Manufacturing method of iron-nickel based superalloy thick-wall elbow and elbow manufactured thereby
By employing a multi-stage controlled heating and heat treatment process, the forming challenge of thick-walled elbows made of iron-nickel-based high-temperature alloys has been solved, achieving stability in high-temperature strength and oxidation resistance. This process is suitable for mass production on conventional equipment, eliminates weak points in the welding of dissimilar steels, and improves the reliability of high-temperature pipeline systems.
Patent Information
- Application Number
- CN202611654050.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-26
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies cannot effectively solve the forming problem of thick-walled elbows made of iron-nickel-based high-temperature alloys, which makes dissimilar material welded joints prone to cracking during high-temperature service and unable to fully utilize the material performance advantages.
The process employs a multi-stage controlled heating and heat treatment process, including controlled heating in the front and rear stages, combined with flattening and pressing processes, to control the precipitation temperature and holding time of the γ´ phase, ensuring uniformity and strength of the grain structure, and is suitable for mass production using conventional equipment.
Stable forming of iron-nickel-based high-temperature alloy thick-walled elbows has been achieved, with no surface defects and grain size controlled at 2.0~5.0. It possesses high-temperature strength, oxidation resistance, and structural stability, eliminates weak links in dissimilar steel welding, and improves the reliability of high-temperature pipeline systems.
Smart Images

Figure CN123149301A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hot forming technology for alloy elbows, specifically to a method for manufacturing a thick-walled iron-nickel-based high-temperature alloy elbow and the elbow manufactured therefrom, which is particularly suitable for manufacturing medium and large diameter thick-walled iron-nickel-based high-temperature alloy elbows. Background Technology
[0002] Due to their excellent high-temperature strength, oxidation resistance, and structural stability, as well as their high Fe content and good economic efficiency, iron-nickel-based supercritical alloys have become important candidate materials for high-temperature pressure-bearing components such as main steam pipes, headers, and superheaters / reheaters in advanced ultra-supercritical thermal power units with a temperature range of 650~700℃, and have broad prospects for engineering applications.
[0003] However, iron-nickel-based superalloys have a high degree of alloying, strong resistance to high-temperature deformation, and are highly sensitive to grain size with an extremely narrow hot working window. Elbow forming is a hot working process with large deformation. Thick-walled elbows, especially tube blanks with a wall thickness t to outer diameter D ratio t / D not less than 0.1, have large deformation amounts and long deformation durations. The forming difficulty increases significantly with increasing wall thickness, and there is a lack of mature and reliable forming processes that meet the requirements of use.
[0004] Elbows are key components in high-temperature pipeline systems for changing flow direction. The lack of a forming process for thick-walled elbows made of iron-nickel-based superalloys directly limits the engineering application of this material. If stable forming of thick-walled elbows cannot be achieved, once this material is used in engineering applications, elbows and other pipe fittings can only be manufactured using dissimilar materials. Dissimilar material elbows and iron-nickel-based superalloy main pipelines inevitably form dissimilar steel welded joints. Due to the mismatch in the thermal expansion coefficients and high-temperature creep strength of the two materials, these dissimilar steel joints are prone to generating significant thermal stress and microstructural differences during high-temperature service, often becoming weak points in the pipeline system. They tend to crack prematurely after a certain period of service, severely restricting the long-term safe operation of the unit and failing to fully utilize the overall performance advantages of iron-nickel-based superalloys.
[0005] For materials with high thermal sensitivity, such as titanium alloys and high-temperature alloys, existing technologies have developed forming methods that take into account both deformation and microstructure control, such as isothermal forging, hot die forging, and local induction heating forming.
[0006] Isothermal forging or hot die forging, where the die and billet are at the same temperature and deform at an extremely low strain rate, can resolve the time contradiction between high-temperature plasticity and grain growth. However, its implementation is subject to three limitations: it is only suitable for die-forged parts such as discs, shafts, and blades; isothermal tooling requires large tonnage and long-term pressure holding, which is geometrically impossible for rotating pipe fittings such as elbows; and cost dictates that it is only used for critical aerospace components and is difficult to use for mass production of power plant pipe fittings.
[0007] For precipitation-strengthened superalloys, the prevailing understanding in the field is that the temperature range in which the precipitate is easily nucleated and grown should be passed as quickly as possible to shorten the residence time in this temperature range and avoid the precipitation or growth of the strengthening phase during the forming process. Therefore, the traditional hot bending process is considered unsuitable for the bending forming of such alloys because it involves a long residence time in this temperature range.
[0008] In the prior art, Chinese patent CN116372508B discloses a medium-frequency induction local heating bend, which uses a narrow heating zone and rapid advance to compress the high temperature exposure time. Its limitations are: local instantaneous rapid heating and cooling leads to uneven grains and microstructure gradients; γ´ reinforced alloys have high deformation resistance and are prone to cracking during advance bending; and it relies on special equipment and tooling, resulting in high investment and manufacturing costs, and cannot be applied to large deformation pipe fittings such as iron-nickel-based high-temperature alloy thick-walled elbows.
[0009] Chinese patent application CN116079347A discloses a method for manufacturing a large-diameter, thick-walled, seamless hot-pressed elbow made of nickel-based alloy. However, nickel-based alloys have a wider hot working window and are not sensitive to heating regimes; while iron-nickel-based high-temperature alloys have an extremely narrow hot working window and high deformation resistance, which is fundamentally different from the process premise of this patent.
[0010] Chinese patent application CN119307836A discloses an aging treatment method for nickel-iron-based high-temperature alloy materials, which is used for microstructure preparation before cold working such as rolling and straightening. Its heating and heat preservation arrangements are designed for cold working conditions with small deformation, but do not involve the large deformation of thick-walled tube blanks for hot forming, and cannot solve the problem of elbow forming.
[0011] In summary, existing methods for controlling the crystallization of heat-sensitive alloys rely on specialized equipment and cannot be applied to elbow manufacturing. While existing elbow forming processes can achieve geometric shaping, the resulting elbows fail to meet the microstructure and mechanical properties required for high-temperature pressure-bearing components. Furthermore, existing alloy heating and heat treatment processes are not geared towards large-deformation hot forming conditions. A manufacturing method for thick-walled iron-nickel-based high-temperature alloy elbows has consistently lacked the ability to maintain acceptable grain structure and satisfactory mechanical properties while achieving the desired shape. Therefore, there is an urgent need to develop a manufacturing method for thick-walled iron-nickel-based high-temperature alloy elbows, ensuring that the elbow is made of the same material as the main pipeline, fundamentally eliminating the weak points in dissimilar steel welded joints, and fully leveraging the performance advantages of this type of alloy. Summary of the Invention
[0012] In view of the difficulties in forming iron-nickel-based superalloys due to their narrow hot working window, high resistance to high-temperature deformation, and high sensitivity of grain size to temperature, this invention provides a method for manufacturing a thick-walled elbow made of iron-nickel-based superalloys and the elbow manufactured therefrom.
[0013] In order to achieve the objectives of this invention, the following techniques are proposed: This invention provides a method for manufacturing a thick-walled elbow made of iron-nickel-based high-temperature alloy, comprising a forming process and a heat treatment process, wherein the forming process includes the following steps: Heating: The iron-nickel-based high-temperature alloy raw material billet is subjected to multi-stage controlled heating, including at least a first stage controlled heating and a last stage controlled heating; wherein the initial temperature of the first stage controlled heating is 300~700℃, and the temperature is increased at a rate of 100~200℃ / h to 20~80℃ above the γ´ phase precipitation temperature and held at that temperature for 0.7~1.5min / mm; the last stage controlled heating is increased at a rate of 50~150℃ / h to 120~200℃ above the γ´ phase precipitation temperature and held at that temperature for 0.7~1.5min / mm. Flattening: Flattening the heated raw material tube blank to the middle size; Pressing: The flattened tube blank is pressed with a mold, and the final pressing temperature is not lower than the precipitation temperature of the γ´ phase, followed by cooling.
[0014] Furthermore, the initial temperature of the controlled heating in the front section is 400~600℃, the heating rate is 120~170℃ / h, the temperature is raised to 40~70℃ above the γ´ phase precipitation temperature, and the holding time is 0.7~1.3min / mm.
[0015] Furthermore, the controlled heating rate in the final stage is 70~150℃ / h, the temperature is raised to 130~180℃ above the γ´ phase precipitation temperature, and the holding time is 0.7~1.3min / mm.
[0016] Furthermore, the outer diameter of the intermediate dimension is 0.93 to 0.99 times the outer diameter of the raw material tube blank.
[0017] Furthermore, the ratio of the wall thickness t of the raw material tube blank to its outer diameter D is t / D ≥ 0.1.
[0018] Furthermore, the heat treatment process after the elbow is formed includes at least a first-stage heating and a second-stage heating; wherein the first-stage heating starts at a temperature of 200~500℃, the heating rate is 100~200℃ / h, the temperature is raised to 20~60℃ above the γ´ phase precipitation temperature and held for 0.7~1.5min / mm; the second-stage heating raises the temperature at a rate of 50~150℃ / h to 80~150℃ above the γ´ phase precipitation temperature and holds for 0.7~1.5min / mm, followed by cooling.
[0019] Furthermore, the heating rate of the first stage is 130~170℃ / h, heating to 40~60℃ above the γ´ phase precipitation temperature, and holding at that temperature for 0.8~1.3min / mm; the heating rate of the second stage is 70~140℃ / h, heating to 80~120℃ above the γ´ phase precipitation temperature, and holding at that temperature for 0.8~1.3min / mm, followed by water cooling.
[0020] Furthermore, the iron-nickel-based superalloy comprises the following components by weight percentage: Fe 35~45%, Cr 15~21%, Mo 0.5~1.4%, W 0.1~0.8%, Ti 1.8~2.5%, Al 0.8~2.5%, Mn≤1.0%, Nb≤0.1%, Co≤2%, Si≤0.05%, C 0.03~0.10%, B 0.001~0.005%, P≤0.01%, with the balance being Ni; wherein the weight percentage of Cr+Ni is greater than 50%, and the weight percentage of W+Mo is 0.6~1.5%.
[0021] The present invention also provides a thick-walled elbow made of iron-nickel-based high-temperature alloy, which is manufactured by any of the above manufacturing methods.
[0022] Furthermore, the elbow has a grain size of 2.0~5.0, is free of mixed crystals, and has a room temperature tensile strength Rm of not less than 600MPa and a plastic elongation strength Rp. 0.2 Not less than 280MPa, elongation after fracture not less than 48%, and room temperature impact toughness KV2 not less than 130J.
[0023] In the above manufacturing method, the target temperature for each stage is determined based on the same γ' phase precipitation temperature. The target temperatures, heating rates, and holding times of the first and last stages, as well as the intermediate dimensions during flattening and the final pressing temperature, constitute an interconnected whole: the stage sequence determines the order of temperature homogenization and grain growth in the tube blank cross-section; the heating rates of each stage and the holding times calculated based on the tube blank wall thickness jointly determine the total amount of time the tube blank spends in the temperature range above the γ' phase precipitation temperature; the intermediate dimensions during flattening determine the distribution of deformation between the flattening and pressing steps; and the final pressing temperature determines whether the γ' phase precipitates during the pressing stage. These parameters must be coordinated as a whole; any deviation from their defined range will lead to grain coarsening, mixed crystal formation, or incomplete molding.
[0024] To facilitate understanding of the technical solution of this invention, the following key terms are explained: The γ' phase precipitation temperature described in this invention: The γ' phase (gamma prime phase) is the main precipitation strengthening phase in iron-nickel-based superalloys, with the chemical formula Ni3(Al,Ti). The γ' phase precipitation temperature refers to the critical temperature at which the γ' phase begins to precipitate from the austenitic matrix, and is usually determined by differential scanning calorimetry (DSC) or phase diagram thermodynamic calculations.
[0025] The controlled heating described in this invention refers to the process of actively controlling the heating rate of the furnace according to a set heating curve, so that the billet heats up with the furnace. Unless otherwise specified, the heating rate, starting temperature, and target temperature of each segment mentioned in this invention are all based on the furnace temperature. After the billet enters the furnace from ambient temperature, the heating rate is not actively controlled when the furnace temperature is lower than the starting temperature of the controlled heating; this segment is not counted in the number of controlled heating segments. From the moment the furnace temperature reaches the starting temperature of the controlled heating, the furnace temperature heats up at the set rate; this segment is counted in the number of controlled heating segments.
[0026] The multi-stage controlled heating described in this invention refers to dividing the controlled heating process into at least two stages, each with a different heating rate and / or target temperature. The first stage of controlled heating is called the pre-stage controlled heating, the last stage is called the final stage controlled heating, and the stage in between is called the mid-stage controlled heating. Multi-stage controlled heating is based on the pre-stage and final stage controlled heating, i.e., two-stage controlled heating; alternatively, an additional stage can be added between the pre-stage and final stage, i.e., three-stage controlled heating. This invention preferably uses a two-stage controlled heating system.
[0027] The first and second stage heating stages mentioned in this invention refer to the controlled heating stages divided in sequence during the heat treatment process after the elbow is formed. The first stage heating stage comes first, followed by the second stage heating stage. The target temperature is set based on the γ´ phase precipitation temperature, and the heating rate and holding time are limited respectively.
[0028] The intermediate dimension mentioned in this invention refers to the outer diameter of the tube blank after it has been flattened, which is between the outer diameter of the finished elbow and the outer diameter of the raw tube blank.
[0029] The final pressing temperature mentioned in this invention refers to the actual temperature of the tube blank when the die pressing is completed.
[0030] The elbows described in this invention include, but are not limited to: 45° elbows, 90° elbows, 180° elbows, long-radius elbows, and short-radius elbows.
[0031] Compared with the prior art, the technical solution of the present invention achieves the following overall effects: This invention solves the long-standing problem of unstable forming of thick-walled elbows made of iron-nickel-based high-temperature alloys. The method of this invention is applicable to thick-walled tube blanks with a t / D ratio of not less than 0.1, and the elbows produced are free from defects such as cracks, laps, folds, and dents on the surface, and the finished product dimensions and non-destructive testing are all qualified.
[0032] The grain structure is controllable throughout the forming process of this invention, and no mixed crystals occur. Since the heating and heat treatment stages are set with the γ´ phase precipitation temperature as the reference and the holding time is limited, and the flattening first undertakes part of the deformation and the pressing stage is completed above the γ´ phase precipitation temperature, the γ´ phase does not precipitate during the deformation process, and the deformation resistance and deformation uniformity are controlled.
[0033] The strength and service behavior of the iron-nickel-based superalloy of this invention are jointly controlled by the grain structure and the state of the precipitated phases. When the grains are fine and uniform, grain boundary strengthening and precipitation strengthening work synergistically, and the material maintains high strength and plasticity levels at room temperature, 600°C, and 700°C. Fine and uniform grains result in low grain boundary migration driving force and low grain growth tendency during long-term high-temperature service, leading to long-term stable microstructure. Elements such as chromium and aluminum in the alloy impart oxidation resistance by forming a dense oxide film on the surface, and the fine grain structure makes the oxide film adhere more firmly, further delaying the oxidation process. The grain size of the elbow of this invention is controlled at 2.0 to 5.0 and free of mixed crystals, which perfectly matches the above-mentioned material characteristics, thus possessing high-temperature strength, oxidation resistance, and microstructure stability.
[0034] This invention offers a wide process window and strong adaptability to specifications. Under the conditions that the end point of each heating stage is based on the γ´ phase precipitation temperature, the holding time is limited to 0.7~1.5 min / mm, and the final pressing temperature is not lower than the γ´ phase precipitation temperature, tube blanks of different t / D specifications can be flattened and pressed in one furnace charge to obtain qualified microstructure and properties. Adjusting parameters within the limited range does not affect the forming stability, making it easy to organize production according to different product specifications and ensuring good batch production quality consistency.
[0035] This invention features short processes, universal equipment, and controllable costs, making it suitable for industrial mass production. It requires only a conventional heating furnace and press; the mold can be preheated using conventional methods, eliminating the need for isothermal forging equipment, specialized induction bending equipment, or long-term pressure-holding fixtures. The tube blank undergoes continuous flattening and pressing within a single furnace loading, eliminating the need for intermediate reheating and avoiding the grain coarsening caused by secondary high-temperature exposure. This shortens the process cycle and reduces energy consumption and equipment investment.
[0036] This invention eliminates the weak points in high-temperature pipeline systems. Elbows can be manufactured using the same iron-nickel-based high-temperature alloy as the main pipeline, avoiding early cracking failure caused by the mismatch between the thermal expansion coefficient and high-temperature creep strength of dissimilar steel welded joints. This fully leverages the performance advantages of iron-nickel-based high-temperature alloys at high temperatures of 650~700℃, improving the overall reliability and service life of high-temperature pipeline systems. Attached Figure Description
[0037] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.
[0038] Figure 1 This is a process flow diagram of the manufacturing method of the present invention.
[0039] Figure 2 This is a schematic diagram of the segmented temperature rise curves during the heating process in Example 1.
[0040] Figure 3 This is a cross-sectional view of the tube blank being moved onto the press in preparation for pressing during the pressing process in Example 1.
[0041] Figure 4 This is a schematic cross-sectional view of the tube blank after pressing in Example 1.
[0042] Figure 5 The two-stage temperature-time curves of the heat treatment in Example 1 are shown.
[0043] Figure 6 Metallographic micrograph of the center of wall thickness of the finished elbow prepared in Example 1.
[0044] Figure 7 Metallographic microstructure of the inner surface of the finished elbow prepared in Example 1.
[0045] Figure 8 Metallographic micrograph of the outer surface of the finished elbow prepared in Example 1.
[0046] Figure 9 Metallographic microstructure of the finished elbow prepared for Comparative Example 3.
[0047] In the diagram: 1 is the tube blank, 2 is the press head, and 3 is the mold. Detailed Implementation
[0048] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0049] The present invention will be further described below with reference to embodiments.
[0050] Example 1
[0051] The composition of the iron-nickel-based superalloy in this embodiment, by weight percentage, includes: Fe 35%, Cr 15%, Mo 0.5%, W 0.1%, Ti 1.8%, Al 0.8%, Mn 1.0%, Nb 0.1%, Co 2%, Si 0.05%, C 0.03%, B 0.001%, P 0.01%, with the balance being Ni; the weight percentage of Cr+Ni is 58.6%, and the weight percentage of W+Mo is 0.6%.
[0052] A 90° elbow with an OD of 474mm × 75mm (t / D≈0.158) was prepared using an iron-nickel-based superalloy with the above composition. The preparation process is as follows: Figure 1 As shown.
[0053] Raw material tube blank: Provide iron-nickel based high-temperature alloy tube blank with the above composition, outer diameter OD=508mm, wall thickness t=83mm, t / D≈0.163.
[0054] Heating: such as Figure 2 As shown, a regenerative chamber natural gas heater is used. The bottom of the raw material billet is raised by 30cm. A two-stage controlled heating method is adopted. When the furnace temperature is below 500℃, the heating rate is not controlled. When the furnace temperature reaches 500℃, the first stage of controlled heating begins, with a heating rate of 150℃ / h, reaching 50℃ above the γ´ phase precipitation temperature (γ´+50℃) and holding at that temperature for 1min / mm. Then, the final stage of controlled heating begins, with a heating rate of 100℃ / h, reaching 150℃ above the γ´ phase precipitation temperature (γ´+150℃) and holding at that temperature for 0.8min / mm. Figure 2 In the middle section, m1 represents the time required for the controlled heating in the first stage to rise from 500℃ to γ´+50℃; m2 represents the time required for the controlled heating in the last stage to rise to γ´+150℃.
[0055] Flattening: The heated raw material tube blank is flattened to 490mm using a 5000-ton press; Suppression: such as Figure 3 and Figure 4 As shown, an 8000-ton press was used to press the flattened tube blank using a mold (air pressure). The mold was preheated to 550°C, and the tube was pressed in one pass until the mold was completely closed. The final pressing temperature was 8°C above the γ´ phase precipitation temperature (γ´+8°C). The tube was then cooled to room temperature using water quenching. The final pressing temperature was measured using an infrared thermometer. After pressing, the process allowances at both ends were removed, and the tube was finished.
[0056] Heat treatment: such as Figure 5As shown, the heating rate is not controlled below 300℃. Above 300℃, it is the first stage of heating, with a heating rate of 150℃ / h. After heating to 50℃ (γ´+50℃) above the γ´ phase precipitation temperature, it is held for 1min / mm. The subsequent second stage of heating is carried out at 140℃ / h to 120℃ (γ´+120℃) above the γ´ phase precipitation temperature, and held for 1min / mm. Then it is cooled to room temperature by rapid cooling with clean water. Figure 5 In this context, m1 represents the time required to raise the temperature from 300℃ to γ´+50℃, and m2 represents the time required to raise the temperature to γ´+120℃.
[0057] Inspection: Visual inspection revealed that the elbow surface was free of defects such as cracks, laps, folds, dents, and sharp scratches; the finished product dimensions and non-destructive testing were all qualified.
[0058] Figure 6 The image shows the metallographic examination of the center of the elbow wall thickness, with a grain size of 3.5. Figure 7 The image shows the metallographic examination of the inner surface, with a grain size of 3.0. Figure 8 The metallographic image shows the outer surface, with a grain size of 4.0 and a carbide grade of 1, exhibiting no mixed crystals. Mechanical testing revealed a room temperature tensile strength Rm = 629 MPa and a ductile elongation strength Rp. 0.2 =330MPa, elongation after fracture A=54.0%, reduction of area 64%, impact toughness KV2=147J, Brinell hardness HBW=160~166; high temperature at 600℃ Rm=561MPa, plastic tensile strength Rp 0.2 =332MPa, elongation after fracture A=45.5%, high temperature at 700℃ Rm=528MPa, plastic tensile strength Rp 0.2 =334MPa, elongation after fracture A=44.0%, and good high-temperature mechanical properties.
[0059] The detection methods in all embodiments of this invention are the same, wherein the metallographic carbide detection uses the method of GB / T 13298-2015; the metallographic grain size detection uses the method of GB / T 6394-2017; the room temperature tensile strength, plastic extension strength and elongation after fracture detection uses the method of GB / T 228.1-2021; the Brinell hardness detection uses the method of GB / T 231.1-2018; the high temperature tensile strength, plastic extension strength and elongation after fracture at 600℃ and 700℃ uses the method of GB / T 228.2-2015; and the impact toughness detection uses the method of GB / T 229-2020.
[0060] Example 1a The forming process of this embodiment, including the raw material specifications, the controlled heating regime in the front stage, the controlled heating regime in the final stage, the flattening intermediate dimensions, and the final pressing temperature, is exactly the same as that of Embodiment 1. The only difference is the heat treatment method used after forming: this embodiment adopts a common single-stage heat treatment method, that is, after forming, the formed elbow is directly heated from room temperature to 120°C above the γ´ phase precipitation temperature at a heating rate of 150°C / h, held at that temperature for 1.5 min / mm, and then taken out of the furnace for air cooling, without setting a low-temperature homogenization section.
[0061] Compared to Example 1, all performance indicators in this example are reduced: grain size coarsened by approximately 0.5 grade, to grade 2.5~3.5, with no mixed crystals. Mechanical testing showed a room temperature tensile strength Rm = 612 MPa and a plastic elongation strength Rp... 0.2 =314MPa, elongation after fracture A=52.0%, reduction of area 62%, impact toughness KV2=137J, Brinell hardness HBW=156~162; high temperature at 600℃ Rm=545MPa, plastic tensile strength Rp 0.2 =315MPa, elongation after fracture A=43.5%, high temperature at 700℃ Rm=513MPa, plastic tensile strength Rp 0.2 =317MPa, elongation after fracture A=42.5%.
[0062] Compared to Example 1, all performance indicators in this example are reduced: the grain size is coarsened by about 0.5 grade to 2.5~3.5 grade, there is no mixed crystal, and the impact toughness is reduced to 137J, which is close to the lower limit of 130J. The remaining indicators still fall within the product performance range defined by this invention, but are lower than those in Example 1 overall.
[0063] Example 2 The composition of the iron-nickel-based superalloy in this embodiment, by weight percentage, includes: Fe 44.0%, Cr 21%, Mo 0.7%, W 0.3%, Ti 2.5%, Al 1.2%, Mn 0.3%, Nb 0.03%, Co 0.4%, Si 0.01%, C 0.10%, B 0.005%, P 0.003%, with the balance being Ni. The weight percentage of Cr+Ni is 50.45%, and the weight percentage of W+Mo is 1.0%.
[0064] A 90° elbow with an OD of 426mm × 50mm (t / D≈0.117) was prepared using an iron-nickel-based superalloy with the aforementioned composition. The preparation process is as follows: Figure 1 As shown.
[0065] Raw material tube blank: Provide iron-nickel based high-temperature alloy tube blank with the above composition, outer diameter OD=457mm, wall thickness t=55mm, t / D≈0.120.
[0066] Heating: A regenerative chamber natural gas heater is used. The bottom of the raw material billet is raised by 30cm. A two-stage controlled heating method is adopted. When the furnace temperature is below 300℃, the heating rate is not controlled. When the furnace temperature exceeds 300℃, the first stage of controlled heating begins, heating at 100℃ / h to 20℃ above the γ´ phase precipitation temperature (γ´+20℃) and holding for 0.7min / mm. The final stage of controlled heating then heats at 50℃ / h to 120℃ above the γ´ phase precipitation temperature (γ´+120℃) and holds for 0.7min / mm.
[0067] Flattening: The heated raw material tube blank is flattened to 430mm using a 5000-ton press.
[0068] Pressing: Using an 8000-ton press, the flattened tube blank is placed in a mold preheated to 500°C and pressed in a single pass until the mold is completely closed. The final pressing temperature is 17°C above the γ´ phase precipitation temperature, followed by rapid water cooling to room temperature. The final pressing temperature is measured using an infrared thermometer. After pressing, the process allowances at both ends are removed and the tube is finished.
[0069] Heat treatment: Below 200℃, the heating rate is not controlled. Above 200℃, it is the first stage of heating, with a heating rate of 100℃ / h. After heating to 20℃ above the γ´ phase precipitation temperature (γ´+20℃), it is held for 0.7min / mm. Then, in the second stage, the temperature is increased at 50℃ / h to 80℃ above the γ´ phase precipitation temperature (γ´+80℃), and held for 0.7min / mm. Then, it is rapidly cooled to room temperature with clean water.
[0070] Inspection: Visual inspection revealed no defects such as cracks, laps, folds, dents, or sharp scratches on the surface of the elbow. Metallographic examination of the finished elbow's wall center, inner surface, and outer surface showed a grain size of 3.0-4.0, a carbide grade of 1, and no mixed crystals. Mechanical testing showed a room temperature tensile strength Rm = 638 MPa and a plastic elongation strength Rp. 0.2 =313MPa, elongation after fracture A=52.5%, reduction of area 62%, impact toughness KV2=141J, Brinell hardness HBW=162~168; high temperature at 600℃ Rm=569MPa, plastic tensile strength Rp 0.2 =316MPa, elongation after fracture A=44.0%, high temperature at 700℃ Rm=540MPa, plastic tensile strength Rp 0.2 =319MPa, elongation after fracture A=42.0%, and good high-temperature mechanical properties.
[0071] Example 3 The composition of the iron-nickel-based superalloy in this embodiment, by weight percentage, includes: Fe 40%, Cr 17%, Mo 0.9%, W 0.6%, Ti 2%, Al 2.5%, Mn 0.8%, Nb 0.07%, Co 1.6%, Si 0.03%, C 0.07%, B 0.003%, P 0.006%, with the balance being Ni. The weight percentage of Cr+Ni is 51.42%, and the weight percentage of W+Mo is 1.5%.
[0072] A 90° elbow with an OD588mm×114mm (t / D≈0.194) was prepared using an iron-nickel-based superalloy with the aforementioned composition. The preparation process is as follows: Figure 1 As shown.
[0073] Raw material tube blank: Provide iron-nickel based high-temperature alloy tube blank with the above composition, outer diameter OD=630mm, wall thickness t=126mm, t / D≈0.2.
[0074] Heating: A regenerative chamber natural gas heater is used. The bottom of the raw material billet is raised by 35cm. A two-stage controlled heating method is adopted. When the furnace temperature is below 680℃, the heating rate is not controlled. When the furnace temperature exceeds 680℃, the first stage of controlled heating begins, heating at 200℃ / h to 80℃ above the γ´ phase precipitation temperature (γ´+80℃) and holding for 1.5min / mm. The final stage of controlled heating heats up at 150℃ / h to 200℃ above the γ´ phase precipitation temperature (γ´+200℃) and holds for 1.5min / mm.
[0075] Flattening: The heated raw material tube blank is flattened to 608mm using a 5000-ton press.
[0076] Pressing: Using an 8000-ton press, the flattened tube blank is placed in a mold preheated to 600°C and pressed in a single pass until the mold is completely closed. The final pressing temperature is the γ´ phase precipitation temperature (γ´). It is then rapidly cooled to room temperature with water. The final pressing temperature was measured using an infrared thermometer. After pressing, the process allowances at both ends are removed and the tube is finished.
[0077] Heat treatment: The heating rate is not controlled below 420℃. At 420℃, the first stage of heating begins at a heating rate of 155℃ / h. The temperature is raised to 55℃ above the γ´ phase precipitation temperature (γ´+55℃) and held for 1.5min / mm. Then, the second stage of heating begins at a rate of 150℃ / h to raise the temperature to 150℃ above the γ´ phase precipitation temperature (γ´+150℃) and held for 1.5min / mm. The temperature is then rapidly cooled to room temperature with clean water.
[0078] Inspection: Visual inspection revealed no defects such as cracks, laps, folds, dents, or sharp scratches on the surface of the elbow. Metallographic examination of the finished elbow's wall center, inner surface, and outer surface showed a grain size of 2.5-3.5, a carbide grade of 1, and no mixed crystals. Mechanical testing showed a room temperature tensile strength Rm = 615 MPa and a plastic elongation strength Rp. 0.2 =296MPa, elongation after fracture A=50.5%, reduction of area 60%, impact toughness KV2=136J, Brinell hardness HBW=156~162; high temperature at 600℃ Rm=547MPa, plastic tensile strength Rp 0.2 =299MPa, elongation after fracture A=42.5%, high temperature at 700℃ Rm=511MPa, plastic tensile strength Rp 0.2 =302MPa, elongation after fracture A=41.0%, and good high-temperature mechanical properties.
[0079] Examples 4 to 6 Examples 4 to 6 use the iron-nickel-based superalloy of Example 1 and manufacture iron-nickel-based superalloy elbows with different t / D raw material billets. The manufacturing steps are the same as in Example 1, except that the parameters at each stage are shown in Table 1.
[0080] Table 1. Process parameters and test results for Examples 1, 4 to 6
[0081] Tests showed that, under the conditions of Examples 4 to 6, the elbows could be successfully formed, and the metallographic, mechanical property, finished product dimensions, and non-destructive testing all passed.
[0082] In summary, the iron-nickel-based high-temperature alloy thick-walled elbows prepared in Examples 1 to 6 have a grain size of 2.0 to 5.0 and are free of mixed grains; their room temperature tensile strength Rm is not less than 600 MPa and their plastic elongation strength Rp is not less than 600 MPa. 0.2 Not less than 280MPa, elongation after fracture not less than 48%, room temperature impact toughness KV2 not less than 130J; tensile strength Rm at 600℃ not less than 530MPa, plastic elongation strength Rp 0.2 Not less than 285MPa, elongation after fracture not less than 40%; tensile strength Rm at 700℃ not less than 500MPa, and plastic elongation strength Rp 0.2 The strength is not less than 290 MPa and the elongation after fracture is not less than 38%.
[0083] Comparative Example 1 (using conventional forming and heating process) Elbows of the same specifications (OD474mm×75mm) were prepared using iron-nickel-based high-temperature alloy tube blanks (outer diameter 508mm, wall thickness 83mm) with the same composition as in Example 1. The flattening method, pressing method, mold preheating temperature, and post-forming heat treatment were all the same as in Example 1. The only difference was that the heating stage adopted conventional forming heating process in the art. After the tube blank was loaded into the heating furnace, the temperature was continuously increased at 200℃ / h from the furnace temperature of 500℃ to 150℃ above the γ´ phase precipitation temperature, and held for 1.5min / mm (approximately 125min for a wall thickness of 83mm). Then, the tube blank was taken out of the furnace, flattened, and pressed.
[0084] Results: The deformation resistance during the pressing process was lower than that in Example 1, but cracks appeared on the outer arc surface of the elbow. After pressing, longitudinal cracks were observed distributed along the axial direction, with a length of about 120 mm and a maximum depth of about 8 mm. The cracks extended along the grain boundaries. Metallographic analysis showed that the sample was taken from a location outside the cracks, with a grain size of 0.5~1.0, uniform and coarse grains, no mixed grain structure, and a carbide grade of 1. Mechanical analysis showed that the sample was taken from a location far from the cracks, with a room temperature tensile strength of about 566 MPa, a plastic extension strength of about 286 MPa, an elongation after fracture of about 47.0%, a reduction of area of about 57%, an impact toughness of about 79 J, and a Brinell hardness of about 144~150. At 600℃, the tensile strength was about 481 MPa, the plastic extension strength was about 283 MPa, and the elongation after fracture was about 39.5%. At 700℃, the tensile strength was about 452 MPa, the plastic extension strength was about 281 MPa, and the elongation after fracture was about 37.5%.
[0085] It is evident that under a continuous heating regime, even if the heating rate is not fast, the heat preservation is sufficient, and the resistance to pressing deformation is lower, thick-walled tube blanks cannot obtain fine and uniform grain structure, and the thermoplasticity of the coarse grain structure is insufficient to support pressing deformation, resulting in cracking and rejection during the forming stage.
[0086] Comparative Example 2 (using stepped heating) Elbows of the same specifications (OD474mm×75mm) were prepared using iron-nickel-based high-temperature alloy tube blanks (outer diameter 508mm, wall thickness 83mm) with the same composition as in Example 1. The flattening method, pressing method, mold preheating temperature, and post-forming heat treatment were all the same as in Example 1. The only difference was that the heating adopted a conventional stepped heating method in the art. The tube blank was loaded into the heating furnace from room temperature and heated in six steps from 300°C below the γ´ phase precipitation temperature to 120°C above the γ´ phase precipitation temperature. Each step was heated by 70°C and held at that temperature for 30 minutes. Then, the tube blank was taken out of the furnace, flattened, and pressed.
[0087] Results: Cracks appeared on the outer arc surface of the elbow during the pressing process. Post-pressing inspection revealed multiple fine cracks distributed in a network, mostly 2-3 mm deep, with some reaching a depth of about 5 mm. The cracks propagated along grain boundaries. The final pressing temperature was similar to that of Example 1. Metallographic analysis showed that the samples were taken from areas outside the cracks, with grain sizes ranging from 1.5 to 3.5. The difference between the largest and smallest grain sizes within the same field of view reached 2.0, indicating a distinct mixed-grain structure and a carbide grade of 1. Mechanical testing showed that the samples were taken from areas far from the cracks. The part exhibits the following characteristics: room temperature tensile strength approximately 605 MPa, ductile elongation approximately 313 MPa, elongation after fracture approximately 46.5%, reduction of area approximately 58%, impact toughness approximately 96 J, Brinell hardness approximately 154-160; 600℃ tensile strength approximately 507 MPa, ductile elongation approximately 305 MPa, elongation after fracture approximately 38.5%; 700℃ tensile strength approximately 481 MPa, ductile elongation approximately 301 MPa, elongation after fracture approximately 36.0%; the forming quality is substandard.
[0088] The comparative example was divided into sections with equal increments of 70°C, and the holding time for each section was a fixed 30 minutes, without being adjusted according to the billet wall thickness. The endpoint of its final section was close to the target temperature range of the controlled heating in the final section of this invention, yet it still failed to meet the elongation-to-fracture standard and was rejected due to cracking caused by mixed crystals. It is evident that simply adding a segmented format without simultaneously determining the target temperature for each section based on the γ´ phase precipitation temperature and adjusting the holding time according to the billet wall thickness cannot achieve qualified microstructure and properties while completing large deformation forming.
[0089] Comparative Example 3 (using rapid heating) Elbows of the same specifications were prepared using iron-nickel-based high-temperature alloy tube blanks with the same composition as in Example 1. The forming process was basically the same as in Example 1, except that after the temperature reached 500°C, the temperature was increased to 150°C (γ´+150°C) above the γ´ phase precipitation temperature at a rate of 5°C / min (i.e., 300°C / h), and the temperature was held for 1 min / mm (approximately 83 min). The tubes were then directly removed from the furnace and flattened and pressed. The flattening and pressing methods were the same as in Example 1.
[0090] Results: The elbow was well-formed, with no cracks, laps, folds, or other defects on the surface. Metallographic examination revealed grain size ranging from 0.5 to 2.0, with the largest grain size in the same field of view being more than three times the smallest grain size. A distinct mixed-grain structure was observed, with a carbide grade of 2. Local grain boundaries showed oxidation pores and remelting characteristics, indicating an overheated structure (see attached metallographic report). Figure 9Mechanical testing showed that the room temperature tensile strength was approximately 552 MPa, the plastic elongation strength was approximately 268 MPa, the elongation after fracture was approximately 44.0%, the reduction of area was approximately 57%, the impact toughness was approximately 51 J, and the Brinell hardness was approximately 140~146. At 600℃, the tensile strength was approximately 459 MPa, the plastic elongation strength was approximately 261 MPa, and the elongation after fracture was approximately 36.0%. At 700℃, the tensile strength was approximately 428 MPa, the plastic elongation strength was approximately 258 MPa, and the elongation after fracture was approximately 34.5%.
[0091] It is evident that, when a rapid heating path exceeding the limits of this invention is adopted on thick-walled tube blanks, although the total amount of residence in the temperature range above the γ´ phase precipitation temperature does not increase and no forming defects are observed on the elbow surface, abnormal grain growth occurs, along with mixed grains and overheated structures. Room temperature tensile strength, ductile elongation, elongation after fracture, and impact toughness all decrease significantly. Heating regimes oriented towards rapidly passing through the precipitation phase temperature range cannot yield satisfactory microstructure and properties on iron-nickel-based superalloy thick-walled tube blanks.
[0092] Comparative Example 4 (Shortening the heat preservation time) Elbows of the same specifications (OD474mm×75mm) were prepared using iron-nickel-based high-temperature alloy tube blanks (outer diameter 508mm, wall thickness 83mm) with the same composition as in Example 1. The forming process was basically the same as in Example 1, except that the holding time for both the controlled heating at the front and the controlled heating at the end was shortened to 0.5min / mm (approximately 41.5min for a wall thickness of 83mm).
[0093] Results: The deformation resistance during flattening was increased compared to Example 1; during pressing, the metal flow on the inner arc side of the elbow was lagging, resulting in local under-pressurization and incomplete mold shape; metallographic analysis showed an overall grain size of 3.0-4.0, with localized grain growth and coarsening to 1.5-2.0; the difference between the maximum and minimum grain size within the same field of view reached 2.0; the coarse-grained region was discontinuously distributed circumferentially, forming localized mixed crystals, with a carbide level of 1; mechanical testing showed that the sample was taken from a part far from the coarse-grained region. The elbow exhibits the following characteristics: room temperature tensile strength approximately 622 MPa, ductile elongation approximately 324 MPa, elongation after fracture approximately 51.5%, reduction of area approximately 62%, impact toughness approximately 112 J, and Brinell hardness approximately 158-164. At 600℃, the tensile strength is approximately 549 MPa, ductile elongation approximately 322 MPa, and elongation after fracture approximately 43.5%. At 700℃, the tensile strength is approximately 519 MPa, ductile elongation approximately 319 MPa, and elongation after fracture approximately 42.0%. The elbow has under-pressure on the inner arc side, incomplete die forming, and the forming quality does not meet the usage requirements. Furthermore, localized mixed crystalline structures are present, rendering the entire elbow unusable.
[0094] It is evident that after the heat preservation time is shortened, the conventional tensile properties such as tensile strength, plastic extension strength and elongation after fracture do not change much, but the impact toughness has dropped to 112J; the uneven deformation caused by insufficient heat penetration in the core of the tube blank has already manifested as underpressure on the inner arc side and incomplete mold shape in the forming stage, and local mixed crystals have appeared in the microstructure, so the elbow is rejected as a whole.
[0095] Comparative Example 5 (front insulation removed) Elbows of the same specifications (OD474mm×75mm) were prepared using iron-nickel-based high-temperature alloy tube blanks (outer diameter 508mm, wall thickness 83mm) with the same composition as in Example 1. The forming process was basically the same as in Example 1, except that the heat preservation after the controlled heating in the first stage was cancelled. That is, the heat preservation was not carried out after the controlled heating in the first stage reached 50°C above the precipitation temperature of the γ´ phase, and the controlled heating in the last stage was directly started.
[0096] Results: The elbow was formed intact, and the deformation resistance during the pressing process was increased compared to Example 1. No defects such as cracks, laps, or folds were observed on the surface. Metallographic examination showed a grain size of 2.0–4.0 grade, with the difference between the maximum and minimum grain size in the same field of view reaching 2.0 grade, indicating a clear mixed-grain structure and a carbide grade of 1. Mechanical testing showed a room temperature tensile strength of approximately 614 MPa, a plastic extension strength of approximately 318 MPa, an elongation after fracture of approximately 47.5%, a reduction of area of approximately 57%, an impact toughness of approximately 103 J, and a Brinell hardness of approximately 156–162. At 600°C, the tensile strength was approximately 533 MPa, the plastic extension strength was approximately 311 MPa, and the elongation after fracture was approximately 39.5%. At 700°C, the tensile strength was approximately 505 MPa, the plastic extension strength was approximately 309 MPa, and the elongation after fracture was approximately 37.5%.
[0097] Although the strength does not change much after the controlled heating is removed, the plasticity is greatly reduced due to the wide-range mixed crystals.
[0098] Comparative Example 6 (Improving the endpoint of controlled temperature rise in the final stage) Elbows of the same specifications (OD474mm×75mm) were prepared using iron-nickel-based high-temperature alloy tube blanks (outer diameter 508mm, wall thickness 83mm) with the same composition as in Example 1. The forming process was basically the same as in Example 1, except that the controlled heating endpoint of the final stage was 230°C above the γ´ phase precipitation temperature (γ´+230°C), and the controlled heating rate and holding time of the final stage were the same as in Example 1.
[0099] Results: The elbow was well-formed, and the deformation resistance during pressing was lower than that in Example 1. No forming defects were observed on the surface. Metallographic examination showed a grain size of 1.5~2.0, with overall coarsening and uniform distribution of grains, no mixed crystals, and a carbide grade of 1. Mechanical testing showed a room temperature tensile strength of approximately 588 MPa, a plastic extension strength of approximately 302 MPa, an elongation after fracture of approximately 49.0%, a reduction of area of approximately 59%, an impact toughness of approximately 92 J, and a Brinell hardness of approximately 149~155. At 600℃, the tensile strength was approximately 512 MPa, the plastic extension strength was approximately 298 MPa, and the elongation after fracture was approximately 41.0%. At 700℃, the tensile strength was approximately 488 MPa, the plastic extension strength was approximately 294 MPa, and the elongation after fracture was approximately 40.0%.
[0100] Although increasing the controlled heating endpoint at the end of the process reduces deformation resistance and improves formability, the grain coarsening is irreversible, and the grain size is already below the lower limit of grade 2.0. The tensile strength at room temperature and at 600℃ and 700℃, as well as the impact toughness at room temperature, are significantly reduced.
Claims
1. A method for manufacturing a thick-walled elbow made of iron-nickel-based high-temperature alloy, comprising a forming process and a heat treatment process, characterized in that: The forming process includes the following steps: Heating: The iron-nickel-based high-temperature alloy raw material billet is subjected to multi-stage controlled heating, including at least a first stage controlled heating and a last stage controlled heating; wherein the initial temperature of the first stage controlled heating is 300~700℃, and the temperature is increased at a rate of 100~200℃ / h to 20~80℃ above the γ´ phase precipitation temperature and held at that temperature for 0.7~1.5min / mm; the last stage controlled heating is increased at a rate of 50~150℃ / h to 120~200℃ above the γ´ phase precipitation temperature and held at that temperature for 0.7~1.5min / mm. Flattening: Flattening the heated raw material tube blank to the middle size; Pressing: The flattened tube blank is pressed with a mold, and the final pressing temperature is not lower than the precipitation temperature of the γ´ phase, followed by cooling.
2. The manufacturing method according to claim 1, characterized in that: The initial temperature of the controlled heating in the front section is 400~600℃, the heating rate is 120~170℃ / h, the temperature is raised to 40~70℃ above the γ´ phase precipitation temperature, and the holding time is 0.7~1.3min / mm.
3. The manufacturing method according to claim 1, characterized in that: The controlled heating rate in the final stage is 70~150℃ / h, the temperature is raised to 130~180℃ above the γ´ phase precipitation temperature, and the holding time is 0.7~1.3min / mm.
4. The manufacturing method according to claim 1, characterized in that: The outer diameter of the intermediate dimension is 0.93 to 0.99 times the outer diameter of the raw material tube blank.
5. The manufacturing method according to claim 1, characterized in that: The ratio of the wall thickness t of the raw material tube blank to its outer diameter D is t / D ≥ 0.
1.
6. The manufacturing method according to claim 1, characterized in that: The heat treatment process after the elbow is formed includes at least a first-stage heating and a second-stage heating; wherein the first-stage heating starts at a temperature of 200~500℃, the heating rate is 100~200℃ / h, the temperature is raised to 20~60℃ above the γ´ phase precipitation temperature and held for 0.7~1.5min / mm; the second-stage heating raises the temperature at a rate of 50~150℃ / h to 80~150℃ above the γ´ phase precipitation temperature and holds for 0.7~1.5min / mm, followed by cooling.
7. The manufacturing method according to claim 6, characterized in that: The heating rate of the first stage is 130~170℃ / h, heating to 40~60℃ above the γ´ phase precipitation temperature, and holding at that temperature for 0.8~1.3min / mm. The heating rate of the second stage is 70~140℃ / h, heating to 80~120℃ above the γ´ phase precipitation temperature, and holding at that temperature for 0.8~1.3min / mm, followed by water cooling.
8. The manufacturing method according to claim 1, characterized in that: The iron-nickel-based superalloy comprises the following components by weight percentage: Fe 35~45%, Cr 15~21%, Mo 0.5~1.4%, W 0.1~0.8%, Ti 1.8~2.5%, Al 0.8~2.5%, Mn≤1.0%, Nb≤0.1%, Co≤2%, Si≤0.05%, C 0.03~0.10%, B 0.001~0.005%, P≤0.01%, with the balance being Ni; The weight percentage of Cr+Ni is greater than 50%, and the weight percentage of W+Mo is 0.6~1.5%.
9. A thick-walled elbow made of iron-nickel-based high-temperature alloy, manufactured by any one of claims 1 to 8.
10. The iron-nickel-based high-temperature alloy thick-walled elbow according to claim 9, characterized in that: The elbow has a grain size of 2.0~5.0, is free of mixed crystals, and has a room temperature tensile strength Rm of not less than 600MPa and a plastic elongation strength Rp. 0.2 Not less than 280MPa, elongation after fracture not less than 48%, and room temperature impact toughness KV2 not less than 130J.
Citation Information
Patent Citations
Manufacturing method of nickel-based alloy large-diameter thick-wall seamless hot-pressing elbow and elbow
CN116079347A
A Method for Medium-Frequency Bending of Thick-Walled Pipes Made of GH4070P Nickel-Iron-Based Superalloy
CN116372508B
Nickel-iron-based high-temperature alloy material and aging treatment method thereof
CN119307836A