By employing a multi-stage controlled heating, multiple pressing, and two-stage heat treatment method, the problems of grain control and thin-wall instability in the forming process of iron-nickel-based high-temperature alloy elbows have been solved, resulting in elbow products with high-temperature strength and oxidation resistance, suitable for high-temperature pipeline systems in thermal power, nuclear power, and petrochemical fields.

CN123149302APending Publication Date: 2026-11-24HEBEI YADU PIPELINE EQUIP GROUP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611654052.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies cannot precisely control the grain structure of iron-nickel-based high-temperature alloy elbows during the multiple heating processes of staged forming, leading to thin-walled structural instability and the formation of mixed-grain structures. This makes it difficult to obtain elbow products with uniform structure and reliable performance, thus limiting their application in high-end pipeline systems.

Method used

A multi-stage controlled heating and multi-stage pressing method is adopted, combined with an internal support structure and two-stage heat treatment, to control the grain structure, prevent thin-wall instability, and ensure the uniformity of the structure and plasticity reserve during the forming process.

Benefits of technology

Precise grain control of large-diameter, thin-walled iron-nickel-based high-temperature alloy elbows has been achieved, preventing thin-wall instability and obtaining elbow products without mixed crystals. These products possess high-temperature strength, oxidation resistance, and structural stability, making them suitable for high-temperature pipeline systems in thermal power, nuclear power, and petrochemical fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149302A_ABST
    Figure CN123149302A_ABST
Patent Text Reader

Abstract

This invention discloses a method for manufacturing an iron-nickel-based high-temperature alloy elbow and the elbow manufactured therefrom, belonging to the field of hot forming of metal elbows. The elbow forming process of this method includes staged heating and staged pressing, wherein the staged heating includes at least an initial heating and a final heating, and the staged pressing includes at least an initial pressing and a final pressing. The initial heating employs multi-stage controlled heating. This invention also discloses an elbow manufactured by the above method. The manufacturing method of this invention can achieve precise control of grain size, prevent thin-wall instability, and maintain production efficiency, resulting in an iron-nickel-based alloy elbow that possesses high-temperature strength, oxidation resistance, and structural stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hot forming technology for alloy elbows, specifically to a method for manufacturing an iron-nickel-based high-temperature alloy elbow and the elbow manufactured therefrom, which is particularly suitable for manufacturing large-diameter, thin-walled iron-nickel-based high-temperature alloy elbows. Background Technology

[0002] Iron-nickel-based superalloys, due to their excellent high-temperature strength, oxidation resistance, and microstructural stability, have significant application prospects in high-end equipment fields such as ultra-supercritical thermal power, nuclear power, and petrochemicals. These alloys belong to the solid solution strengthening and precipitation strengthening type of superalloys, and do not undergo allotropic transformation. Their mechanical properties and service life are highly sensitive to grain size and the size and distribution of the γ' phase; the uniformity of grain size directly determines the service reliability of the final product. The ability to precisely control the grain structure during hot working is a key prerequisite for the successful fabrication of various pipe components from these alloys.

[0003] In high-temperature pressure piping systems, elbows are essential components for changing flow direction, and their forming quality directly determines the overall safety and service life of the piping system. Larger diameters and thinner walls are inevitable trends in the design of pipelines for large-capacity, high-parameter units. Larger diameters meet the demands of high-flow-rate transport, while thinner walls help reduce the overall weight and thermal stress of the pipeline. Large-diameter thin-walled elbows typically refer to elbows with an outer diameter OD ≥ 400 mm and a wall thickness t to outer diameter ratio t / D < 0.15. Due to the thin wall thickness and large diameter of the tube blank, and the high high-temperature deformation resistance of iron-nickel-based alloys, with a hot working window typically only 100~200℃, the hot working process faces multiple superimposed effects of material properties and geometric characteristics, making the forming difficulty significantly higher than that of conventional elbows.

[0004] Firstly, there is a contradiction between the heating rate and grain control. Iron-nickel-based alloys have low thermal conductivity. Large-diameter tube blanks have high heat capacity, but thin walls dissipate heat quickly, resulting in a significant temperature difference between the inner and outer walls during heating. During rapid heating, the outer wall passes through the sensitive temperature zone between the γ' phase precipitation temperature and the dissolution temperature before the inner wall, leading to asynchronous cross-sectional microstructure and the formation of a mixed-grain structure. While slowing down the heating can reduce the cross-sectional temperature difference, it prolongs the residence time within the sensitive temperature zone. The primary γ' phase at the grain boundaries preferentially dissolves and loses its pinning effect. Simultaneously, γ' particles mature, their pinning ability decreases, and their distribution becomes uneven. Adjacent grains lose mutual restraint, significantly increasing the inconsistency in grain growth and again forming a mixed-grain structure. The maturation of the γ' phase and the coarsening of the grains cannot be reversed by subsequent heat treatment; they can only be refined by reintroducing plastic deformation.

[0005] Secondly, there is a contradiction between deformation and thin-walled instability. Thin-walled structures have low stiffness, and their resistance to instability decreases further under hot conditions. When subjected to a large deformation during pressing, the pipe wall is prone to wrinkling and collapse, resulting in excessive local thinning.

[0006] Third, the contradiction of grain inheritance in multi-pass forming. Due to the limitation of deformation amount in a single pass, forming must be completed in multiple pressings. The intermediate billet must be reheated to the forming temperature and kept warm. Each reheating is a window for grain growth. The risk of refined grains growing again during reheating accumulates with the number of heating cycles.

[0007] In the prior art, Chinese patent application CN114130873A discloses a forming method for large-diameter thin-walled elbows, which also addresses the instability problem in the forming of thin-walled elbows. However, it is designed for carbon steel and alloy steel materials, which differ significantly from iron-nickel-based high-temperature alloys in terms of high-temperature deformation behavior, hot working window, and grain control requirements. Therefore, its forming process is difficult to directly apply to these alloys. Chinese patent CN116372508B discloses a high-temperature alloy pipe bending forming method, but this method is designed for thick-walled products and does not address the instability problem during the pressing of thin-walled tube blanks, making it difficult to solve the wrinkling and collapse defects caused by insufficient stiffness in thin-walled structures. Regarding the heating regime, Chinese patent application CN119307836A discloses a heat treatment method for nickel-iron-based alloys. The heating rate for both heat treatments is 5~20℃ / min, i.e., 300~1200℃ per hour, which is considered rapid heating. The heating orientation provided is rapid heating in the range above the γ´ phase dissolution temperature, followed by a sufficiently long holding time to make the microstructure more uniform. It is evident that existing technologies in the direction of elbow forming target the forming force and geometric accuracy, while in the direction of alloy heating target the homogenization of the microstructure during the heat treatment process. Neither of these heating processes takes the grain structure as the control target, and both are single continuous heating processes, without involving the microstructure control of the deformation formed by multiple pressing and the reheating process during the cooling cycle.

[0008] Therefore, existing processes cannot coordinate the heating process between multiple heating stages in the forming process, ensuring that each heating and pressing stage complements each other. This makes it difficult to maintain uniform cross-sectional microstructure and forming plasticity while suppressing uneven grain growth, resulting in a lack of stable production of elbow products with uniform microstructure and reliable performance. This has become a key bottleneck restricting the engineering application of iron-nickel-based superalloys in high-end pipeline systems. Developing a manufacturing method for iron-nickel-based superalloy elbows that can simultaneously achieve precise control of grain microstructure and prevent thin-wall instability is crucial to overcoming the bottleneck in the engineering application of this material, and has urgent engineering value and practical significance. Summary of the Invention

[0009] To address the difficulties in hot pressing large-diameter thin-walled elbows made of iron-nickel-based superalloys in existing technologies, caused by the combined effects of a narrow alloy hot working window, poor anti-instability of thin-walled structures, and uneven heat penetration of large billets, this invention provides a manufacturing method for iron-nickel-based superalloy elbows that can simultaneously achieve precise control of grain size, prevent thin-wall instability, and maintain production efficiency, resulting in iron-nickel-based alloy elbows that possess high-temperature strength, oxidation resistance, and structural stability.

[0010] In order to achieve the objectives of this invention, the following techniques are proposed: This invention provides a method for manufacturing an iron-nickel-based high-temperature alloy elbow, including a forming process and a heat treatment process. The forming process includes heating and pressing the iron-nickel-based high-temperature alloy raw material billet in stages, wherein the stage heating includes at least a first heating and a final heating, and the stage pressing includes at least a first pressing and a final pressing. The initial heating process involves multi-stage controlled heating of the raw material billet, including at least a pre-stage controlled heating and a final stage controlled heating. The initial temperature of the pre-stage controlled heating is 300-700℃, with a heating rate of 100-200℃ / h, heating to 20-80℃ above the γ´ phase precipitation temperature and holding at that temperature for no more than 1.2 min / mm. The final stage controlled heating has a heating rate of 50-150℃ / h, heating to 120-200℃ above the γ´ phase precipitation temperature and holding at that temperature for no more than 1.2 min / mm. The first pressing: After the raw material tube blank is first heated, it is flattened to the intermediate size, and a support structure is installed inside the tube blank. The first mold pressing is then performed to form an intermediate blank. The final heating: the intermediate billet is heated to 120~200℃ above the γ´ phase precipitation temperature and held at that temperature for no more than 1.2 min / mm; The final pressing: the heated intermediate billet is flattened to the finished product size, pressed with a final mold, and then cooled to form an elbow.

[0011] Furthermore, the multi-stage controlled heating is a two-stage controlled heating. The initial temperature of the first stage of controlled heating is 400~600℃, the heating rate is 130~160℃ / h, the temperature is raised to 40~70℃ above the γ´ phase precipitation temperature and held at that temperature for a duration not exceeding 1.2min / mm; the heating rate of the final stage of controlled heating is 80~120℃ / h, the temperature is raised to 130~180℃ above the γ´ phase precipitation temperature and held at that temperature for a duration not exceeding 1.2min / mm.

[0012] Furthermore, the holding time during the first or last heating is 0.5~1 min / mm.

[0013] Furthermore, the final pressing temperature of the first or last mold pressing is not lower than the γ´ phase precipitation temperature.

[0014] Furthermore, the starting temperature of the final heating is not lower than the precipitation temperature of the γ´ phase, the heating rate is 80~120℃ / h, and the temperature of the intermediate billet is not lower than the precipitation temperature of the γ´ phase.

[0015] Furthermore, the outer diameter OD of the raw material tube blank is ≥400mm, and the ratio of wall thickness t to outer diameter OD is t / D <0.15.

[0016] Furthermore, the multi-stage controlled heating does not exceed 3 stages of controlled heating, the staged heating does not exceed 3 times, and the staged pressing does not exceed 3 times.

[0017] Furthermore, the heat treatment of the elbow after forming adopts the following steps: when the temperature is 200~500℃, the heating rate is 100~200℃ / h, the temperature is raised to 20~60℃ above the γ´ phase precipitation temperature and held at that temperature for no more than 1.2min / mm, then the temperature is raised to 80~120℃ above the γ´ phase precipitation temperature at a rate of 50~150℃ / h and held at that temperature for no more than 1.2min / mm, followed by cooling.

[0018] Furthermore, the iron-nickel-based superalloy comprises the following components by weight percentage: Fe 35~45%, Cr 15~21%, Mo 0.5~1.4%, W 0.1~0.8%, Ti 1.8~2.5%, Al 0.8~2.5%, Mn≤1.0%, Nb≤0.1%, Co≤2%, Si≤0.05%, C 0.03~0.10%, B 0.001~0.005%, P≤0.01%, with the balance being Ni; wherein the weight percentage of Cr+Ni is greater than 50%, and the weight percentage of W+Mo is 0.6~1.5%.

[0019] The present invention also provides an iron-nickel-based high-temperature alloy elbow, manufactured by any of the above-mentioned manufacturing methods, wherein the elbow has an outer diameter OD ≥ 400 mm, a wall thickness t to outer diameter OD ratio t / D < 0.15, a grain size of 2.0~5.0 grade, no mixed crystals, a room temperature tensile strength Rm of not less than 600 MPa, and a plastic elongation strength Rp 0.2 The tensile strength at 650℃ is not less than 280 MPa, the elongation after fracture is not less than 50%, and the room temperature impact toughness KV2 is not less than 130 J; and the tensile strength at 650℃ is not less than 500 MPa, and the plastic elongation strength Rp is not less than 130 J. 0.2 The strength is not less than 320 MPa and the elongation after fracture is not less than 45%.

[0020] To facilitate understanding of the technical solution of this invention, the following key terms are explained: The γ' phase precipitation temperature described in this invention: The γ' phase (gamma prime phase) is the main precipitation strengthening phase in iron-nickel-based superalloys, with the chemical formula Ni3(Al,Ti). The γ' phase precipitation temperature refers to the critical temperature at which the γ' phase begins to precipitate from the austenitic matrix, and is usually determined by differential scanning calorimetry (DSC) or phase diagram thermodynamic calculations.

[0021] The multi-stage pressing method described in this invention divides the tube blank forming process into at least two stages: a first pressing (forming an intermediate shape) and a final pressing (completing the final shape). Two pressing stages reduce the amount of deformation per pass, allowing the thin-walled tube blank to deform gradually rather than all at once, preventing instability. This can be extended to three pressing stages: a first, intermediate, and final pressing. The intermediate heating stage is performed before the intermediate pressing stage, and the intermediate heating stage can be the same as the final heating stage. The intermediate pressing stage can also be the same as the first pressing stage, with the size of the intermediate blank decreasing progressively. Generally, no more than three pressing stages are required.

[0022] The controlled heating described in this invention refers to the process of actively controlling the heating rate of the furnace according to a set heating curve, so that the billet heats up with the furnace. Unless otherwise specified, the heating rate, starting temperature, and target temperature of each segment mentioned in this invention are all based on the furnace temperature. After the billet enters the furnace from ambient temperature, the heating rate is not actively controlled when the furnace temperature is lower than the starting temperature of the controlled heating; this segment is not counted in the number of controlled heating segments. From the moment the furnace temperature reaches the starting temperature of the controlled heating, the furnace temperature heats up at the set rate; this segment is counted in the number of controlled heating segments.

[0023] The multi-stage controlled heating described in this invention refers to dividing the controlled heating process of the tube blank into at least two stages: a front stage and a final stage, with different heating rates and / or target temperatures in each stage. In terms of the number of controlled heating stages, multi-stage controlled heating is based on two stages: a front stage controlled heating and a final stage controlled heating, i.e., two-stage controlled heating; it can be extended to a three-stage system: a front stage controlled heating, a middle stage controlled heating, and a final stage controlled heating.

[0024] The support structure described in this invention is a structural component placed inside the tube blank during the pressing process to prevent thin-walled collapse and instability. It may include supports distributed along the inner wall (such as core supports), end supports (such as end braces), internal mandrels, etc. Those skilled in the art can select a suitable support structure according to actual needs.

[0025] The final pressing temperature mentioned in this invention refers to the actual temperature of the tube blank when the die pressing is completed.

[0026] The elbows described in this invention include, but are not limited to, 45° elbows, 90° elbows, 180° elbows, long-radius elbows, and short-radius elbows.

[0027] The intermediate dimension mentioned in this invention refers to the outer diameter of the tube blank after flattening, which is between the outer diameter of the finished elbow and the outer diameter of the raw tube blank. When the pressing is performed in two stages (first and last), there is one intermediate dimension; when the pressing is performed in three stages (first, middle, and last), there are two intermediate dimensions, which decrease progressively. The intermediate dimension is selected based on the principle that the deformation in a single pass does not exceed the stability limit of the thin-walled tube blank, and is determined according to the outer diameter of the tube blank before flattening, the ratio of wall thickness to outer diameter, and the bending angle and bending radius of the elbow. As a preferred embodiment, the reduction in the outer diameter of the tube blank after flattening (i.e., the intermediate dimension) relative to the outer diameter before flattening is 0.3% to 5%.

[0028] Compared with the prior art, the technical solution of the present invention achieves the following overall effects: This invention uses the γ´ phase precipitation temperature as the anchor for each heating step in the microstructure forming process, incorporating temperature anchoring, heating rate, holding time, and pressing passes into the same grain control system. This allows for the simultaneous achievement of three previously mutually restrictive goals: precise control of grain structure, prevention of thin-wall instability, and consideration of process efficiency. Specific effects are as follows.

[0029] The invention employs a segmented controlled heating process, consisting of a pre-stage and a post-stage heating. The pre-stage heating is controlled to a temperature 20-80°C above the γ' phase precipitation temperature and held there, establishing γ' phase pinning at the grain boundaries. The post-stage heating is controlled to pass through the sensitive temperature zone at a rate of 50-150°C / h, reaching a temperature 120-200°C above the γ' phase precipitation temperature, with each stage holding for no more than 1.2 min / mm. Temperature anchoring, heating rate, and holding limit are all crucial and interconnected: anchoring ensures the grain boundaries are pinned throughout the subsequent heating process; the controlled rate ensures the inner and outer walls of the tube blank pass through the sensitive temperature zone nearly synchronously; and the holding limit halts the γ' phase maturation process. If only the heating is slowed down without temperature anchoring and holding constraints, γ' particles will mature, pinning will fail, and their distribution will be uneven, resulting in mixed crystals. If only cross-sectional synchronization is pursued without a pinning establishment stage, the uneven grain growth during the period when the outer wall loses pinning cannot be suppressed.

[0030] The controlled heating rate range in the final stage is defined by two opposing physical constraints. Its upper limit is determined by the cross-sectional synchronization requirement: the thermal conductivity of iron-nickel-based superalloys is approximately one-third to one-quarter that of carbon steel; large-diameter thin-walled tube blanks have large heat capacity but rapid heat dissipation due to their thin walls, resulting in a significant temperature difference between the inner and outer walls. If the rate is too high, the outer wall crosses the sensitive temperature zone before the inner wall, leading to asynchronous cross-sectional microstructure. Its lower limit is determined by the γ' phase ripening behavior: if the rate is too low, the residence time in the sensitive temperature zone is prolonged, resulting in γ' particle ripening, pinning failure, and uneven distribution. Each end of the rate range is determined by an independent physical constraint, not by a choice of values ​​within a known rate range, but by the anchoring benchmark set at the γ' phase precipitation temperature, a necessary result jointly determined by cross-sectional synchronization and ripening constraints. Heating based on the γ' phase dissolution temperature occurs within the single-phase region, where there are no conditions for pinning microstructure establishment; the heating rate is only constrained by heat transfer and efficiency.

[0031] This invention addresses the instability problem of large-diameter, thin-walled tube blanks during hot pressing by employing a multi-stage pressing process combined with a support structure. The first pressing only completes partial deformation, keeping the deformation within a safe range for tube blank stability, while the support structure constrains non-uniform deformation in the thin-walled sections. The final pressing completes the remaining deformation under the condition that the intermediate blank already possesses an initial bend shape, significantly improving the geometric stability of the tube blank. Simultaneously, the plastic deformation introduced by the first pressing refines the grains and homogenizes the microstructure of the intermediate blank through recrystallization, providing a microstructural basis for subsequent heating stages.

[0032] The starting temperature of the final heating in this invention is no lower than the precipitation temperature of the γ' phase. Starting directly from this temperature eliminates the need for a slow initial heating process. The temperature is then raised at a controlled rate to 120-200°C above the γ' phase precipitation temperature and held at this temperature. This reduces the risk of mixed crystals introduced by repeated heating and shortens the reheating cycle. This effect depends on the conditions created by the pressing process: the deformation and recrystallization during the first pressing refines the grains of the intermediate billet. The fine-grained structure increases its tolerance to the heating rate, allowing the final heating to avoid mixed crystal formation without the need for a slow initial heating. Conversely, segmented, rate-controlled heating provides the final pressing with an intermediate billet that is uniform in structure and has sufficient plasticity reserves, preventing instability during the final pressing and ensuring that deformation is concentrated on geometric shaping without inducing structural deterioration. Heating and pressing are thus mutually conditional: the heating regime is predicated on the structural changes introduced by the pressing passes, and the pressing regime is based on the structural state provided by the heating regime. If either deviates from this condition, the other loses its prerequisite.

[0033] This invention further achieves the connection between residual stress elimination and full solution treatment through a two-stage heat treatment: the first stage is low-temperature holding, which eliminates the residual stress introduced by the pressing process without significant grain growth; the second stage is high-temperature holding, which yields elbow products with uniform microstructure and excellent comprehensive mechanical properties. The residual stress introduced by the forming process is precisely the object of heat treatment, and the grain refinement effect of the forming process provides the microstructure basis for heat treatment. The heat treatment regime is logically connected with the preceding forming process.

[0034] This invention provides a method for stably manufacturing large-diameter, thin-walled iron-nickel-based high-temperature alloy elbows. The resulting elbows have a grain size of 2.0~5.0 and are free of mixed grains. The finished product meets the requirements for dimensional accuracy and non-destructive testing. The room temperature tensile strength Rm is not less than 600MPa and the plastic elongation strength Rp is not less than 600MPa. 0.2 Not less than 280MPa, elongation after fracture not less than 50%, room temperature impact toughness KV2 not less than 130J, tensile strength Rm at 650℃ not less than 500MPa, and plastic elongation strength Rp 0.2 With a strength of not less than 320 MPa and an elongation after fracture of not less than 45%, the nickel-iron-based superalloy with fine and uniform grains achieves excellent high-temperature strength through the synergistic effect of grain boundary strengthening and precipitation strengthening. Its grain boundary migration driving force is small and its grain growth tendency is low, which makes the microstructure stable for a long time. The fine grain surface is also conducive to the formation and adhesion of a dense oxide film, thus delaying high-temperature oxidation. The elbows made from this alloy have high-temperature strength, oxidation resistance and microstructure stability, and can be used reliably for a long time under high temperature and high pressure conditions of 650℃ and above. They are suitable for high-temperature pipeline systems in thermal power, nuclear power, petrochemical and other fields. Attached Figure Description

[0035] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.

[0036] Figure 1 This is a process flow diagram of the manufacturing method of the present invention.

[0037] Figure 2 This is a schematic diagram of the segmented temperature rise curve during the first heating in Example 1.

[0038] Figure 3 This is a cross-sectional view of the tube blank after the support structure was installed during the first pressing in Example 1.

[0039] Figure 4 This is a cross-sectional view of the tube blank being moved onto the press during the first pressing in Example 1, in preparation for die pressing.

[0040] Figure 5 This is a cross-sectional view of the tube blank after it has been pressed by a mold in the first pressing of Example 1.

[0041] Figure 6 The two-stage temperature-time curves of the heat treatment in Example 1 are shown.

[0042] Figure 7 Metallographic micrograph of the center of wall thickness of the finished elbow prepared in Example 1.

[0043] Figure 8 Metallographic microstructure of the inner surface of the finished elbow prepared in Example 1.

[0044] Figure 9 Metallographic micrograph of the outer surface of the finished elbow prepared in Example 1.

[0045] Figure 10 Metallographic microstructure of the finished elbow prepared for Comparative Example 1.

[0046] In the diagram: 1 is the tube blank, 2 is the core support, 3 is the end support, 4 is the press head, and 5 is the mold. Detailed Implementation

[0047] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0048] The technical problem this invention aims to solve stems from the contradiction between the material properties of iron-nickel-based superalloys and the structural characteristics of large-diameter thin-walled elbows in the same forming process. Iron-nickel-based superalloys do not undergo allotropic transformation; grain refinement can only be achieved through recrystallization during hot deformation. The refined grains will irreversibly grow in each subsequent heating. However, the deformation amount of large-diameter thin-walled elbows in a single operation is limited by the stability of the thin-walled structure, requiring multiple pressing operations, which necessitates multiple heating operations. Therefore, under the condition of multiple pressing, repeated heating of the intermediate billet is unavoidable. For precipitation-strengthened alloys, repeated heating again crosses the sensitive temperature range where the γ' phase precipitation temperature is located, causing asynchrony between pinning and recrystallization, leading to a mixed-grain structure. The number of heating operations thus becomes a microstructural variable as important as deformation.

[0049] Regarding the aforementioned obstacles, using known technical solutions in the field, whether it is a slow overall heating, a rapid overall heating, or a limited holding time, it is impossible to avoid crystal mixing.

[0050] This invention employs a multi-stage controlled heating process: In the low-temperature zone below the γ' phase precipitation temperature, the first stage involves rapid controlled heating to minimize prolonged dwell time in the low-temperature phase; in the zone approaching the γ' phase precipitation temperature, the final stage involves controlled heating, ensuring uniform temperature penetration across the cross-section of the large-diameter thin-walled tube blank during repeated heating, simultaneous passage of the sensitive temperature zone across both the inner and outer walls, and consistent pinning. The maturation process of the γ' phase is halted with a holding temperature not exceeding 1.2 min / mm. Furthermore, the final heating eliminates the need for the slow initial heating, directly targeting temperatures 120°C to 200°C above the γ' phase precipitation temperature. Leveraging the microstructure homogeneity established during the first heating and the refinement effect of deformation recrystallization introduced by the first pressing, the risk of mixed crystals during repeated heating is reduced. Residual stress introduced during the forming process is addressed by a two-stage heat treatment after forming: the first stage involves holding at a low temperature of 20°C to 60°C above the γ' phase precipitation temperature to release residual stress before significant grain growth; the second stage involves heating to a higher temperature for complete solution solidification.

[0051] As can be seen from the above process, the multi-stage controlled heating, multi-stage pressing, internal support structure, multi-stage heating and two-stage heat treatment are not independent processes in this invention, but rather a coordinated whole: heating provides a uniform structure and sufficient plasticity reserve for pressing, the deformation introduced by pressing provides a basis for grain refinement for subsequent heating, and the structural effects of heating and pressing together determine the initial structure of heat treatment.

[0052] The present invention will be further described below with reference to embodiments.

[0053] Example 1 (Preparation of an OD711mm×50mm elbow) The composition of the iron-nickel-based superalloy in this embodiment, by weight percentage, includes: Fe 35%, Cr 15%, Mo 0.5%, W 0.1%, Ti 1.8%, Al 0.8%, Mn 1.0%, Nb 0.1%, Co 2%, Si 0.05%, C 0.03%, B 0.001%, P 0.01%, with the balance being Ni; the weight percentage of Cr+Ni is 58.6%, and the weight percentage of W+Mo is 0.6%.

[0054] A 90° elbow with an OD of 711mm × 50mm (t / D ≈ 0.0703) is prepared using an iron-nickel-based superalloy with the aforementioned composition; the process flow is as follows. Figure 1 As shown.

[0055] Tube blank preparation: Provide an iron-nickel-based high-temperature alloy tube blank with the above composition, an outer diameter of 770 mm, a wall thickness of 55 mm, and t / D≈0.071.

[0056] Initial heating: such as Figure 2 The diagram shows a regenerative chamber natural gas heater with the tube blank bottom raised by 30cm. Below 500℃, the heating rate is not controlled. Starting from 500℃, the initial heating is controlled at 150℃ / h to 50℃ above the γ´ phase precipitation temperature (γ´+50℃), and held for 0.8min / mm. Subsequently, the final heating is controlled at 100℃ / h to 150℃ above the γ´ phase precipitation temperature (γ´+150℃), and held for 0.6min / mm. Figure 2 In the middle section, m1 represents the time required for the controlled heating in the first stage to rise from 500℃ to γ´+50℃; m2 represents the time required for the controlled heating in the last stage to rise to γ´+150℃.

[0057] Initial pressing: After the tube blank exits the furnace, it is flattened to the intermediate size using a 5000-ton press, with an outer diameter of 762mm. A support structure is then installed (core supports distributed along the inner wall, and end supports placed at the tube blank ends). Figures 3-5 As shown, the first die pressing was performed on a 3200T press using a 762 die. The final pressing temperature was about 27°C above the γ´ phase precipitation temperature. The core support and end support were then removed to form an intermediate billet.

[0058] Final heating: The furnace chamber has been preheated to 50°C above the γ´ phase precipitation temperature. The intermediate billet is immediately placed into the furnace after final pressing. The temperature of the intermediate billet is about 27°C above the γ´ phase precipitation temperature. The temperature is increased to 150°C above the γ´ phase precipitation temperature at a rate of 100°C / h, and held for 1 min / mm.

[0059] Final pressing: After the intermediate billet exits the furnace, it is flattened to the finished size using a 5000-ton press with an outer diameter of 711mm. Then, it is pressed in the final mold using a 711 mold on an 8000-ton press. The final pressing temperature is about 60°C above the γ´ phase precipitation temperature. It is then cooled to room temperature to form a finished billet with an OD of 711mm × 50mm and a 90° bend. The cooling method is water quenching.

[0060] Heat treatment: such as Figure 6 As shown, the temperature was increased from 300℃ to 50℃ (γ´+50℃) above the γ´ phase precipitation temperature at a rate of 150℃ / h, and held for 0.8 min / mm. Then, the temperature was increased to 100℃ (γ´+100℃) above the γ´ phase precipitation temperature at a rate of 100℃ / h and held for 1 min / mm. Subsequently, the temperature was cooled to room temperature by water quenching. Figure 6 In this context, m1 represents the time required to raise the temperature from 300℃ to γ´+50℃, and m2 represents the time required to raise the temperature to γ´+100℃.

[0061] The results show that the elbow was successfully formed under the conditions of this embodiment; Figure 7 The image shows the metallographic examination of the center of the wall thickness of the finished elbow; the grain size is grade 3.5. Figure 8 The image shows the metallographic examination of the inner surface of the finished elbow, with a grain size of 4.0. Figure 9 The metallographic image shows the outer surface of the finished elbow. The grain size is grade 3.5; the overall carbide grade is grade 1, with no mixed crystals. Mechanical testing shows a room temperature tensile strength Rm = 650 MPa and a plastic elongation strength Rp. 0.2 =309MPa, elongation after fracture A=54.5%, impact toughness KV2=180J, Brinell hardness HBW=161~179; high temperature tensile strength Rm=531MPa, plastic elongation strength Rp 0.2 =347MPa, elongation after fracture A=55.5%, reduction of area 66%; tensile strength at 700℃ Rm=552MPa, plastic elongation strength Rp 0.2 =362MPa, elongation after fracture A=50.5%, mechanical testing qualified; finished product dimensions and non-destructive testing qualified, product toughness and strength are good.

[0062] The detection methods in all embodiments of this invention are the same. Specifically, the metallographic carbide detection uses the method of GB / T 13298-2015; the metallographic grain size detection uses the method of GB / T 6394-2017; the room temperature tensile strength, plastic extension strength, and elongation after fracture are detected using the method of GB / T 228.1-2021; the Brinell hardness is detected using the method of GB / T 231.1-2018; the high temperature tensile strength, plastic extension strength, and elongation after fracture at 650℃ and 700℃ are all detected using the method of GB / T 228.2-2015; and the impact toughness is detected using the method of GB / T 229-2020.

[0063] Example 1a (forming process is the same as Example 1, using conventional heat treatment) A 90° elbow with an OD711mm×50mm diameter was prepared using an iron-nickel-based superalloy with the aforementioned composition. The forming process was exactly the same as in Example 1. The only difference was the heat treatment method: this example used conventional heat treatment, that is, the elbow was directly heated from 300℃ to 100℃ above the γ´ phase precipitation temperature at a rate of 150℃ / h, held at that temperature for 1min / mm, and then water-cooled.

[0064] The results showed that the elbow could be successfully formed, and the product dimensions, shape, and non-destructive testing were all qualified. Metallographic analysis showed that the grain size of the finished elbow was 2.5~3.0 grade (3.5~4.0 grade in Example 1), the carbide grade was 1, and there were no mixed crystals. Mechanical testing showed that the room temperature tensile strength Rm = 630MPa (650MPa in Example 1) and the plastic elongation strength Rp 0.2=301MPa (309MPa in Example 1), elongation after fracture A=50.0% (54.5% in Example 1), reduction of area Z=60% (66% in Example 1), impact toughness KV2=150J (180J in Example 1), Brinell hardness HBW=155~173 (161~179 in Example 1); tensile strength at 650℃ Rm=512MPa, plastic elongation strength Rp 0.2 =338MPa, elongation after fracture A=51.0% (531MPa, 347MPa, and 55.5% respectively in Example 1); tensile strength at 700℃ Rm=533MPa, plastic elongation strength Rp 0.2 =353MPa, elongation at break A=46.0% (Example 1: 552MPa, 362MPa, 50.5% respectively). The product performance is acceptable and meets the usage requirements, but overall it is lower than that of Example 1.

[0065] The comparison between this embodiment and Embodiment 1 shows that, under the condition that the forming process is exactly the same and only the heat treatment regime is different, the grain size of the elbow treated with conventional heat treatment decreases from grade 3.5~4.0 to grade 2.5~3.0, the room temperature tensile strength decreases from 650MPa to 630MPa, the plastic elongation strength decreases from 309MPa to 301MPa, and the elongation after fracture decreases from 54.5% to 50%. It can be seen that the first stage of the two-stage heat treatment of this invention, which involves holding at a low temperature of 20~60°C above the γ´ phase precipitation temperature, releases the residual stress introduced during the pressing process before the grains grow significantly, providing a fine initial structure for the second stage of high-temperature holding, thereby maintaining the grain size.

[0066] Example 2 (Preparation of OD820mm×80mm elbow)

[0067] The composition of the iron-nickel-based superalloy in this embodiment, by weight percentage, includes: Fe 44.0%, Cr 21%, Mo 0.7%, W 0.3%, Ti 2.5%, Al 1.2%, Mn 0.3%, Nb 0.03%, Co 0.4%, Si 0.01%, C 0.10%, B 0.005%, P 0.003%, with the balance being Ni; the weight percentage of Cr+Ni is 50.45%, and the weight percentage of W+Mo is 1.0%.

[0068] A 90° elbow with an OD of 820mm × 80mm (t / D≈0.0975) was prepared using an iron-nickel-based superalloy with the aforementioned composition. The preparation process is as follows: Figure 1 As shown.

[0069] Tube blank preparation: Provide an iron-nickel-based high-temperature alloy tube blank with the above composition, an outer diameter of 870 mm, a wall thickness of 85 mm, and t / D≈0.0977.

[0070] Initial heating: A regenerative chamber natural gas heater is used, with the bottom of the tube blank raised by 35cm; the heating rate is not controlled below 700℃, and the initial heating is controlled from 700℃, at 200℃ / h to 80℃ above the γ´ phase precipitation temperature, and held for 1.2min / mm; then the final heating is controlled at 150℃ / h to 200℃ above the γ´ phase precipitation temperature, and held for 1.2min / mm.

[0071] First pressing: After the tube blank is taken out of the furnace, it is flattened to the intermediate size with an outer diameter of 866mm using a 5000-ton press. The support structure is then installed (the core support is distributed along the inner wall, and the end support is placed at the end of the tube blank). The first die pressing is performed on a 3200T press using an 866 die. The final pressing temperature is about 50°C above the γ´ phase precipitation temperature. The core support and end support are then removed to form the intermediate blank.

[0072] Final heating: The furnace chamber has been preheated to 50°C above the γ´ phase precipitation temperature. The intermediate billet is immediately placed into the furnace after final pressing. The temperature of the intermediate billet is about 50°C above the γ´ phase precipitation temperature. The temperature is increased to 200°C above the γ´ phase precipitation temperature at a rate of 120°C / h, and held for 1.2 min / mm.

[0073] Final pressing: After the intermediate billet exits the furnace, it is flattened to the finished size using a 5000-ton press with an outer diameter of 820mm. Then, it is pressed in the final mold using an 820 mold on an 8000-ton press. The final pressing temperature is about 100°C above the γ´ phase precipitation temperature. It is then quenched with water to form a finished billet with an OD of 820mm × 80mm and a 90° bend.

[0074] Heat treatment: Heat the temperature from 500℃ to 60℃ above the γ´ phase precipitation temperature at a rate of 200℃ / h, hold for 1.2 min / mm, then heat the temperature to 120℃ above the γ´ phase precipitation temperature at a rate of 150℃ / h, hold for 1.2 min / mm, and then quench with water.

[0075] The results show that the elbow was successfully formed under the conditions of this embodiment; metallographic examination revealed that the grain size at the center of the wall thickness was grade 3.5, the grain size on the inner surface was grade 4.0, the grain size on the outer surface was grade 3.0, the overall grain size was grade 3.0-4.0, the carbide grade was grade 1, and there were no mixed crystals; mechanical testing showed that the room temperature tensile strength Rm = 629 MPa and the plastic elongation strength Rp 0.2 =300MPa, elongation after fracture A=53%, reduction of area Z=64%, impact toughness KV2=210J, Brinell hardness HBW=156~172; high temperature at 650℃ Rm=540MPa, plastic tensile strength Rp 0.2 =353MPa, elongation after fracture A=54.0%; high temperature at 700℃ Rm=562MPa, plastic tensile strength Rp 0.2=373MPa, elongation after fracture A=49.0%; mechanical testing qualified; finished product dimensions and non-destructive testing qualified.

[0076] Example 3 (Preparation of OD615mm×30mm elbow)

[0077] The composition of the iron-nickel-based superalloy in this embodiment, by weight percentage, includes: Fe 40%, Cr 17%, Mo 0.9%, W 0.6%, Ti 2%, Al 2.5%, Mn 0.8%, Nb 0.07%, Co 1.6%, Si 0.03%, C 0.07%, B 0.003%, P 0.006%, with the balance being Ni; the weight percentage of Cr+Ni is 51.42%, and the weight percentage of W+Mo is 1.5%.

[0078] A 90° elbow with an OD of 615mm × 30mm (t / D ≈ 0.049) was prepared using an iron-nickel-based superalloy with the aforementioned composition. The preparation process is as follows: Figure 1 As shown.

[0079] Tube blank preparation: Provide an iron-nickel-based high-temperature alloy tube blank with the above composition, an outer diameter of 660 mm, a wall thickness of 35 mm, and t / D≈0.053.

[0080] Initial heating: A regenerative chamber natural gas heater is used, with the bottom of the tube billet raised by 25cm; the heating rate is not controlled below 300℃, and the initial heating is controlled from 300℃, at 100℃ / h to 20℃ above the γ´ phase precipitation temperature, and held for 0.5min / mm; then the final heating is controlled at 50℃ / h to 120℃ above the γ´ phase precipitation temperature, and held for 0.5min / mm.

[0081] First pressing: After the tube blank is taken out of the furnace, it is flattened to the intermediate size with an outer diameter of 655mm using a 5000-ton press. The support structure is then installed (the core support is distributed along the inner wall, and the end support is placed at the tube blank port). The first die pressing is performed on a 3200T press using a 655 mold. The final pressing temperature is the γ´ phase precipitation temperature. The core support and end support are then removed to form the intermediate blank.

[0082] Final heating: The furnace chamber has been preheated to 50°C above the γ´ phase precipitation temperature. The intermediate billet is immediately placed into the furnace after final pressing. The temperature of the intermediate billet is the γ´ phase precipitation temperature. The temperature is increased to 120°C above the γ´ phase precipitation temperature at a rate of 80°C / h, and held for 0.5 min / mm.

[0083] Final pressing: After the intermediate billet exits the furnace, it is flattened to the finished size using a 5000-ton press with an outer diameter of 615mm. Then, it is pressed in the final mold using a 615 mold on an 8000-ton press. The final pressing temperature is approximately the γ´ phase precipitation temperature. Subsequently, it is quenched with water to form a finished billet with an OD of 615mm × 30mm and a 90° bend.

[0084] Heat treatment: Increase the temperature from 200℃ to 20℃ above the γ´ phase precipitation temperature at a rate of 100℃ / h, hold for 0.5 min / mm, then increase the temperature to 80℃ above the γ´ phase precipitation temperature at a rate of 50℃ / h, hold for 0.5 min / mm, quench with water, and remove from the furnace and immerse completely in water for about 80 seconds.

[0085] The results show that the elbow was successfully formed under the conditions of this embodiment; metallographic examination revealed that the grain size at the center of the wall thickness was grade 4.0, the inner surface grain size was grade 4.5, the outer surface grain size was grade 3.5, the overall grain size was grade 3.5-4.5, the carbide grade was grade 1, and there were no mixed crystals; mechanical testing showed that the room temperature tensile strength Rm = 634 MPa and the plastic elongation strength Rp 0.2 =301MPa, elongation after fracture A=51%, reduction of area Z=62%, impact toughness KV2=147J, Brinell hardness HBW=158~174; high temperature at 650℃ Rm=548MPa, plastic tensile strength Rp 0.2 =365MPa, elongation after fracture A=52.0%; high temperature at 700℃ Rm=570MPa, plastic tensile strength Rp 0.2 =390MPa, elongation after fracture A=47.0%; mechanical testing qualified; finished product dimensions and non-destructive testing qualified.

[0086] Examples 4 to 6

[0087] Examples 4 to 6 use iron-nickel-based high-temperature alloys with the composition described in Example 1. The raw material tube blanks and the dimensions of the elbows prepared in each example are as follows: Example 4: A 90° elbow with an OD508mm×54mm (t / D≈0.106) was prepared from an iron-nickel-based high-temperature alloy tube blank with an OD550mm×60mm. Example 5: A 90° elbow with an OD of 739mm × 104mm (t / D≈0.141) was prepared from an iron-nickel-based high-temperature alloy tube blank with an OD of 800mm × 115mm. Example 6: A 90° elbow with an OD711mm×48mm (t / D≈0.068) was prepared from an iron-nickel-based high-temperature alloy tube blank with an OD770mm×53mm. The manufacturing steps of Examples 4 to 6 are the same as those of Example 1, and the parameters for each stage are shown in Table 1.

[0088] Table 1. Process parameters and test results for Examples 1 and 4 to 6

[0089] Under the conditions of Examples 4 to 6, the elbows can be successfully formed, and the metallographic test, mechanical property test, finished product dimensions and non-destructive testing are all qualified.

[0090] Example 7 (Preparation of an OD711mm×50mm elbow by three heating and three pressing processes) This embodiment uses an iron-nickel-based superalloy with the composition described in Example 1 to prepare a 90° elbow with an OD of 711mm × 50mm (t / D≈0.0703). The difference from Example 1 is that the forming process in this embodiment uses three heating and three pressing processes, namely, first heating, second heating, and final heating, as well as first pressing, second pressing, and final pressing.

[0091] Tube blank preparation: Provide an iron-nickel-based high-temperature alloy tube blank with the above composition, an outer diameter of 770 mm, a wall thickness of 55 mm, and t / D≈0.071.

[0092] Initial heating: A regenerative chamber natural gas heater is used, with the bottom of the tube billet raised by 30cm; the heating rate is not controlled below 500℃, and the initial heating is controlled from 500℃, at a rate of 150℃ / h to 50℃ above the γ´ phase precipitation temperature, and held for 0.6min / mm; then the final heating is controlled at a rate of 100℃ / h to 150℃ above the γ´ phase precipitation temperature, and held for 0.5min / mm.

[0093] First pressing: After the tube blank is taken out of the furnace, it is flattened to the intermediate size with an outer diameter of 762mm using a 5000-ton press. The support structure is installed (the core support is distributed along the inner wall and the end support is placed at the end of the tube blank). The first die pressing is carried out on a 3200T press using a 762 die. The final pressing temperature is about 30°C above the γ´ phase precipitation temperature. The core support and end support are removed to form the intermediate blank.

[0094] Secondary heating: The furnace chamber has been preheated to 50°C above the γ´ phase precipitation temperature. The intermediate billet is immediately put into the furnace after final pressing. The temperature of the intermediate billet is about 30°C above the γ´ phase precipitation temperature. The temperature is increased to 150°C above the γ´ phase precipitation temperature at a rate of 100°C / h, and held for 0.6 min / mm.

[0095] Intermediate pressing: After the intermediate billet exits the furnace, it is flattened to the intermediate size using a 5000-ton press with an outer diameter of 736mm. The support structure is then reinstalled (the core support is distributed along the inner wall, and the end support is placed at the port of the intermediate billet). On an 8000-ton press, the intermediate billet is pressed using a 736 die. The final pressing temperature is approximately 40°C above the γ´ phase precipitation temperature. The core support and end support are then removed to form the intermediate billet.

[0096] Final heating: The furnace chamber has been preheated to 60°C above the γ´ phase precipitation temperature. The intermediate billet is immediately placed into the furnace after final pressing. The temperature of the intermediate billet is about 40°C above the γ´ phase precipitation temperature. The temperature is increased to 150°C above the γ´ phase precipitation temperature at a rate of 100°C / h, and held for 0.7 min / mm.

[0097] Final pressing: After the intermediate billet exits the furnace, it is flattened to the finished size using a 5000-ton press with an outer diameter of 711mm. Then, it is pressed in the final mold using a 711 mold on an 8000-ton press. The final pressing temperature is about 60°C above the γ´ phase precipitation temperature. It is then quenched with water to form the finished billet OD711mm×50mm with a 90° bend.

[0098] Heat treatment: Heat the temperature from 300℃ to 50℃ above the γ´ phase precipitation temperature at a rate of 150℃ / h, hold for 0.8 min / mm, then heat the temperature to 100℃ above the γ´ phase precipitation temperature at a rate of 100℃ / h, hold for 1 min / mm, and then quench with water.

[0099] The results show that the elbow was successfully formed under the conditions of this embodiment. Metallographic examination revealed that the grain size at the center of the wall thickness was grade 4.0, the inner surface grain size was grade 4.5, the outer surface grain size was grade 4.0, and the overall grain size was grade 4.0-4.5. The grain size difference between the inner and outer walls of the same cross-section did not exceed grade 0.5, the carbide grade was grade 1, and there were no mixed crystals. Mechanical testing showed that the room temperature tensile strength Rm = 652 MPa and the plastic elongation strength Rp 0.2 =310MPa, elongation after fracture A=54.0%, reduction of area Z=65%, impact toughness KV2=182J, Brinell hardness HBW=162~180; high temperature tensile strength Rm=534MPa, plastic elongation strength Rp 0.2 =348MPa, elongation after fracture A=55.0%; high temperature tensile strength Rm=556MPa, plastic extension strength Rp0.2=363MPa, elongation after fracture A=50.0%; finished product dimensions and non-destructive testing are all qualified.

[0100] Comparative Example 1 (Initial heating with single-stage rapid temperature rise)

[0101] An OD711mm×50mm elbow was prepared using an iron-nickel-based superalloy with the aforementioned composition. The difference lies in the initial heating method: a single-stage rapid heating was used, directly raising the temperature from 500℃ to 150℃ above the γ´ phase precipitation temperature at a rate of 300℃ / h, without segmented speed control.

[0102] Test results: such as Figure 10 As shown, the finished product has a grain size lower than grade 1, which is below the acceptable range of grade 2.0 to 5.0. Intergranular characteristics are visible in the mixed crystal region. The room temperature tensile strength is 560 MPa, the plastic elongation strength is 252 MPa, the elongation after fracture is 31%, the reduction of area is 42%, the room temperature impact toughness KV2 is 35 J, and the Brinell hardness is 136~154. At 650℃, the tensile strength is 450 MPa, the plastic elongation strength is 275 MPa, and the elongation after fracture is 26.0%. At 700℃, the tensile strength is 468 MPa, the plastic elongation strength is 284 MPa, and the elongation after fracture is 19.0%.

[0103] The above results indicate that after eliminating segmented speed control, the billet passes through the γ´ phase sensitive temperature zone rapidly at 300℃ / h. The outer wall crosses the sensitive temperature zone before the inner wall and loses pinning. Furthermore, there is no heat preservation stage to establish pinning in the heating path, allowing the grains to grow and form mixed crystals without pinning constraints. The finished product's grain size is more than 2.5 grades lower than in Example 1, its impact toughness is 19% of Example 1, its elongation after fracture is reduced by 43%, and its tensile strength at 650℃ and 700℃ is reduced by 15.3% and 15.2%, respectively, with the high-temperature strength reduction being greater than the room-temperature reduction. This alloy does not exhibit allotropic transformation, and the coarsened grains cannot be reversed by subsequent processes. The deformation amounts in the first and last pressing passes are insufficient to completely recrystallize and refine the coarse grains.

[0104] Comparative Example 2 (Initial heating without front-end insulation) An OD711mm×50mm elbow was prepared using an iron-nickel-based superalloy with the aforementioned composition. Except for the initial heating, the remaining steps were the same as in Example 1. The difference was that the initial heating was not segmented; starting from 500℃, the temperature was continuously increased at 150℃ / h, passing 50℃ above the γ' phase precipitation temperature, without holding at that temperature. Then, the temperature was increased at 100℃ / h to 150℃ above the γ' phase precipitation temperature and held for 0.6 min / mm.

[0105] Test results: The finished product has a grain size of 2.5~3.0 grade, with increased grain size differences within the same field of view. The difference between the largest and smallest grain size is about 1.0 grade, which does not meet the mixed crystal judgment. The room temperature tensile strength is 618MPa, the plastic extension strength is 289MPa, the elongation after fracture is 49%, the reduction of area is 63%, the room temperature impact toughness KV2 is 124J, and the Brinell hardness is 151~169. The 650℃ tensile strength is 503MPa, the plastic extension strength is 325MPa, and the elongation after fracture is 48.0%. The 700℃ tensile strength is 525MPa, the plastic extension strength is 339MPa, and the elongation after fracture is 42.5%. The fracture surface exhibits a ductile transgranular morphology.

[0106] The above results indicate that after eliminating the initial heat preservation stage, there is no pinning establishment stage in the heating path. The grains begin to grow unevenly after exceeding the γ´ phase precipitation temperature. The finished grain size is about one grade lower than that of Example 1, the impact toughness is 69% of that of Example 1, the room temperature tensile strength decreases by 4.9%, and the elongation after fracture decreases by 10%. Compared with Comparative Example 1, this comparative example retains the final stage controlled heating and heat preservation, and the degree of microstructure deterioration is significantly reduced, indicating that the final stage controlled heating and heat preservation cannot replace the pinning establishment effect of the initial heat preservation stage.

[0107] Comparative Example 3 (Front-end insulation exceeds the upper limit) An OD711mm×50mm elbow was prepared using an iron-nickel-based superalloy with the aforementioned composition. Except for the holding time during the controlled heating phase before the initial heating, the remaining steps were the same as in Example 1. The difference was that the holding time during the controlled heating phase before the initial heating, at 50°C above the γ´ phase precipitation temperature, was changed from 0.8 min / mm to 2.0 min / mm; all other parameters remained unchanged.

[0108] Test results: The finished product has a grain size of 2.0~3.0 grade and obvious mixed crystal structure; room temperature tensile strength is 606MPa, plastic elongation strength is 280MPa, elongation after fracture is 42%, reduction of area is 57%, room temperature impact toughness KV2 is 95J, and Brinell hardness is 148~166; at 650℃, tensile strength is 490MPa, plastic elongation strength is 311MPa, and elongation after fracture is 38.5%; at 700℃, tensile strength is 512MPa, plastic elongation strength is 323MPa, and elongation after fracture is 32.0%; the fracture surface is mainly ductile morphology with local intergranular features.

[0109] The above results indicate that extending the initial heat preservation time from 0.8 min / mm to 2.0 min / mm causes the γ´ phase particles to mature during prolonged heat preservation, resulting in decreased pinning ability, uneven distribution, increased inconsistency in grain growth, and the formation of obvious mixed crystals. The finished product grain size decreased by 1-1.5 grades compared to Example 1, the impact toughness was 53% of Example 1, and the elongation after fracture decreased by 23%. This result suggests that a longer initial heat preservation time is not necessarily more beneficial for grain control; its upper limit is determined by the γ´ phase maturation behavior, rather than by the requirement for uniform heat penetration.

[0110] Comparative Example 4 (using rapid heating and long-term heat preservation) An OD711mm×50mm elbow was prepared using an iron-nickel-based superalloy with the aforementioned composition. Except for the initial and final heating, the remaining steps were the same as in Example 1. The difference was that the controlled heating rate at the end of the initial heating and the heating rate at the final heating were both 600℃ / h. After heating to 150℃ above the γ´ phase precipitation temperature, the temperature was held for 1.0h, while all other parameters remained unchanged.

[0111] Test results: The grain size of the intermediate billet after the first pressing was grade 3.5~4.0; before the last pressing, the grain size of the outer wall of the intermediate billet was grade 2.5, and the grain size of the inner wall was grade 3.0~3.5, with a grain size difference of 0.5~1.0 between the inner and outer sides of the same cross section; the grain size of the finished product was grade 2.5~3.0, and the grain size difference between the inner and outer walls was comparable to that before the last pressing; the room temperature tensile strength was 616MPa, the plastic extension strength was 287MPa, the elongation after fracture was 44%, the reduction of area was 61%, the room temperature impact toughness KV2 was 110J, and the Brinell hardness was 150~168; the 650℃ tensile strength was 502MPa, the plastic extension strength was 319MPa, and the elongation after fracture was 41.5%; the 700℃ tensile strength was 524MPa, the plastic extension strength was 331MPa, and the elongation after fracture was 35.5%; the fracture surface was mainly ductile with local intergranular features.

[0112] The above results indicate that the grain size of the intermediate billet after the first pressing is the same as that in Example 1, ranging from 3.5 to 4.0. The microstructure deterioration occurs after the final heating. The final heating involves a rapid temperature rise of 600°C / h and a holding time of 1.0 h, causing the inner and outer walls of the intermediate billet to pass through the sensitive temperature zone at different times, forming a cross-sectional difference of 0.5 to 1.0 grade that persists to the finished product. The grain size of the finished product decreases by 1 to 1.5 grades compared to Example 1, and the impact toughness is 61% of that in Example 1. Under the condition that the initial heating regime and heat treatment regime remain unchanged, the deterioration of the finished product's microstructure is attributed to the heating method of the final heating, indicating that the existing heating orientation of rapid heating combined with hourly holding cannot be transferred to the reheating process.

[0113] Comparative Example 5 (Multi-stage stepped long-term heat preservation during initial heating) An OD711mm×50mm elbow was prepared using an iron-nickel-based superalloy with the aforementioned composition. Except for the initial heating at the final stage, the remaining steps were the same as in Example 1. The difference was that the controlled heating at the final stage of the initial heating started 300°C below the γ' phase precipitation temperature, and was increased in five steps to 150°C above the γ' phase precipitation temperature. Each step increased by 90°C and was held at that temperature for 30 minutes, for a total holding time of approximately 150 minutes. This employed the existing method of gradient heating combined with segmented holding to organize the final stage heating, while all other parameters remained unchanged.

[0114] Test results: The finished product has a grain size of 2.0~2.5; room temperature tensile strength is 601MPa, plastic elongation strength is 276MPa, elongation after fracture is 41%, reduction of area is 56%, room temperature impact toughness KV2 is 86J, and Brinell hardness is 145~163; at 650℃, tensile strength is 486MPa, plastic elongation strength is 303MPa, and elongation after fracture is 37.0%; at 700℃, tensile strength is 508MPa, plastic elongation strength is 314MPa, and elongation after fracture is 30.0%; the fracture surface is mainly ductile morphology, with about one-third intergranular.

[0115] The above results indicate that each stage of the gradient heating is within the sensitive temperature range of the γ´ phase. The cumulative duration of approximately 150 minutes allows the γ´ phase particles to fully mature, resulting in a non-uniform distribution of pinning failure. The proportion of intergranular fracture surfaces is approximately one-third, which corresponds to the inconsistency between the deformation of the mixed-grain structure and the overall structure. This comparative example shows that long-term segmented holding based on the absolute temperature node structure, without targeting the grain structure, also cannot obtain uniform and fine grains.

[0116] Comparative Example 6 (The final heating process involved cooling followed by reheating in the furnace). An OD711mm×50mm elbow was prepared using an iron-nickel-based superalloy with the aforementioned composition. Except for the final heating, the remaining steps were the same as in Example 1. The difference was that the intermediate billet was cooled to room temperature after the initial pressing and then heated in a furnace. The furnace temperature was pre-set to 150°C above the γ´ phase precipitation temperature, and the temperature was increased at 200°C / h and held for 1.2 min / mm. No segmented temperature control was performed, and the initial temperature and heating rate of the intermediate billet upon entering the furnace were not limited.

[0117] Test results: The finished product has a grain size of 2.0~2.5 grade, with local mixed crystal structure; room temperature tensile strength is 600MPa, plastic elongation strength is 279MPa, elongation after fracture is 43%, reduction of area is 58%, room temperature impact toughness KV2 is 88J, and Brinell hardness is 146~164; at 650℃, tensile strength is 478MPa, plastic elongation strength is 310MPa, and elongation after fracture is 39.0%; at 700℃, tensile strength is 497MPa, plastic elongation strength is 322MPa, and elongation after fracture is 32.5%; local intergranular characteristics are visible on the fracture surface.

[0118] The grain size of the product obtained in this comparative example decreased by about 1.5 grades compared with Example 1, and local mixed crystal structure appeared. The impact toughness was 49% of that of Example 1. The tensile strength at 650°C and 700°C decreased by 10.0% and 9.9% respectively, and the decrease in high-temperature strength was greater than that at room temperature.

[0119] Comparative Example 7 (conventional multi-stage heating with limited heat preservation time) An OD711mm×50mm elbow was prepared using an iron-nickel-based superalloy with the aforementioned composition. The forming structure of this comparative example is the same as in Example 1, still including a first heating, a first pressing, a final heating, a final pressing, and a two-stage heat treatment after forming. The holding time for each heating is also exactly the same as in Example 1, with the holding time for the first heating being 0.6 min / mm and the holding time for the final heating being 1 min / mm. The heat treatment regime is the same as in Example 1. The only difference lies in the organization of the heating method: the first heating does not distinguish between the front and rear sections, and the temperature is continuously increased from 500℃ at 200℃ / h to 150℃ above the γ´ phase precipitation temperature, and held at that temperature for 0.6 min / mm; in the final heating, the intermediate billet is still placed into the furnace after final pressing, but its initial temperature and heating rate are not limited, and it is heated at 200℃ / h to 150℃ above the γ´ phase precipitation temperature and held for 1 min / mm. This comparative example simply raises the temperature to the forming temperature and controls the holding time using conventional methods.

[0120] Test results: The grain size of the intermediate billet after the first pressing was 2.5~3.0 grade, with local mixed crystal structure; the grain size of the intermediate billet before the last pressing was 2.0~3.0 grade, and the mixed crystal structure extended to the inner and outer walls of the same cross section; the grain size of the finished product was 2.0~3.0 grade, with local mixed crystal structure, a decrease of about 1~1.5 grade compared to Example 1; room temperature tensile strength was 608 MPa, plastic extension strength was 282 MPa, elongation after fracture was 44%, reduction of area was 59%, room temperature impact toughness KV2 was 102 J, and Brinell hardness was 148~166; at 650℃, tensile strength was 494 MPa, plastic extension strength was 313 MPa, and elongation after fracture was 41.0%; at 700℃, tensile strength was 516 MPa, plastic extension strength was 326 MPa, and elongation after fracture was 35.0%; the fracture surface was mainly ductile morphology with local intergranular features.

[0121] The above results indicate that the holding time for each heating cycle was exactly the same as in Example 1, and the heat treatment regime was also the same. However, the grain size of the finished product decreased by 1 to 1.5 grades compared to Example 1, and mixed grains appeared. The impact toughness was 57% of that in Example 1, the elongation after fracture decreased by 19%, and the tensile strength at 650℃ and 700℃ decreased by 7.0% and 6.5%, respectively. The grain size of the intermediate billet had already decreased to grade 2.5 to 3.0 after the first pressing, and the microstructure deterioration appeared from the first heating and spread to the entire cross-section with the last heating. Under the condition that the holding time did not differ, the deterioration of the finished product's microstructure could only be attributed to the microstructure of the heating process, indicating that the holding time does not constitute an independent grain control mechanism, but its effect depends on the segmented microstructure anchored by the γ´ phase precipitation temperature during the heating process.

[0122] Comparative Example 8 (One-time pressing)

[0123] An OD711mm×50mm elbow is prepared using an iron-nickel-based high-temperature alloy with the aforementioned composition. The difference is that the tube blank undergoes an initial heating and initial pressing, using a finished product mold to press the elbow into a finished product in one step; no final heating or final pressing is performed.

[0124] Test results: The thin-walled portion of the tube blank became unstable and wrinkled during the pressing process; the finished product had a grain size of 2.5~3.5, with localized mixed crystal structures. The mixed crystal zone was distributed along the deformation concentration zone, and the difference between the maximum and minimum grain size in the same field of view reached 2.0; mechanical testing showed a room temperature tensile strength of 625 MPa, a plastic extension strength of 288 MPa, an elongation after fracture of 39%, a reduction of area of ​​55%, a room temperature impact toughness KV2 of 92 J, and a Brinell hardness of 152~170; at 650℃, the tensile strength was 504 MPa, the plastic extension strength was 318 MPa, and the elongation after fracture was 34.5%; at 700℃, the tensile strength was 526 MPa, the plastic extension strength was 330 MPa, and the elongation after fracture was 27.5%; the surface quality of the wrinkled areas did not meet the requirements.

[0125] The above results indicate that the critical deformation for instability in a single pass of the thin-walled tube blank is limited. The total deformation required for a single pressing exceeds this critical value, leading to instability and wrinkling in the thin-walled portion. The presence of mixed-grain structure in the finished product suggests that the intermediate blank's microstructure refinement process was omitted during the single-pass forming. Wrinkling is a geometric defect, while mixed-grain structure cannot be repaired by subsequent heat treatment because the alloy lacks allotropic transformation and the coarsened grains cannot be refined again by heat treatment.

[0126] The results of Examples 1 to 6 and Comparative Examples 1 to 8 show that the temperature control process, heating rate, holding limit, and multi-stage pressing of the present invention have a synergistic effect, rather than being a simple superposition of processes. Comparative Example 1 shows that rapid heating without segmented speed control results in coarse grains that cannot be reversed by subsequent processes; Comparative Examples 2 and 3 show that both the cancellation and extension of the initial holding stage deteriorate the grain structure, and their impact on the grains has a clear value range; Comparative Examples 4 and 5 show that existing heating orientations, such as rapid heating combined with hourly holding or gradient heating combined with long-term segmented holding, cannot obtain a uniform and fine grain structure in the forming process of this alloy; Comparative Example 6 shows that restoring the forming temperature by cooling to room temperature and then returning it to the furnace will cause the intermediate billet to remain in the sensitive temperature range for a long time and lose its pinning; Comparative Example 7 shows that even if the holding time is taken from the values ​​of the present invention, grain growth cannot be suppressed under the condition that the heating method does not make corresponding structural changes; Comparative Example 8 shows that single-stage pressing will cause the thin-walled structure to become unstable, and the deterioration of the structure and properties cannot be repaired by subsequent heat treatment.

[0127] Grain size and its uniformity are the primary microstructural factors affecting the mechanical properties of this type of alloy. Grain refinement improves both strength and plasticity, while grain coarsening and the appearance of mixed-grain structures cause a much greater decrease in impact toughness and elongation after fracture than in strength, and the high-temperature strength retention also declines simultaneously. Therefore, grain size is not only an inspection item after forming, but also an object that needs to be stably controlled during the forming process of this invention.

Claims

1. A method for manufacturing an iron-nickel-based high-temperature alloy elbow, comprising a forming process and a heat treatment process, characterized in that: The forming process includes multiple heating and multiple pressing of the iron-nickel-based high-temperature alloy raw material billet, wherein the multiple heating includes at least a first heating and a last heating, and the multiple pressing includes at least a first pressing and a last pressing. The initial heating process involves multi-stage controlled heating of the raw material billet, including at least a pre-stage controlled heating and a final stage controlled heating. The initial temperature of the pre-stage controlled heating is 300-700℃, with a heating rate of 100-200℃ / h, heating to 20-80℃ above the γ´ phase precipitation temperature and holding at that temperature for no more than 1.2 min / mm. The final stage controlled heating has a heating rate of 50-150℃ / h, heating to 120-200℃ above the γ´ phase precipitation temperature and holding at that temperature for no more than 1.2 min / mm. The first pressing: After the raw material tube blank is first heated, it is flattened to the intermediate size, and a support structure is installed inside the tube blank. The first mold pressing is then performed to form an intermediate blank. The final heating: the intermediate billet is heated to 120~200℃ above the γ´ phase precipitation temperature and held at that temperature for no more than 1.2 min / mm; The final pressing: the heated intermediate billet is flattened to the finished product size, pressed with a final mold, and then cooled to form an elbow.

2. The manufacturing method according to claim 1, characterized in that: The multi-stage controlled heating is a two-stage controlled heating. The initial temperature of the first stage of controlled heating is 400~600℃, the heating rate is 130~160℃ / h, the temperature is raised to 40~70℃ above the γ´ phase precipitation temperature and held at that temperature for no more than 1.2min / mm. The heating rate of the last stage of controlled heating is 80~120℃ / h, the temperature is raised to 130~180℃ above the γ´ phase precipitation temperature and held at that temperature for no more than 1.2min / mm.

3. The manufacturing method according to claim 1, characterized in that: The holding time during the first or last heating is 0.5~1 min / mm.

4. The manufacturing method according to claim 1, characterized in that: The final pressing temperature of the first or last mold pressing shall not be lower than the precipitation temperature of the γ´ phase.

5. The manufacturing method according to claim 1, characterized in that: The starting temperature of the final heating is not lower than the precipitation temperature of the γ´ phase, the heating rate is 80~120℃ / h, and the temperature of the intermediate billet is not lower than the precipitation temperature of the γ´ phase.

6. The manufacturing method according to claim 1, characterized in that: The outer diameter OD of the raw material tube blank is ≥400mm, and the ratio of wall thickness t to outer diameter OD is t / D <0.

15.

7. The manufacturing method according to claim 1, characterized in that: The multi-stage controlled heating does not exceed 3 stages of controlled heating, the staged heating does not exceed 3 times, and the staged pressing does not exceed 3 times.

8. The manufacturing method according to claim 1, characterized in that: The heat treatment of the elbow after forming adopts the following steps: when the temperature is 200~500℃, the heating rate is 100~200℃ / h, the temperature is raised to 20~60℃ above the γ´ phase precipitation temperature and held at that temperature for no more than 1.2min / mm, then the temperature is raised to 80~120℃ above the γ´ phase precipitation temperature at a rate of 50~150℃ / h and held at that temperature for no more than 1.2min / mm, followed by cooling.

9. The manufacturing method according to claim 1, characterized in that: The iron-nickel-based superalloy comprises the following components by weight percentage: Fe 35~45%, Cr 15~21%, Mo 0.5~1.4%, W 0.1~0.8%, Ti 1.8~2.5%, Al 0.8~2.5%, Mn≤1.0%, Nb≤0.1%, Co≤2%, Si≤0.05%, C 0.03~0.10%, B 0.001~0.005%, P≤0.01%, with the balance being Ni; The weight percentage of Cr+Ni is greater than 50%, and the weight percentage of W+Mo is 0.6~1.5%.

10. A nickel-based high-temperature alloy elbow, manufactured by the manufacturing method according to any one of claims 1 to 9, characterized in that: The elbow has an outer diameter OD ≥ 400 mm, a wall thickness t to outer diameter OD ratio t / D < 0.15, a grain size of 2.0~5.0 grade, no mixed crystals, a room temperature tensile strength Rm of not less than 600 MPa, and a plastic elongation strength Rp 0.2 The tensile strength at 650℃ is not less than 280 MPa, the elongation after fracture is not less than 50%, and the room temperature impact toughness KV2 is not less than 130 J; and the tensile strength at 650℃ is not less than 500 MPa, and the plastic elongation strength Rp is not less than 130 J. 0.2 The strength is not less than 320 MPa and the elongation after fracture is not less than 45%.

Citation Information

Patent Citations

  • Large-diameter thin-wall elbow forming method

    CN114130873A

  • A Method for Medium-Frequency Bending of Thick-Walled Pipes Made of GH4070P Nickel-Iron-Based Superalloy

    CN116372508B

  • Nickel-iron-based high-temperature alloy material and aging treatment method thereof

    CN119307836A