clamping structure of the traction device does not restrict the circumferential rotational freedom of the tube, but only provides axial traction force. The traction speed matches the thread lead, ensuring that the axial feed per unit time corresponds to the thread lead and avoiding thread misalignment.

[0033] The cooling and shaping unit 6 is equipped with a ring-shaped spray water cooling section and an axial flow air cooling section. The water cooling section has a water temperature of 25℃ and a spray water pressure of 0.3MPa, and the spray range covers the entire circumference of the pipe. The air cooling section is equipped with a high-pressure fan with a wind speed of 15m / s. An infrared thermometer is installed at the outlet to monitor the temperature of the pipe after cooling.

[0034] The traction unit 7 adopts a tracked traction device. The traction track is made of polyurethane material with anti-slip teeth on the surface. The traction force adjustment range is 200~1000N, and the traction speed can be steplessly adjusted.

[0035] The winding and cutting unit 8 integrates an automatic winding device and a flying saw for fixed-length cutting, and the working mode can be switched through the control system. The maximum roll diameter of the winding device is 700mm, and the maximum weight of a single roll is 150kg; the flying saw has a cutting accuracy of ±1mm, and the cutting speed is synchronized with the production line speed.

[0036] The control system 9 employs a programmable logic controller (PLC) that connects to the sensors and actuators of each unit to achieve closed-loop control of temperature, pressure, speed, and tension. The preheating unit 3 is linked to the outer aluminum liquid supply unit 4 for temperature control, monitoring the temperature difference between the inner and outer layers in real time. When the temperature difference deviates from the set range of 80~120℃, the heating power of the insulation tundish is adjusted first, supplemented by fine-tuning the output power of the induction heating device, to quickly bring the temperature difference back to the set range. When the traction speed is adjusted, the control system synchronously adjusts the opening of the aluminum liquid outlet gate valve and the pressure of the extrusion main cylinder to ensure stable coating thickness and interface bonding strength.

[0037] Based on the above equipment, combined with Figure 1 The production method described in this embodiment, as shown in the process flow diagram, has the following specific steps: Step 1: Unwinding and feeding of the inner aluminum tube. The 6063 aluminum alloy seamless tube in coil form is mounted on the air shaft of the unwinding bracket. After inflation and tightening, the tension control mechanism is activated, and the unwinding tension is set to 100N. After being corrected by the guide roller group, the aluminum tube is continuously fed into the surface pretreatment unit at a linear speed of 8m / min. In this embodiment, the initial outer diameter of the inner aluminum tube is 10mm, and the wall thickness is 1.0mm.

[0038] Step 2, Inner Tube Surface Pretreatment. The aluminum tube is processed sequentially through the following five stations: Hot alkaline solution immersion: Immerse in a 75℃, 10% sodium hydroxide solution for 5 seconds to dissolve the original alumina film on the surface; Rinse with clean water: Rinse with 0.4MPa high-pressure water spray for 3 seconds to thoroughly remove alkaline residue; Mechanical grinding and polishing: Grinding rollers and polishing wheels contact the outer wall of the aluminum tube in sequence to remove the residual oxide layer and obtain an activated and fresh metal surface; Acid neutralization: Immerse in a 3% dilute phosphoric acid solution for 3 seconds to neutralize any residual alkaline substances on the surface; Cleaning and drying: After rinsing with clean water, dry with hot air at 100℃ for 5 seconds to remove surface moisture and prevent secondary oxidation.

[0039] Step 3, Preheating. The dried aluminum tube enters the induction heating coil, where high-frequency induction heating raises the temperature to 450°C. An infrared thermometer provides real-time temperature feedback, and the control system adjusts the heating power to maintain a stable temperature. The preheated aluminum tube is then quickly fed into the extrusion station via a transition roller conveyor to minimize temperature drop.

[0040] Step 4: Melting and holding the outer layer of molten aluminum. The 4045 aluminum alloy ingot is placed in the melting furnace and heated to 620℃ until completely melted. The molten aluminum is then poured into a holding tundish via a flow channel. The temperature control system stabilizes the temperature of the molten aluminum at 580℃. At this point, the molten aluminum is in a semi-molten state 5-10℃ above the solidus, possessing both fluidity and appropriate viscosity. The solidus temperature of 4045 aluminum alloy is approximately 577℃, and the liquidus temperature is approximately 590℃. Within this temperature range, the solid fraction of the molten aluminum is approximately 30%-40%, resulting in optimal wettability.

[0041] Step 5, hot extrusion composite and synchronous internal thread forming. The preheated inner tube enters the inner core 52 channel of the annular extrusion die at a speed of 8 m / min; at the same time, the flow gate valve of the heat preservation tundish is opened, and the semi-molten aluminum liquid 54 at 580℃ enters the annular forming cavity 53. The extrusion main cylinder applies an extrusion force of 300MPa, pushing the aluminum liquid to uniformly cover the outer wall of the inner tube.

[0042] Under high temperature and pressure, atomic interdiffusion occurs at the interface between the semi-molten outer aluminum alloy and the solid inner aluminum alloy, forming a metallurgical bonding layer with a thickness of about 5~10μm and high interfacial bonding strength. No protective atmosphere is required during extrusion; a dense alumina film naturally forms on the surface of the outer aluminum melt at high temperature, preventing further oxidation of the inner aluminum melt.

[0043] Meanwhile, the inner wall of the inner tube is tightly fitted with the internal thread forming module 55 fixed at the end of the inner mold core 52. The 6063 aluminum alloy, in its hot state, exhibits good plasticity. Under the combined action of axial thrust and radial constraint force of the mold, the inner wall is simultaneously extruded with continuous triangular internal threads 12. The flat key anti-rotation structure can counteract the circumferential friction force generated by the axial movement of the inner tube on the module, preventing circumferential displacement of the module and ensuring the consistency and coaxiality of the thread profile of the entire roll of pipe. In this embodiment, the outer layer coating thickness is 0.5 mm, and the total wall thickness of the finished composite pipe is 1.5 mm.

[0044] Step 6, Cooling and Shaping. After leaving the extrusion die, the composite pipe enters the cooling and shaping unit 6. It is first rapidly cooled by annular spray water cooling, and then further cooled by air cooling to remove residual heat. The pipe outlet temperature is controlled below 80℃. Rapid cooling can fix the metallurgical bonding interface structure and the shape of the internal thread, avoiding excessive grain growth at high temperatures.

[0045] Step 7, Traction and Rewinding Cutting. The cooled composite pipe is clamped and pulled out by a tracked traction device, with the traction speed and extrusion speed maintained synchronously at 8m / min. When switching to rewinding mode according to production needs, the composite pipe is guided and wound into a roll. When the roll diameter reaches 600mm, it is automatically cut and the roll is changed. When switching to fixed length mode, the flying saw cuts the pipe to the set length, and the cut pipe falls into the collection device.

[0046] The final aluminum-aluminum composite pipe is composed of an inner aluminum alloy pipe 10 and an outer aluminum alloy layer 11, with continuous internal threads 12 formed on the inner wall.

[0047] The composite tube prepared in this embodiment was subjected to performance testing, and the results are as follows: Interface bonding performance: The interfacial shear strength was tested by tensile method, with an average value of about 75 MPa, which is much higher than the 20~30 MPa of conventional mechanical coating. There was no delamination at the interface. After 200 cycles of thermal cycling test from -20℃ to 120℃, the interface bonding strength retention rate reached about 92%, with no cracking or delamination.

[0048] Internal thread forming accuracy: The thread depth deviation of a 1000m roll of pipe is controlled within ±0.02mm, the circumferential misalignment rate of the tooth profile is less than 0.5%, and the yield rate reaches 98%, which is far higher than the production scheme without anti-rotation structure.

[0049] Corrosion resistance: After 1000 hours of continuous spraying using a neutral salt spray test (GB / T 10125), only slight corrosion was observed on the surface of the pipe, and no corrosion perforation was found in the inner layer. Under the same test conditions, the corrosion depth of the pure 6063 aluminum pipe was approximately 3.2 times that of the composite pipe, which verified the sacrificial anode protection effect of the outer 4-series aluminum alloy.

[0050] Heat transfer performance: Under the same flow rate conditions, the heat transfer coefficient of the internally threaded composite tube in this embodiment is about 85% higher than that of the smooth pure aluminum tube, and the heat transfer coefficient is comparable to that of the pure copper internally threaded tube, while the weight is reduced by about 63%.

[0051] Example 2 The difference between this embodiment and Embodiment 1 lies in the material system and process parameters. A thick-walled composite tube with an inner layer of 6061 aluminum alloy and an outer layer of 4047 aluminum alloy is prepared and applied to an oil cooler.

[0052] In this embodiment, the inner 6061 aluminum alloy tube has an initial outer diameter of 16mm and a wall thickness of 1.5mm; the preheating temperature is set to 480℃. The outer 4047 aluminum alloy has a solidus temperature of approximately 573℃ and a liquidus temperature of approximately 595℃, and the temperature of the insulation tundish is controlled at 582℃, placing it in a semi-molten state. The extrusion pressure is set to 500MPa, and the production line traction speed is 5m / min. The internal thread adopts a trapezoidal tooth profile with a pitch of 1.5mm and a tooth depth of 0.3mm; the internal thread forming module uses a positioning pin structure to achieve circumferential anti-rotation, with the positioning pin radially embedded between the module mounting shaft and the mating surface of the inner mold core.

[0053] The composite pipe prepared in this embodiment has an average interfacial shear strength of about 82 MPa and a pressure bearing capacity of up to 12 MPa, which meets the high-pressure operating requirements of the oil cooler. After 800 hours of alkaline salt spray test, there is no corrosion damage to the inner layer, and the corrosion resistance is excellent. The thread profile of the long pipe is consistent, and the yield is about 97.8%.

[0054] Comparative Example This comparative example uses a step-by-step process to prepare aluminum-aluminum composite internally threaded tubes of the same specifications: first, internal threads are processed on the inner wall of 6063 aluminum tubes using a drawing process, and then a 4045 aluminum alloy layer is coated on the outer wall of the tubes using a hot-dip galvanizing process.

[0055] Test results showed that the average interfacial shear strength of the comparative example was approximately 28 MPa, only about 37% of that of Example 1; local delamination occurred at the interface after 100 thermal cycles. In terms of production efficiency, the total production speed of the step-by-step process was approximately 2 m / min, only about 25% of that of Example 1. Regarding internal thread accuracy, after hot-dip galvanizing at high temperatures, the thread profile accuracy decreased by approximately 15%, with a total pipe tooth depth deviation of ±0.06 mm, resulting in significant fluctuations in heat exchange performance.

[0056] As can be seen from the above embodiments and comparative examples, the present invention, through the combination of semi-molten hot extrusion composite and synchronous internal thread forming process, combined with precise matching of inner and outer layer temperatures and circumferential anti-rotation design of internal thread module, can simultaneously achieve a metallurgical interface with high bonding strength, high-precision internal thread forming and high yield. The production efficiency and product performance are significantly better than the step-by-step process.

[0057] The above description is only a preferred embodiment of the present invention and does not limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the technical concept of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for producing an aluminum-aluminum composite pipe for heat exchange, characterized in that, Using an inner solid tubular aluminum alloy tube as the base, an outer semi-molten aluminum alloy is hot-extruded and composited onto the outer wall of the inner solid tubular aluminum alloy tube to form an aluminum-aluminum composite tube, and internal threads are processed simultaneously during the composite process; The inner aluminum alloy is a 6-series wrought aluminum alloy with a preheating temperature of 400-500℃; the outer aluminum alloy is a 4-series cast aluminum alloy with its semi-molten state temperature controlled within a range of 5-15℃ higher than its solidus temperature, and the temperature of the outer semi-molten aluminum alloy is 80-120℃ higher than the preheating temperature of the inner layer. Includes the following steps: S1: Inner aluminum tube unwinding and feeding. Solid aluminum alloy tubes in coil form are used as inner tubes. The aluminum tubes are continuously fed into the production line through the unwinding device and the feeding device. S2: The inner tube surface is pretreated by hot alkaline solution immersion to dissolve the original alumina film, rinsing with water to remove alkaline residue, mechanical grinding or polishing to further remove the oxide layer, neutralizing residual alkaline substances with acid, and cleaning and drying to prevent secondary oxidation. S3: Preheating treatment, using an induction heating device or a resistance preheating furnace to heat the preheated inner tube to the preheating temperature; S4: Outer layer aluminum liquid melting and heat preservation. The outer layer aluminum alloy is melted in a melting furnace and then introduced into the heat preservation intermediate ladle, and the temperature is controlled in the semi-molten temperature range. S5: Hot extrusion composite and synchronous internal thread forming. The outer semi-molten aluminum alloy is wrapped around the outer wall of the inner tube under pressure through an annular extrusion die to form an aluminum-aluminum metallurgical interface. At the same time, under the action of the internal thread extrusion module integrated in the hot extrusion composite die, continuous internal threads are extruded synchronously on the inner wall of the inner tube. During the extrusion process, the circumferential rotation of the internal thread extrusion module is restricted by the circumferential anti-rotation positioning structure. S6: Cooling and shaping, using water cooling or air cooling devices to quickly cool and shape the hot-extruded composite pipe; S7: Traction and winding cutting. The composite tube is pulled out from the extrusion station by the traction device, and the finished composite aluminum tube is wound into a coil by the winding device, or the tube is cut to a predetermined length by the fixed length cutting device.

2. The production method according to claim 1, characterized in that, The inner aluminum alloy is 6063 or 6061 wrought aluminum alloy, and the outer aluminum alloy is 4045 or 4047 cast aluminum alloy; the semi-molten temperature of the outer aluminum alloy is controlled at 575~585℃.

3. The production method according to claim 1, characterized in that, The specific process for surface pretreatment in step S2 is as follows: S21: Hot alkaline solution immersion, immersing the inner tube in a 5%~15% sodium hydroxide or sodium carbonate solution at a solution temperature of 60~90℃ for 3~10s to dissolve the original alumina film. S22: Rinse with clean water, using a high-pressure water spray of 0.3~0.5MPa for 2~5 seconds to remove alkaline residue; S23: Mechanical grinding or polishing, using grinding rollers with a speed of 1000~3000r / min and polishing wheels with a speed of 500~1500r / min to treat the outer surface of the aluminum tube, remove residual oxide layer and activate the surface; S24: Acid neutralization. Immerse the inner tube in a 1%~5% dilute phosphoric acid or dilute acetic acid solution for 2~5 seconds to neutralize residual alkaline substances. S25: Clean and dry. After rinsing with clean water, dry with hot air at 80~120℃ for 3~8 seconds to prevent secondary oxidation.

4. The production method according to claim 1, characterized in that, In step S5, the hot extrusion pressure is controlled at 100~800MPa, and the production line traction speed is 5~20m / min. Under the extrusion pressure, the outer semi-molten aluminum alloy undergoes atomic diffusion with the outer wall of the inner tube to form a metallurgical bonding interface. No additional protective atmosphere is required during the extrusion process, and an aluminum oxide protective film naturally forms on the outer surface.

5. The production method according to claim 1, characterized in that, In step S5, the internal thread extrusion module is a detachable structure, and the extruded internal thread profile is triangular or trapezoidal with a pitch of 0.5~2.0mm and a tooth depth of 0.1~0.5mm. During the axial feeding of the pipe, the pipe rotates circumferentially along the spiral surface of the internal thread extrusion module. The traction device only provides axial traction force and does not restrict the circumferential rotational freedom of the pipe.

6. The production method according to claim 1, characterized in that, In step S6, primary cooling is first performed using annular spray water cooling at 15~30℃ and 0.2~0.4MPa, followed by secondary cooling using air cooling at a wind speed of 10~20m / s, to reduce the surface temperature of the composite pipe to below 100℃ and complete the shaping process.

7. The production method according to claim 1, characterized in that, In step S7, a tracked or clamping traction device is used to pull the composite pipe, and the traction force is controlled at 100~2000N; the finished roll diameter is 500~800mm and the weight of a single roll is 50~200kg; the fixed length cutting is done by flying saw cutting, and the cutting accuracy is ±1mm.

8. A production equipment employing the method for producing aluminum-aluminum composite pipes for heat exchange according to any one of claims 1-7, characterized in that, The production units are arranged horizontally in sequence to form a horizontal continuous production line, including: Inner tube unwinding and feeding unit, used for unwinding and feeding solid aluminum alloy inner tubes in the form of coiled materials; The surface pretreatment unit includes, in sequence, a hot alkaline solution immersion tank, a clean water rinsing tank, a mechanical grinding device, an acid neutralization tank, and a cleaning and drying device, which are used to pretreat the surface of the inner tube to remove the original oxide film. The preheating unit uses an induction heating device or a resistance preheating furnace to heat the pretreated inner tube to 400~500℃; The outer aluminum liquid supply unit includes an aluminum alloy melting furnace and a heat-insulating intermediate ladle, which is used to melt and heat-insulate the outer 4-series aluminum alloy to a semi-molten state, wherein the temperature of the semi-molten state is 5~15°C higher than the solidus temperature of the outer aluminum alloy; A hot extrusion composite unit includes an annular extrusion die and an internal thread forming module integrated into the inner core of the annular extrusion die. The annular extrusion die is used to hot extrude and composite an outer semi-molten aluminum alloy layer onto the outer wall of an inner tube. The internal thread forming module is used to simultaneously extrude and form internal threads on the inner wall of the inner tube during the composite process. A circumferential anti-rotation positioning structure is provided between the mating end faces of the internal thread forming module and the inner core. The circumferential anti-rotation positioning structure is used to restrict the circumferential rotation of the internal thread forming module relative to the inner core. The cooling and shaping unit uses a combination of water cooling and air cooling devices to cool and shape the composite pipe. The traction unit, using a tracked or clamping traction device, is used to pull the composite pipe out from the extrusion station; The winding and cutting unit uses a finished product winding device or a fixed-length cutting device to wind or cut finished products. The control system is connected to the preheating unit and the outer aluminum liquid supply unit respectively, and is used to control the preheating temperature of the inner tube and the temperature of the outer aluminum liquid in a coordinated manner, so that the temperature of the semi-molten aluminum alloy in the outer layer is 80~120℃ higher than the preheating temperature of the inner tube.

9. The production equipment according to claim 8, characterized in that, The annular extrusion die includes an outer die sleeve, an inner die core, and a die base. An annular forming cavity is formed between the outer die sleeve and the inner die core. The aluminum liquid outlet of the heat-insulating intermediate ladle is connected to the annular forming cavity. A resistance heating coil or induction heating coil is provided on the outside of the die, and the working temperature of the die is maintained at 200~350℃.

10. The production equipment according to claim 8, characterized in that, The internal thread forming module includes a thread extrusion die and a die fixing mechanism. The outer wall of the thread extrusion die is provided with a raised thread profile. The circumferential anti-rotation positioning structure is a flat key or a positioning pin, which is embedded between the mating end faces of the thread extrusion die and the inner die core. The die fixing mechanism adopts a detachable structure with a locking cover and screw connection, which is fixed to the end of the inner die core and is used to replace extrusion dies with different thread parameters.