Method for processing a metal gilled tube
By using a metal hook-tooth tube processing method, a metal hook-tooth tube with grooves on both the inner and outer walls has been realized, which solves the problem of insufficient heat exchange enhancement on the outer side of the tube in the existing technology, significantly improves the heat exchange performance, and is suitable for air conditioning and two-phase cooling devices.
Patent Information
- Application Number
- CN202611617033.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies only achieve groove forming on the inner wall of heat exchanger tubes, and the control of the medium flow field on the outer side of the tube is insufficient, resulting in limited heat exchange enhancement effect on the outer side of the tube and room for improvement in overall heat exchange performance.
The metal hook-tooth tube processing method involves a complete process chain of cold rolling, multi-pass stretching, annealing, inner groove forming, and outer groove forming. The inner groove is spun by a floating mandrel ball and the outer groove is cut by a coaxial die, forming a metal hook-tooth tube with grooves on both the inner and outer walls.
It significantly increases the heat exchange contact area, guides the medium on the outside of the pipe to flow towards the center inside the pipe, shortens the heat transfer distance between the hot and cold media, and improves the overall heat exchange effect. It is suitable for air conditioning heat exchange and two-phase cooling devices.
Smart Images

Figure CN123149277A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of heat exchanger tube processing technology, specifically to a method for processing metal toothed tubes. Background Technology
[0002] Heat exchanger pipes are widely used in heat exchange equipment such as air conditioning and two-phase cooling. By setting grooves on the pipe wall, the contact area between the medium and the heat exchanger can be increased, thereby enhancing the heat exchange capacity.
[0003] Chinese invention patent CN101817025A discloses a method for preparing an internally grooved heat-conducting copper tube. This method involves cold rolling, annealing, and stretching a copper billet, then using a meteor spinning process to machine grooves into the inner wall of the tube. The heat transfer area of the medium inside the tube is increased solely by these inner grooves, resulting in a heat-transferring copper tube with a smooth outer wall. While this process can produce a complete toothed inner groove, it only achieves groove formation on one side of the tube. The outer wall remains smooth, making it impossible to control the flow field of the medium outside the tube. The heat transfer medium outside the tube is far from the center of the medium inside the tube, resulting in a large heat transfer distance between the hot and cold media. Therefore, the heat transfer enhancement effect on the outer side of the tube is limited, and there is still room for improvement in the overall heat transfer performance. Summary of the Invention
[0004] The present invention aims to at least partially solve one of the technical problems in the aforementioned technologies. Therefore, the objective of the present invention is to provide a method for processing metal toothed tubes, which enables the complete fabrication and processing of metal toothed tubes, ensures reliable groove forming, and offers strong process compatibility.
[0005] To achieve the above objectives, the present invention proposes a method for processing metal hook-tooth tubes, comprising the following steps: S1. Cold rolling: Providing pipes and cold rolling the pipes; S2. Stretching: The cold-rolled tube is subjected to multiple continuous stretching processes. S3, First Annealing: Annealing is performed on the stretched pipe; S4. Inner groove forming: The inner groove is formed by rotating and pressing the outer spherical ball bearings of the floating mandrel while stretching and spinning. S5. Second annealing: The pipe after the inner groove is formed is annealed again; S6. External groove forming: A forming device including a traction mechanism, a mandrel clamping device, a mandrel, a front mold base, a mold, and a rear mold base is used. The through holes of the front mold base, the mold, and the rear mold base are arranged coaxially. External groove forming includes the following sub-steps: S6-1, Assembly: Sleeve the pipe over the mandrel and clamp the end of the mandrel with a mandrel clamping device; S6-2, Passing through the mold: Pass the tube with the assembled mandrel through the front mold base, the mold, and the rear mold base in sequence; S6-3, Traction and Stretching: The traction mechanism clamps the end of the pipe and stretches it, using the cutting edge angle of the front end of the mold to process an outer groove on the outer wall of the pipe.
[0006] This invention discloses a method for processing metal hooked tubes. Using metal tubes as the starting material, the tube blank undergoes pretreatment through cold rolling, multi-pass stretching, and a first annealing. Subsequently, a moving mandrel is used to spin-form the inner grooves of the tube, followed by a second annealing to adjust the tube's plasticity. A coaxially arranged front mold base, die, and rear mold base, along with a mandrel, are used for clamping and positioning. The mandrel remains stationary during processing, providing radial support to the tube's interior and applying traction and stretching. The outer grooves are then formed using the cutting edge angle of the mold. This method forms a complete process chain from tube pretreatment to the processing of inner and outer grooves. The rationally designed sequence of each process, combined with the synergistic effect of the mandrel and mold base, ensures the stability of the forming process. It is adaptable to processing metal raw materials with different plasticities and effectively improves the groove forming effect.
[0007] In addition, the metal hook-tooth tube processing method proposed in the above embodiments of the present invention may also have the following additional technical features: Optionally, in step S1, the provided pipe is a copper pipe.
[0008] Optionally, after cold rolling in step S1, the outer diameter of the tube is 50mm~55mm and the wall thickness is 2mm~3mm.
[0009] Optionally, after stretching in step S2, the outer diameter of the tube is 9mm~10mm and the wall thickness is 0.2mm~0.5mm.
[0010] Optionally, step S3, first annealing: annealing temperature 500℃~600℃, holding time 3h~6h.
[0011] Optionally, after the inner groove is formed in step S4, the outer diameter of the pipe is 2mm~10mm, the wall thickness is 0.1mm~0.5mm, and the number of teeth in the inner groove is 10~120.
[0012] Optionally, step S5 involves a second annealing process: annealing temperature of 300℃~600℃, and holding time of 1h~3h.
[0013] Optionally, in step S6-3, the angle between the cutting edge angle at the front end of the mold and the axis of the tube is 0.5°~5°.
[0014] Optionally, a straight pipe heading step may be included before the S6-1 assembly step: one end of the pipe is reduced in diameter to form a reduced-diameter end for clamping by the traction mechanism.
[0015] Furthermore, prior to cold rolling in step S1, the process includes melting the metal raw material and preparing the pipe by horizontal continuous casting. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the external groove forming structure of a pipe according to an embodiment of the present invention; Figure 2 A cross-sectional view of a metal hook-tooth tube according to an embodiment of the present invention; Figure 3 A cross-sectional view of a metal hook-shaped tube according to another embodiment of the present invention; Figure 4 A process flow diagram of a metal hook-tooth tube processing method according to an embodiment of the present invention; Explanation of reference numerals in the attached figures: Traction mechanism 1, mandrel clamping device 2, mandrel 3, front mold base 4, mold 5, cutting edge 51, rear mold base 6, tube 7, inner groove 71, outer groove 72. Detailed Implementation
[0017] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0018] To better understand the above technical solutions, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the invention to those skilled in the art.
[0019] To better understand the above technical solutions, the following will provide a detailed explanation of the technical solutions in conjunction with the accompanying drawings and specific implementation methods.
[0020] The following is for reference. Figures 1-4 The implementation of the metal hook-tooth tube processing method proposed in the embodiments of the present invention will be described in detail.
[0021] A method for machining a metal hook-tooth tube according to an embodiment of the present invention includes the following steps: S1, Cold rolling: Provide tube 7 and perform cold rolling on tube 7; S2. Stretching: The cold-rolled tube 7 is subjected to multiple continuous stretching processes. S3, First Annealing: Annealing treatment is performed on the stretched pipe 7; S4. Inner groove 71 forming: The inner groove 71 is formed on the inner wall of the tube 7 by using a rotating pressing method with the outer spherical ball bearing of the floating mandrel head, stretching and spinning at the same time. S5. Second annealing: The pipe 7 after the inner groove 71 is formed is annealed again; S6. External groove 72 forming: A forming device including a traction mechanism 1, a mandrel 3, a clamping device 2, a mandrel 3, a front mold base 4, a mold 5, and a rear mold base 6 is used. The through holes of the front mold base 4, the mold 5, and the rear mold base 6 are arranged coaxially. The external groove 72 forming includes the following sub-steps: S6-1. Assembly: Fit the pipe 7 onto the outside of the mandrel 3, and use the mandrel 3 clamping device 2 to clamp the end of the mandrel 3. S6-2, Passing through the mold: Pass the tube 7 with the assembled mandrel 3 through the front mold base 4, the mold 5 and the rear mold base 6 in sequence; S6-3, Traction and Stretching: The traction mechanism 1 clamps the end of the pipe 7 and stretches it. The cutting edge 51 at the front end of the mold 5 is used to process the outer groove 72 on the outer wall of the pipe 7.
[0022] In other words, this processing method uses metal tube 7 as the starting raw material, and then gradually reduces the wall thickness and outer diameter of tube 7 through cold rolling and multi-pass continuous stretching. Combined with a first annealing to eliminate work hardening of tube 7, it provides a matrix material with good plasticity for subsequent groove forming. The metal tube 7 can be obtained by melting metal raw materials and then horizontally casting. Next, a floating mandrel equipped with spherical balls is placed inside the tube 7. The spherical balls on the outside of the floating mandrel perform rotational rolling on the inner wall of tube 7. The floating mandrel can adopt an existing structure. While tube 7 is being axially stretched and fed, the spherical balls rotate relative to tube 7, compressing the metal on the inner wall of tube 7 to induce plastic flow, thereby forming alternating teeth and inner grooves 71 on the inner wall of tube 7. After the inner grooves 71 are processed, a second annealing is performed to further adjust the plastic state of tube 7, reducing the risk of tube 7 breaking during subsequent outer groove 72 processing. During the outer groove 72 forming stage, the traction mechanism 1, the mandrel 3 clamping device 2, the mandrel 3, and the coaxially arranged front mold base 4, mold 5, and rear mold base 6 are used in conjunction. The tube 7 is sleeved on the outside of the mandrel 3. The mandrel 3 is clamped and fixed by the mandrel 3 clamping device 2 and remains stationary during the processing. The mandrel 3 provides radial rigid support from the inside of the tube 7 to resist the radial extrusion force generated by the cutting of the mold 5, prevent the tube 7 from being flattened and collapsed, and maintain the inner diameter and roundness of the tube 7. After the tube 7 passes through each set of mold bases and mold 5, the end is clamped and stretched by the traction mechanism 1. Multiple outer grooves 72 are cut on the outer peripheral wall of the tube 7 by means of multiple cutting edges 51 distributed in a circle at the front end of the mold 5. The front mold base 4 and mold 5, as well as the mold 5 and rear mold base 6 are hollowed out. This can ensure that the tube 7 has sufficient support strength and facilitate the removal of processing waste. The metal hook-shaped tube prepared by this method has grooved structures on both the inner and outer walls of the tube, which can significantly increase the heat exchange contact area and guide the medium on the outside of the tube to flow towards the center of the medium inside the tube 7, shortening the heat transfer distance between the hot and cold media and further improving the overall heat exchange effect. It can be widely used in heat exchange scenarios such as air conditioning heat exchange and two-phase cooling devices. It has the ability to process and adapt to various plastic metal tubes 7 such as copper, aluminum, copper alloy, and aluminum alloy. Relying on the positioning and cooperation of the mandrel 3 and the coaxial mold base, the stability of the groove forming process is improved and the forming defects are reduced. The number and shape of the inner groove 71 and the outer groove 72 can be set according to the actual application.
[0023] Therefore, this metal hook-tooth tube processing method uses metal tube 7 as the starting material, and then completes the pretreatment of the tube 7 blank through cold rolling, multi-pass stretching, and a first annealing. Subsequently, the inner groove 71 of the tube 7 is processed by ball milling with a moving mandrel, and the plasticity of the tube 7 is adjusted by a second annealing. Then, a coaxially arranged front mold base 4, mold 5, and rear mold base 6, along with a mandrel 3, are used for clamping and positioning. The mandrel 3 remains stationary during processing and provides radial support to the inside of the tube 7, applying traction and stretching to the tube 7. The outer groove 72 is processed by the cutting edge 51 of the mold 5. This scheme forms a complete process chain from tube 7 pretreatment to the processing of the inner and outer grooves 72. The reasonable setting of the sequence of each process, and the synergy between the mandrel 3 and the mold base, ensure the stability of the forming process. It can be adapted to the processing of different plastic metal raw materials and effectively improves the groove forming effect.
[0024] Optionally, in step S1, the provided pipe 7 is a copper pipe. It is understood that... Optionally, after cold rolling in step S1, the outer diameter of the tube 7 is 50mm~55mm, and the wall thickness is 2mm~3mm. Understandably, the cold rolling process achieves preliminary diameter and wall reduction of the tube blank. This parameter is an intermediate transition specification, reserving a reasonable amount of deformation for subsequent multi-pass continuous stretching. If the wall thickness is too thin, the tube 7 is prone to cracking during the cold rolling process; if the wall thickness is too thick, it will increase the load on the subsequent stretching equipment, and the tube 7 is prone to uneven deformation.
[0025] Optionally, after stretching in step S2, the outer diameter of the tube 7 is 9mm~10mm, and the wall thickness is 0.2mm~0.5mm. Understandably, the tube 7 is further thinned to this specification through multiple continuous stretching passes. This size is the blank state before the inner groove 71 is formed. If the wall thickness is too large, it will increase the processing resistance of the subsequent ball-bearing spinning of the inner groove 71; if the wall thickness is too small, the strength of the tube 7 will be insufficient, and the tube wall will easily break during the spinning process.
[0026] Optionally, step S3, the first annealing, involves an annealing temperature of 500℃~600℃ and a holding time of 3h~6h. Understandably, after cold rolling and stretching, the pipe 7 exhibits severe work hardening. This annealing process is used to eliminate internal stress, refine the microstructure, and restore the plasticity of the pipe 7. If the annealing temperature is too low or the holding time is insufficient, the work hardening cannot be fully eliminated; if the temperature is too high or the holding time is too long, abnormal grain growth will occur, leading to a decrease in the mechanical properties of the pipe 7.
[0027] Optionally, after the inner groove 71 is formed in step S4, the outer diameter of the tube 7 is 2mm~10mm, the wall thickness is 0.1mm~0.5mm, and the number of teeth in the inner groove 71 is 10~120. Understandably, the outer diameter and wall thickness of the tube 7 are adapted to the operating conditions of the heat exchange tube; the number of teeth in the groove directly affects the heat exchange area. Too few teeth will limit the heat exchange improvement effect, while too many teeth will increase the difficulty of spinning, and the groove teeth are prone to collapse or missing teeth, resulting in the scrap of the finished product.
[0028] Optionally, step S5 involves a second annealing: annealing temperature of 300℃~600℃, holding time of 1h~3h. Understandably, the forming of the inner groove 71 involves large plastic deformation, causing the pipe 7 to undergo work hardening again. This annealing is used to adjust the plasticity of the pipe 7, preparing it for the cutting and stretching of the outer groove 72. Insufficient annealing results in a pipe 7 with excessive hardness, making it prone to breakage during stretching; excessive annealing makes the pipe 7 too soft, easily causing collapse during forming, and resulting in an incomplete outline of the outer groove 72.
[0029] Optionally, in step S6-3, the angle between the cutting edge 51 at the front end of the mold 5 and the axis of the tube 7 is 0.5°~5°. Understandably, this cutting edge 51 angle is the inclination angle of the cutting edge 51 of the mold 5 relative to the stretching feed axis of the tube 7; if the angle is too small, the cutting forming ability is weak, making it difficult to cut out a clear and complete outer groove 72; if the angle is too large, the cutting resistance increases sharply, and the tube wall is easily cut through during the stretching process, causing the tube 7 to break and be scrapped.
[0030] Optionally, a straight pipe heading step is included before the S6-1 assembly step: one end of the pipe 7 is reduced in diameter to form a reduced-diameter end for clamping by the traction mechanism 1. Understandably, this reduced-diameter end facilitates the passage of the pipe 7 through the mold base and mold 5, while providing a reliable clamping position for the traction mechanism 1 to achieve the stretching feed of the pipe 7; this reduced-diameter end is a process auxiliary end and not an effective part of the finished product. After the outer groove 72 is formed, the reduced-diameter end can be cut off to obtain a qualified metal hook-tooth pipe finished product.
[0031] Furthermore, prior to cold rolling in step S1, the process includes melting the metal raw material and preparing the pipe 7 through horizontal continuous casting. Understandably, by integrating melting and horizontal continuous casting to prepare the pipe 7 billet, direct forming from the metal raw material to the billet can be achieved, reducing intermediate transfer and secondary heating processes. The pipe billet formed by horizontal continuous casting has a dense structure and uniform impurity distribution, which is beneficial for subsequent cold rolling and stretching processes, reducing the probability of cracks occurring during subsequent forming. Of course, the present invention is not limited to this; qualified metal pipe 7 billets can also be directly purchased and used in the cold rolling process to achieve the same processing objective.
[0032] In summary, the above-mentioned optional technical features of this invention can be used individually or in combination. This invention achieves the preparation of metal hook-tooth tubes through a complete process chain. The tube blank can be obtained first through melting and horizontal continuous casting, or a purchased metal tube blank 7 can be used directly. Then, the dimensions and plasticity of the tube 7 are controlled sequentially through cold rolling, stretching, and two annealing processes. The inner groove 71 is formed by ball-bearing spinning, and the outer groove 72 is formed by cutting with a die 5. By optimizing and controlling parameters such as the dimensions of the tube blank and tube 7 at each stage, the annealing process, the number of teeth in the inner groove 71, the cutting edge angle of the die 5, and the straight tube heading process, the risk of defects such as tube breakage, groove tooth collapse, and forming failure can be reduced, ensuring the integrity and dimensional consistency of the inner and outer groove tooth profiles. This invention is applicable to a variety of plastic metals and has a wide range of process applications. The resulting toothed tube has grooved structures on both the inner and outer walls, which not only increases the heat exchange contact area on both sides, but also disturbs the flow field of the medium on the outside of the tube, causing the external medium to move closer to the center of the medium inside the tube, shortening the heat transfer distance between the hot and cold media, resulting in excellent heat exchange effect. It can meet the needs of various heat exchange equipment such as air conditioners and two-phase cooling devices.
[0033] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0034] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.
[0035] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0036] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.
[0037] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. The illustrative expressions of the above terms in this specification should not be construed as necessarily referring to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. In addition, those skilled in the art can combine and integrate the different embodiments or examples described in this specification.
[0038] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A method for processing metal hook-tooth tubes, characterized in that, Includes the following steps: S1. Cold rolling: Providing pipes and cold rolling the pipes; S2. Stretching: The cold-rolled tube is subjected to multiple continuous stretching processes. S3, First Annealing: Annealing is performed on the stretched pipe; S4. Inner groove forming: The inner groove is formed by rotating and pressing the outer spherical ball bearings of the floating mandrel while stretching and spinning. S5. Second annealing: The pipe after the inner groove is formed is annealed again; S6. External groove forming: A forming device including a traction mechanism, a mandrel clamping device, a mandrel, a front mold base, a mold, and a rear mold base is used. The through holes of the front mold base, the mold, and the rear mold base are arranged coaxially. External groove forming includes the following sub-steps: S6-1, Assembly: Sleeve the pipe over the mandrel and clamp the end of the mandrel with a mandrel clamping device; S6-2, Passing through the mold: Pass the tube with the assembled mandrel through the front mold base, the mold, and the rear mold base in sequence; S6-3, Traction and Stretching: The traction mechanism clamps the end of the pipe and stretches it, using the cutting edge angle of the front end of the mold to process an outer groove on the outer wall of the pipe.
2. The method for processing metal hook-tooth tubes according to claim 1, characterized in that, In step S1, the provided pipe is a copper pipe.
3. The method for processing metal hook-toothed tubes according to claim 1, characterized in that, After cold rolling in step S1, the outer diameter of the tube is 50mm~55mm and the wall thickness is 2mm~3mm.
4. The method for processing metal hook-tooth tubes according to claim 1, characterized in that, After stretching in step S2, the outer diameter of the tube is 9mm~10mm and the wall thickness is 0.2mm~0.5mm.
5. The method for processing metal hook-toothed tubes according to claim 1, characterized in that, Step S3 First annealing: Annealing temperature 500℃~600℃, holding time 3h~6h.
6. The method for processing metal hook-tooth tubes according to claim 1, characterized in that, After the inner groove is formed in step S4, the outer diameter of the pipe is 2mm~10mm, the wall thickness is 0.1mm~0.5mm, and the number of teeth in the inner groove is 10~120.
7. The method for processing metal hook-tooth tubes according to claim 1, characterized in that, Step S5 Second annealing: Annealing temperature 300℃~600℃, holding time 1h~3h.
8. The method for processing metal hook-tooth tubes according to claim 1, characterized in that, In step S6-3, the angle between the cutting edge angle at the front end of the mold and the axis of the tube is 0.5°~5°.
9. The method for processing metal hook-tooth tubes according to claim 1, characterized in that, Before the S6-1 assembly step, there is also a straight pipe heading step: one end of the pipe is reduced in diameter to form a reduced diameter end for the traction mechanism to hold.
10. The method for processing metal hook-tooth tubes according to any one of claims 1-9, characterized in that, Before cold rolling in step S1, the process further includes melting the metal raw material and preparing the pipe by horizontal continuous casting.
Citation Information
Patent Citations
Method for preparing internal groove heat-conducting copper pipe
CN101817025A