A large-size thick pole post blanking system based on local transient cryogenic embrittlement
By combining local transient cryogenic embrittlement technology and reheating module, the problems of large collapse angle, wide tear width, high burr and inconsistent cross-sectional roughness in the punching process of large-size thick pole posts are solved, achieving high-precision punching effect and continuous production.
Patent Information
- Application Number
- CN202611348140.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are prone to problems such as large collapse angles, wide tear widths, high burrs, and inconsistent cross-sectional roughness during the punching process of large-size thick electrode posts, making it difficult to meet the production requirements of high-precision battery electrode posts.
The local transient deep cryogenic embrittlement technology is adopted. The local transient deep cryogenic embrittlement module performs localized low-temperature spraying on the working area of the large-size thick pole precision stamping die module, so that the surface temperature of the material drops sharply to below the brittle transition temperature. Combined with the double-layer flow-guiding reheating and anti-frost cover module and the dry reheating gas supply module, low-temperature spraying before stamping and rapid reheating after stamping are achieved to ensure stamping quality.
It significantly improves the cross-sectional flatness, edge perpendicularity, and shearing quality of large-size thick poles, solves the problems of warping, shifting, local bulging, and cold energy dispersion around the die, and enhances the stability and sustainability of continuous punching.
Smart Images

Figure CN123149306A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal plastic forming, and more particularly to a large-size thick pole punching system based on local transient deep cryogenic embrittlement. Background Technology
[0002] With the rapid development of new energy vehicles and large-scale energy storage industries, power batteries and energy storage batteries are evolving towards higher capacity and higher charge / discharge rates. Under this trend, the current-carrying components inside the battery face more stringent current-carrying requirements. As the core hub connecting the battery cell to the external module, the size and thickness of the battery terminals are constantly increasing (e.g., large-size thick terminals with a thickness of over 5mm). These large-size thick terminals are typically made of pure aluminum, pure copper, or copper-aluminum composite materials to ensure extremely low contact resistance and excellent conductivity.
[0003] In the large-scale manufacturing of battery terminals, punching processes (such as strip cutting, edge trimming, blanking, etc.) are currently an indispensable core separation process due to their extremely high production efficiency.
[0004] For example, the prior art disclosed in CN120828085A discloses a method for forming battery terminal blocks by lifting and continuous punching. A block blank in the feeding channel is pressed and falls into the feeding station of the continuous punching die. The block blank in the feeding station is conveyed to the first punching station of the continuous punching die by lifting and continuous feeding, so that the block blank is punched to form a small annular step on its lower outer periphery. The block blank in the first punching station is conveyed to the second punching station of the continuous punching die by lifting and continuous feeding, so that the block blank is punched to form a large annular step, protrusions, and concave holes. The block blank in the second punching station is conveyed to the blanking station of the continuous punching die by lifting and continuous feeding, so that the middle part of the block blank is punched to form a battery terminal block, which falls into the blanking channel. This method results in a high degree of planar accuracy on the lower surface of the produced battery terminal block, meeting the production requirements of high-precision battery terminal blocks.
[0005] Existing technologies often suffer from problems such as large collapse angles, wide tear widths, high burrs, and inconsistent cross-sectional roughness during the punching process of large-size thick poles. In order to solve the problems that are common in this field, this invention was made. Summary of the Invention
[0006] The purpose of this invention is to address the shortcomings of current methods by proposing a large-size thick pole punching system based on local transient deep cryogenic embrittlement.
[0007] To overcome the shortcomings of the prior art, the present invention adopts the following technical solution:
[0008] A large-size thick pole stamping system based on local transient deep cryogenic embrittlement includes:
[0009] The frame and drive module provide overall load-bearing capacity and high-load punching drive for the system;
[0010] A large-size thick electrode precision blanking die module is installed on the frame and drive module and is used for positioning, holding, guiding, blanking and unloading of large-size thick electrode blanks;
[0011] A localized transient cryogenic embrittlement module is arranged around the periphery of the large-size thick electrode precision stamping die module. It is used to perform localized, targeted low-temperature spraying on the working area of the large-size thick electrode precision stamping die module within a predetermined short period of time before the stamping action occurs. This causes the surface temperature of the working area to drop sharply below the brittle transition temperature of the material, thereby inducing the material to transform from a ductile fracture mode to a brittle fracture mode. The working area of the large-size thick electrode precision stamping die module is hereinafter referred to as the working area.
[0012] The double-layer flow-guiding, reheating and anti-frost cover module is set around the large-size thick pole precision punching die module and around the local transient deep cryogenic embrittlement module. It is used to limit and concentrate the low-temperature jet during the low-temperature jetting stage, and to guide the flow, reheat, de-fog and prevent frost in the working area and its surrounding area after punching.
[0013] The drying and rewarming gas supply module is connected to the double-layer flow-guiding rewarming and anti-frost cover module and is used to provide a drying and rewarming airflow to the double-layer flow-guiding rewarming and anti-frost cover module.
[0014] The timing coordination control module is connected to the frame and drive module, the local transient cryogenic embrittlement module and the drying and reheating gas supply module respectively, and is used to control the opening and closing coordination of the local transient cryogenic injection and the reheating airflow according to the timing of the punching stroke.
[0015] The large-size thick pole precision blanking die module includes an upper die base, a lower die base, a punch, a die cavity, a blanking structure, a guiding structure, and a blank positioning support structure. The local transient deep cryogenic embrittlement module includes a low-temperature medium source, a low-temperature delivery pipeline, an annular distribution cavity, and a micro-nozzle array. The double-layer flow guiding and reheating anti-frost cover module includes a cold flow convergence cover located on the inner side and a reheating flow guiding cover located on the outer side. The cold flow convergence cover and the periphery of the working area form a locally confined spray space, and the reheating flow guiding cover and the cold flow convergence cover form an annular or circumferentially connected reheating air passage.
[0016] The timing coordination control module controls the local transient cryogenic embrittlement module to perform transient injection before the punch enters the working area, and controls the drying and warming gas supply module to deliver dry and warming gas flow to the warming gas channel after the punch completes the punching, so as to reduce the frost, condensation and residual cold shrinkage stress after the thick electrode punching, and maintain the stability of continuous punching.
[0017] Furthermore, the frame and drive module includes a frame body, a slider drive mechanism, an upper die mounting base, and a lower die mounting base. The frame body is used to withstand the large punching force during the punching process of large-size thick pole posts. The slider drive mechanism is used to drive the upper die mounting base to reciprocate in a predetermined direction to ensure that the punch performs closed punching with high rigidity and high repeatability relative to the die.
[0018] Furthermore, the pressing structure in the large-size thick electrode precision blanking die module includes one or more combinations of pressing plate, pressing ring or partitioned pressing components. The pressing structure is used to apply a stable pressing force to the surface of the blank before blanking the large-size thick electrode blank, so as to suppress the warping, movement and local bulging of the blank during low temperature spraying and high load blanking process.
[0019] The guiding structure includes a guide post and guide sleeve pair, a guide slider pair, or a composite guide pair. The guiding structure is used to ensure the accuracy of the cutting edge clearance between the punch and the die and the motion stability during the large-contour punching process.
[0020] The blank positioning support structure is used to support large-sized thick pole blanks and define the relative positional relationship between the blanking area and the punch, die and local low-temperature spraying area.
[0021] Furthermore, the cryogenic medium source in the local transient cryogenic embrittlement module is a liquid nitrogen storage and supply unit, the cryogenic delivery pipeline is a cold-insulating delivery pipeline, the annular distribution cavity is located around the die cutting edge, and the micro-nozzle array is arranged around the periphery of the large-size thick pole blank to be sheared and inclined towards the working area, so as to spray the cryogenic medium into the working area in a circumferentially surrounding and locally converging manner, so that the blank enters a cryogenic embrittlement state briefly before punching.
[0022] Furthermore, the micro-nozzle array adopts a multi-nozzle partition structure, with each partition nozzle module connected to the annular distribution cavity. The multi-nozzle partition structure includes at least two sets of nozzle units arranged along the length and circumferential direction of the electrode profile. Each nozzle unit points towards the working area with a predetermined tilt angle and a predetermined convergence direction to adapt to the characteristics of large-size thick electrode profiles with long profiles, large shear circumference, and high local heat capacity, ensuring the uniformity of low-temperature action along the entire punching profile.
[0023] Furthermore, the cold flow convergence cover in the double-layer flow guiding and reheating anti-frost cover module is located near the die cutting edge. The cold flow convergence cover has a confined flow guiding surface facing the die opening area. The confined flow guiding surface, together with the periphery of the die cutting edge and the periphery of the working area, forms a semi-enclosed low-temperature spraying space. This space is used to ensure that the low-temperature medium sprayed by the local transient deep cryogenic embrittlement module acts preferentially on the working area, reducing the diffusion of the low-temperature medium to the mold periphery, the feeding area, and the non-processing area.
[0024] The reheating guide hood in the double-layer flow guiding reheating and anti-frost cover module is sleeved on the outside of the cold flow converging cover, and the two form a ring or circumferentially connected reheating air channel. The reheating guide hood is provided with a reheating gas inlet, a flow guiding slope, and a reheating gas outlet facing the die area and the edge area of the thick electrode post. The reheating guide hood is used to transport the dry reheating airflow along a predetermined direction to the periphery of the cutting edge, the top of the die, and the area adjacent to the cross-section of the thick electrode post blank after the blanking is completed, so as to remove residual cold fog, suppress frost formation, and promote local reheating.
[0025] The double-layer flow-guiding reheating and anti-frost cover module also includes a mist vent and a condensation guide channel. The mist vent is used to discharge the low-temperature mist formed around the die opening during the punching process of large-size thick electrode posts. The condensation guide channel is used to directionally discharge the condensate formed during the reheating process, so as to reduce the risk of condensation and icing on the surface of the thick electrode post blank, the edge of the die opening, and the feeding support area.
[0026] Furthermore, the drying and rewarming gas supply module includes a drying gas source, a pressure stabilizing unit, a gas supply pipeline, and a control valve group. The drying gas source is a dry air source or a dry nitrogen source. The pressure stabilizing unit is used to stabilize the rewarming gas flow pressure. The control valve group is used to provide intermittent or continuous rewarming gas flow to the rewarming gas channel under the control of the timing coordination control module, thereby achieving local rewarming and anti-frost without significantly disturbing the thermal stability of the large-size thick pole precision stamping die module.
[0027] Furthermore, the timing coordination control module includes a stroke detection unit, a timing control unit, and an execution unit connected to the local transient cryogenic embrittlement module and the drying and reheating gas supply module. The stroke detection unit is used to detect the motion stages of the punch approaching the thick pole blank, starting shearing, and completing the punching separation. The timing control unit is used to control the start time of cryogenic injection, the duration of injection, the end time of injection, and the start and stop times of reheating airflow according to the motion stages, so as to form a coordinated workflow of short-term pre-punching chilling embrittlement, high-rigidity punching during punching, and post-punching guiding reheating and demisting.
[0028] Furthermore, the system's workflow includes the following steps:
[0029] S1. After the large-size thick electrode blank enters the punching station, the blank positioning and support structure completes the positioning and support, and the pressing structure stably presses the thick electrode blank above the die.
[0030] S2, the timing coordination control module controls the liquid nitrogen to enter the annular distribution cavity through the cold-insulating delivery pipeline according to the punch stroke state, and then spray it into the working area along the shearing contour of the large-size thick pole by the micro-nozzle array;
[0031] S3, the thick electrode blank changes from ductile fracture mode to brittle fracture mode;
[0032] S4, the punch enters the thick pole blank under the guidance of the guide structure, and completes rigid shearing separation with the die;
[0033] S5. After the punching is completed, the timing coordination control module controls the low temperature injection to be turned off or reduced, and at the same time starts the drying and reheating gas supply module. The drying airflow enters the outer reheating guide shroud, is guided by the reheating air passage and the guide slope, and blows towards the die area and the area adjacent to the thick pole section to quickly complete the defogging, anti-frost and local reheating.
[0034] S6, residual mist is discharged from the mist outlet, and condensate is discharged from the condensate guide channel.
[0035] The beneficial effects achieved by this invention are as follows: 1. Unlike existing technologies that mainly rely on continuous blanking at room temperature, segmented forming, or simply improving the rigidity of the die, this solution does not directly apply forced shearing to the thick electrode under room temperature conditions. Instead, before blanking, it uses a liquid nitrogen storage and supply unit, a cold-insulating and conveying pipeline, an annular distribution cavity, and a micro-nozzle array in a local transient cryogenic embrittlement module to apply short-term, fixed-point, and circumferentially enveloping low-temperature spray to the working area. This rapidly reduces the surface temperature of the steel thick electrode shearing zone to below the brittle transition temperature, and then the punch and die complete the rigid shearing. This solution solves the problems of large collapse angles, wide tear widths, high burrs, and inconsistent cross-sectional roughness that easily occur in the blanking process of large-size thick electrodes in existing technologies. Through the structural synergy of "first local embrittlement, then transient shearing," the fracture mode, which was originally dominated by ductile tearing, is transformed into brittle fracture, thereby significantly improving the flatness of the cross-section, the perpendicularity of the edges, and the shearing quality.
[0036] 2. This solution incorporates a blank positioning support structure, a blank clamping structure, and a guiding structure within the large-size thick electrode precision blanking die module. Combined with a multi-nozzle partitioning structure in the localized transient cryogenic embrittlement module, this ensures that the spray center region, the punch shearing center region, and the confinement center region correspond to each other. This solution addresses issues such as warping, shifting, localized bulging, and inconsistent shearing states in different sections that easily occur during the blanking process of large-size thick electrodes due to their long profile, large plate thickness, and high localized heat capacity. Through the combined action of locating pins, lateral limiting blocks, support pads, blank clamping plates or clamping rings, and guide post / sleeve pairs, along with a micro-nozzle array arranged along the perimeter of the profile, synchronous matching of localized cryogenic effects and mechanical shearing effects is achieved throughout the entire profile range. This improves the consistency of the overall cross-sectional quality and the stability of repeated processing.
[0037] 3. This solution incorporates a cold flow convergence shield near the die cutting edge within the double-layer flow-guiding, reheating, and anti-frost shield module. This shield, along with the confined flow-guiding surface and the periphery of the working area, forms a semi-enclosed cryogenic spraying space. This ensures that the cryogenic medium ejected from the localized transient cryogenic embrittlement module preferentially acts on the working area. This solution addresses common problems in existing cryogenic assisted machining, such as cold flow dispersion, insufficient localized embrittlement efficiency, and overcooling of the die body. Through the spatial coupling between the cold flow convergence shield, the annular distribution cavity, and the micro-nozzle array, limited cooling capacity is concentrated on the area where shear separation truly occurs. This improves cryogenic embrittlement efficiency while reducing overall cryogenic shrinkage, thermal drift, and unnecessary energy loss around the die periphery.
[0038] 4. This solution features a rewarming guide hood outside the cold flow convergence hood, forming a rewarming air passage between them. It also includes a rewarming gas inlet, rewarming gas outlet, guide ramp, mist outlet, and condensation guide groove. An external drying rewarming gas supply module connects to the drying gas source, pressure stabilizing unit, gas pipeline, and control valve assembly. This solution solves the problems of cold mist accumulation, surface frost, condensation and icing in the feeding area, and disruption of subsequent continuous punching cycles after low-temperature spraying. By blowing the dry rewarming airflow in a predetermined direction towards the die area and the area adjacent to the thick electrode section after punching, and promptly discharging mist and condensate, it achieves rapid rewarming, mist removal, and frost prevention after punching, significantly improving the station stability and sustainable operation capability under continuous, high-volume punching conditions. Attached Figure Description
[0039] The invention will be further understood from the following description taken in conjunction with the accompanying drawings. The components in the drawings are not necessarily drawn to scale, but rather the emphasis is on illustrating the principles of the embodiments. In different views, the same reference numerals designate the same parts.
[0040] Figure 1 This is a schematic diagram of the overall structure of the present invention.
[0041] Figure 2This is a flowchart of the process of the present invention.
[0042] Figure 3 This is a comparison diagram of the cross-sectional quality of the present invention and Comparative Example 1.
[0043] Figure 4 This is a comparison diagram of the effects of the present invention and Comparative Example 2 in terms of continuous punching stability.
[0044] Figure descriptions: 1. Frame and drive module; 2. Large-size thick pole precision punching die module; 3. Local transient deep cryogenic embrittlement module; 4. Double-layer flow guiding reheating anti-frost cover module; 5. Drying reheating gas supply module. Detailed Implementation
[0045] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can understand the advantages and effects of the present invention from the content disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and various details in this specification can also be modified and changed based on different viewpoints and applications without departing from the spirit of the present invention. Furthermore, the accompanying drawings of the present invention are for simple illustrative purposes only and are not depictions of actual dimensions; this is stated beforehand. The following embodiments will further describe the relevant technical content of the present invention in detail, but the disclosed content is not intended to limit the scope of protection of the present invention.
[0046] Example 1: This example provides a large-size thick pole punching system based on local transient deep cryogenic embrittlement, including:
[0047] The frame and drive module provide overall load-bearing capacity and high-load punching drive for the system;
[0048] A large-size thick electrode precision blanking die module is installed on the frame and drive module and is used for positioning, holding, guiding, blanking and unloading of large-size thick electrode blanks;
[0049] A localized transient cryogenic embrittlement module is arranged around the periphery of the large-size thick electrode precision stamping die module. It is used to perform localized, targeted low-temperature spraying on the working area of the large-size thick electrode precision stamping die module within a predetermined short period of time before the stamping action occurs. This causes the surface temperature of the working area to drop sharply below the brittle transition temperature of the material, thereby inducing the material to transform from a ductile fracture mode to a brittle fracture mode. The working area of the large-size thick electrode precision stamping die module is hereinafter referred to as the working area.
[0050] The double-layer flow-guiding, reheating and anti-frost cover module is set around the large-size thick pole precision punching die module and around the local transient deep cryogenic embrittlement module. It is used to limit and concentrate the low-temperature jet during the low-temperature jetting stage, and to guide the flow, reheat, de-fog and prevent frost in the working area and its surrounding area after punching.
[0051] The drying and rewarming gas supply module is connected to the double-layer flow-guiding rewarming and anti-frost cover module and is used to provide a drying and rewarming airflow to the double-layer flow-guiding rewarming and anti-frost cover module.
[0052] The timing coordination control module is connected to the frame and drive module, the local transient cryogenic embrittlement module and the drying and reheating gas supply module respectively, and is used to control the opening and closing coordination of the local transient cryogenic injection and the reheating airflow according to the timing of the punching stroke.
[0053] The large-size thick pole precision blanking die module includes an upper die base, a lower die base, a punch, a die cavity, a blanking structure, a guiding structure, and a blank positioning support structure. The local transient deep cryogenic embrittlement module includes a low-temperature medium source, a low-temperature delivery pipeline, an annular distribution cavity, and a micro-nozzle array. The double-layer flow guiding and reheating anti-frost cover module includes a cold flow convergence cover located on the inner side and a reheating flow guiding cover located on the outer side. The cold flow convergence cover and the periphery of the working area form a locally confined spray space, and the reheating flow guiding cover and the cold flow convergence cover form an annular or circumferentially connected reheating air passage.
[0054] The timing coordination control module controls the local transient cryogenic embrittlement module to perform transient injection before the punch enters the working area, and controls the drying and warming gas supply module to deliver dry and warming gas flow to the warming gas channel after the punch completes the punching, so as to reduce the frost, condensation and residual cold shrinkage stress after the thick electrode punching, and maintain the stability of continuous punching.
[0055] Specifically, this solution is only applicable to steel electrodes. Steel is a body-centered cubic (BCC) metal with a defined ductile-brittle transition temperature. Local cooling of the steel electrode edge with liquid nitrogen causes it to transition from ductile fracture to brittle fracture at the moment of punching, resulting in an extremely smooth, burr-free fracture surface. However, this solution is not suitable for copper or aluminum electrodes, as copper and aluminum do not exhibit a ductile-brittle transition.
[0056] Furthermore, the blank positioning support structure includes at least one of a positioning pin, a lateral limiting block, a support pad block, or a contour-fitting support surface. The blank positioning support structure is used to accurately position the large-size thick pole blank at the corresponding position of the punch and the die before local cryogenic spraying, so that the spraying center area of the local transient deep cryogenic embrittlement module, the punch shearing center area, and the confinement center area of the double-layer flow guiding reheating anti-frost cover module correspond to each other, thereby improving the local embrittlement consistency and punching section consistency along the entire large-size thick pole contour.
[0057] Furthermore, the frame and drive module includes a frame body, a slider drive mechanism, an upper die mounting base, and a lower die mounting base. The frame body is used to withstand the large punching force during the punching process of large-size thick pole posts. The slider drive mechanism is used to drive the upper die mounting base to reciprocate in a predetermined direction to ensure that the punch performs closed punching with high rigidity and high repeatability relative to the die.
[0058] Furthermore, the pressing structure in the large-size thick electrode precision blanking die module includes one or more combinations of pressing plate, pressing ring or partitioned pressing components. The pressing structure is used to apply a stable pressing force to the surface of the blank before blanking the large-size thick electrode blank, so as to suppress the warping, movement and local bulging of the blank during low temperature spraying and high load blanking process.
[0059] The guiding structure includes a guide post and guide sleeve pair, a guide slider pair, or a composite guide pair. The guiding structure is used to ensure the accuracy of the cutting edge clearance between the punch and the die and the motion stability during the large-contour punching process.
[0060] The blank positioning support structure is used to support large-sized thick pole blanks and define the relative positional relationship between the blanking area and the punch, die and local low-temperature spraying area.
[0061] Furthermore, the cryogenic medium source in the local transient cryogenic embrittlement module is a liquid nitrogen storage and supply unit, the cryogenic delivery pipeline is a cold-insulating delivery pipeline, the annular distribution cavity is located around the die cutting edge, and the micro-nozzle array is arranged around the periphery of the large-size thick pole blank to be sheared and inclined towards the working area, so as to spray the cryogenic medium into the working area in a circumferentially surrounding and locally converging manner, so that the blank enters a cryogenic embrittlement state briefly before punching.
[0062] Furthermore, the micro-nozzle array adopts a multi-nozzle partition structure, with each partition nozzle module connected to the annular distribution cavity. The multi-nozzle partition structure includes at least two sets of nozzle units arranged along the length and circumferential direction of the electrode profile. Each nozzle unit points towards the working area with a predetermined tilt angle and a predetermined convergence direction to adapt to the characteristics of large-size thick electrode profiles with long profiles, large shear circumference, and high local heat capacity, ensuring the uniformity of low-temperature action along the entire punching profile.
[0063] Furthermore, the cold flow convergence cover in the double-layer flow guiding and reheating anti-frost cover module is located near the die cutting edge. The cold flow convergence cover has a confined flow guiding surface facing the die opening area. The confined flow guiding surface, together with the periphery of the die cutting edge and the periphery of the working area, forms a semi-enclosed low-temperature spraying space. This space is used to ensure that the low-temperature medium sprayed by the local transient deep cryogenic embrittlement module acts preferentially on the working area, reducing the diffusion of the low-temperature medium to the mold periphery, the feeding area, and the non-processing area.
[0064] The reheating guide hood in the double-layer flow guiding reheating and anti-frost cover module is sleeved on the outside of the cold flow converging cover, and the two form a ring or circumferentially connected reheating air channel. The reheating guide hood is provided with a reheating gas inlet, a flow guiding slope, and a reheating gas outlet facing the die area and the edge area of the thick electrode post. The reheating guide hood is used to transport the dry reheating airflow along a predetermined direction to the periphery of the cutting edge, the top of the die, and the area adjacent to the cross-section of the thick electrode post blank after the blanking is completed, so as to remove residual cold fog, suppress frost formation, and promote local reheating.
[0065] The double-layer flow-guiding reheating and anti-frost cover module also includes a mist vent and a condensation guide channel. The mist vent is used to discharge the low-temperature mist formed around the die opening during the punching process of large-size thick electrode posts. The condensation guide channel is used to directionally discharge the condensate formed during the reheating process, so as to reduce the risk of condensation and icing on the surface of the thick electrode post blank, the edge of the die opening, and the feeding support area.
[0066] Specifically, at least one of the cold flow convergence shroud and the rewarming flow guide shroud forms an integrated or combined installation structure with the pressing structure, unloading structure or mold protective cover, so as to compactly integrate the low-temperature spray confinement, rewarming flow guide, anti-frost protection and mold body in space, thereby reducing the space occupied by the peripheral auxiliary mechanism and improving the compactness and assembly stability of the large-size thick pole blanking station arrangement.
[0067] Specifically, the local transient deep cryogenic embrittlement module induces the surface of the billet to enter a brittle fracture state briefly before punching, and the double-layer flow-guiding reheating and anti-frost cover module restricts the effect of low temperature to the area near the cutting edge. This reduces the collapse corner, tear band width and burr height during the punching of large-size thick poles, while also reducing the impact of plastic flow instability of thick materials, inconsistent cross-sectional roughness, and frost formation, condensation and overall low-temperature shrinkage on the stability of continuous punching.
[0068] Specifically, both the cold flow convergence shroud and the rewarming flow guide shroud are detachable modular structures, including at least the shroud body, mounting flange, positioning part and sealing connection part, which facilitates the replacement of the corresponding shroud according to the pole blanks of different sizes, thickness ranges and contours, so as to ensure the adaptability of the local low temperature confinement effect and the rewarming anti-frost effect.
[0069] Furthermore, the drying and rewarming gas supply module includes a drying gas source, a pressure stabilizing unit, a gas supply pipeline, and a control valve group. The drying gas source is a dry air source or a dry nitrogen source. The pressure stabilizing unit is used to stabilize the rewarming gas flow pressure. The control valve group is used to provide intermittent or continuous rewarming gas flow to the rewarming gas channel under the control of the timing coordination control module, thereby achieving local rewarming and anti-frost without significantly disturbing the thermal stability of the large-size thick pole precision stamping die module.
[0070] Specifically, the local transient cryogenic embrittlement module, the double-layer flow-guiding reheating and anti-frost cover module, and the large-size thick electrode precision blanking die module are arranged around the same blanking center or the same blanking contour. The local transient cryogenic embrittlement module is used to implement local transient low-temperature embrittlement on the shear band corresponding to the blanking contour of the large-size thick electrode blank before blanking. The large-size thick electrode precision blanking die module is used to complete the blanking separation when the material is in a low-temperature embrittlement state. The double-layer flow-guiding reheating and anti-frost cover module and the dry reheating gas supply module are used to quickly reheat and defogging and anti-frost the area around the die opening and the area adjacent to the cross-section of the thick electrode after blanking, thereby realizing the large-size thick electrode precision blanking process with local low temperature and overall limited thermal impact.
[0071] Furthermore, the timing coordination control module includes a stroke detection unit, a timing control unit, and an execution unit connected to the local transient cryogenic embrittlement module and the drying and reheating gas supply module. The stroke detection unit is used to detect the motion stages of the punch approaching the thick pole blank, starting shearing, and completing the punching separation. The timing control unit is used to control the start time of cryogenic injection, the duration of injection, the end time of injection, and the start and stop times of reheating airflow according to the motion stages, so as to form a coordinated workflow of short-term pre-punching chilling embrittlement, high-rigidity punching during punching, and post-punching guiding reheating and demisting.
[0072] Furthermore, the system's workflow includes the following steps:
[0073] S1. After the large-size thick electrode blank enters the punching station, the blank positioning and support structure completes the positioning and support, and the pressing structure stably presses the thick electrode blank above the die.
[0074] S2, the timing coordination control module controls the liquid nitrogen to enter the annular distribution cavity through the cold-insulating delivery pipeline according to the punch stroke state, and then spray it into the working area along the shearing contour of the large-size thick pole by the micro-nozzle array;
[0075] Specifically, in this stage, the inner cold flow constriction shroud restricts the cold flow to the vicinity of the blanking profile, preventing the cold energy from diffusing to the outside.
[0076] S3, the thick electrode blank changes from ductile fracture mode to brittle fracture mode;
[0077] S4, the punch enters the thick pole blank under the guidance of the guide structure, and completes rigid shearing separation with the die;
[0078] S5. After the punching is completed, the timing coordination control module controls the low temperature injection to be turned off or reduced, and at the same time starts the drying and reheating gas supply module. The drying airflow enters the outer reheating guide shroud, is guided by the reheating air passage and the guide slope, and blows towards the die area and the area adjacent to the thick pole section to quickly complete the defogging, anti-frost and local reheating.
[0079] S6, residual mist is discharged from the mist outlet, and condensate is discharged from the condensate guide channel.
[0080] The beneficial effects of this solution are as follows: 1. Unlike existing technologies that mainly rely on continuous blanking at room temperature, segmented forming, or simply improving the rigidity of the die, this solution does not directly apply forced shearing to the thick electrode at room temperature. Instead, before blanking, it uses a liquid nitrogen storage and supply unit, a cold-insulating delivery pipeline, an annular distribution cavity, and a micro-nozzle array in a local transient cryogenic embrittlement module to apply short-term, targeted, and circumferentially enveloping low-temperature spray to the working area. This rapidly reduces the surface temperature of the steel thick electrode shearing zone to below the brittle transition temperature, and then the punch and die complete the rigid shearing. This solution solves the problems of large collapse angles, wide tear widths, high burrs, and inconsistent cross-sectional roughness that easily occur in the blanking process of large-size thick electrodes in existing technologies. Through the structural synergy of "first local embrittlement, then transient shearing," the fracture mode, which is mainly ductile tearing, is transformed into brittle fracture, thereby significantly improving the flatness of the cross-section, the perpendicularity of the edges, and the shearing quality.
[0081] 2. This solution incorporates a blank positioning support structure, a blank clamping structure, and a guiding structure within the large-size thick electrode precision blanking die module. Combined with a multi-nozzle partitioning structure in the localized transient cryogenic embrittlement module, this ensures that the spray center region, the punch shearing center region, and the confinement center region correspond to each other. This solution addresses issues such as warping, shifting, localized bulging, and inconsistent shearing states in different sections that easily occur during the blanking process of large-size thick electrodes due to their long profile, large plate thickness, and high localized heat capacity. Through the combined action of locating pins, lateral limiting blocks, support pads, blank clamping plates or clamping rings, and guide post / sleeve pairs, along with a micro-nozzle array arranged along the perimeter of the profile, synchronous matching of localized cryogenic effects and mechanical shearing effects is achieved throughout the entire profile range. This improves the consistency of the overall cross-sectional quality and the stability of repeated processing.
[0082] 3. This solution incorporates a cold flow convergence shield near the die cutting edge within the double-layer flow-guiding, reheating, and anti-frost shield module. This shield, along with the confined flow-guiding surface and the periphery of the working area, forms a semi-enclosed cryogenic spraying space. This ensures that the cryogenic medium ejected from the localized transient cryogenic embrittlement module preferentially acts on the working area. This solution addresses common problems in existing cryogenic assisted machining, such as cold flow dispersion, insufficient localized embrittlement efficiency, and overcooling of the die body. Through the spatial coupling between the cold flow convergence shield, the annular distribution cavity, and the micro-nozzle array, limited cooling capacity is concentrated on the area where shear separation truly occurs. This improves cryogenic embrittlement efficiency while reducing overall cryogenic shrinkage, thermal drift, and unnecessary energy loss around the die periphery.
[0083] 4. This solution features a rewarming guide hood outside the cold flow convergence hood, forming a rewarming air passage between them. It also includes a rewarming gas inlet, rewarming gas outlet, guide ramp, mist outlet, and condensation guide groove. An external drying rewarming gas supply module connects to the drying gas source, pressure stabilizing unit, gas pipeline, and control valve assembly. This solution solves the problems of cold mist accumulation, surface frost, condensation and icing in the feeding area, and disruption of subsequent continuous punching cycles after low-temperature spraying. By blowing the dry rewarming airflow in a predetermined direction towards the die area and the area adjacent to the thick electrode section after punching, and promptly discharging mist and condensate, it achieves rapid rewarming, mist removal, and frost prevention after punching, significantly improving the station stability and sustainable operation capability under continuous, high-volume punching conditions.
[0084] Example 2: This example should be understood as including all the features of any of the foregoing examples, and further improving upon them. It also includes an intelligent punching control method based on a local stress-temperature coupling quantification criterion. This method is used to predict the effect of triggering brittle fracture and control the punching process according to the prediction results.
[0085] This embodiment no longer uses a single temperature below a set value as a qualitative empirical criterion for initiating punching. Instead, it innovatively embeds a real-time calculation unit in the timing collaborative control module to construct a local stress-temperature coupling criterion based on critical cleavage fracture stress, thereby achieving a leap from open-loop timing control to closed-loop quantitative control.
[0086] To achieve this embodiment, during the dynamic process of the punch descending and contacting the steel thick pole blank and undergoing shearing, the timing-coordinated control module calculates the brittle fracture induction index in real time according to the following formula:
[0087]
[0088] in, The brittle fracture initiation index at time t is used to characterize the relative margin by which local stress exceeds the material's low-temperature resistance threshold. The larger the index, the larger the relative margin, the better the effect of triggering brittle fracture, and the better the punching effect. Let be the local equivalent stress at the cutting edge at time t, which is the driving force used to trigger brittle fracture. The surface temperature at the shearing position at time t refers to the real-time temperature of the surface layer of the separation surface (i.e., the target area of deep cryogenic spraying) on the steel pole blank that is about to be sheared by the punch. The theoretical value of this temperature is the temperature threshold required to trigger brittle fracture. The real-time temperature is obtained as follows: An optical observation window (equipped with air curtain protection against frost) is opened on the cold flow convergence cover facing the working area, and a high-speed infrared temperature measurement probe with a response time of less than 1ms is installed. The probe signal is connected to the timing coordination control module to realize temperature detection. For at a temperature of The critical cleavage fracture stress under certain conditions is an intrinsic physical property of steel pole materials. It refers to the minimum stress required for microcracks inside the material to overcome lattice resistance and rapidly propagate through cleavage at that temperature. It can be obtained by consulting relevant literature.
[0089] Furthermore, The cryogenic embrittlement penetration attenuation factor at time t represents the effectiveness of liquid nitrogen cooling from the surface of the electrode to its core. When its value approaches 1, the effectiveness is very high; when its value approaches 0, the effectiveness is very low. It is obtained as follows:
[0090]
[0091] in, It is an exponential function. The thickness of the pole piece, This is the transient thermal penetration depth, which can be determined based on the surface temperature measured by infrared radiation. The duration of liquid nitrogen injection and the thermal conductivity of steel are determined by integrating the simplified one-dimensional unsteady-state partial differential equation of heat conduction built into the system in real time. This model can be obtained by consulting relevant materials.
[0092] Furthermore, Let be the strain rate-induced embrittlement gain factor at time t. Punching is a dynamic process; high strain rates force the material to transition from plastic deformation to brittle fracture. This factor quantifies the promoting effect of strain rate on brittle fracture, and its acquisition method is as follows:
[0093]
[0094] in, The strain rate nonlinear amplification factor is obtained as follows: Using a split Hopkinson bar (SHPB) apparatus, impact compression tests with different strain rates are conducted on the material at a low temperature environment of -100°C to -196°C. The rate of change of the partial derivative of the yield stress with respect to the logarithm of the strain rate is measured within the ductile-brittle transition temperature range. This rate of change is the strain rate nonlinear amplification factor. ; The real-time punching strain rate is calculated by dividing the instantaneous punch speed provided by the servo motor encoder by the pole thickness. get, This is a reference value for the punching strain rate, set by those skilled in the art based on experience;
[0095] Specifically, the local equivalent stress at the cutting edge at time t The instantaneous total punching force can be obtained using the force sensors built into the frame and drive module (such as hydraulic cylinder oil pressure sensors or servo motor torque / current sensors). A "stress concentration factor empirical database" (generated from previous offline finite element simulation fitting) for the specific pole profile and die clearance is pre-set in the timing-coordinated control module. The local equivalent stress can then be obtained according to the following formula. :
[0096]
[0097] in, The stress concentration factor is... Let be the instantaneous total punching force at time t. This is the theoretical punching area, which is set by those skilled in the art based on the punching target.
[0098] Furthermore, the brittle fracture excitation index Each threshold is set, and the timing coordination control module makes a judgment. When the value is greater than or equal to the corresponding threshold, the system confirms that the material has stably entered the brittle fracture-dominated mode and maintains or outputs the maximum punching driving force; if it is detected in the early stage of shearing... When the value is less than or equal to the corresponding threshold, the system will output an alarm or intervene to adjust the punching speed of the drive module.
[0099] Specifically, the threshold is obtained as follows:
[0100] 1. During the system debugging phase, conduct no less than 50 trial punchings using the same process parameters as in formal production (same batch of materials, same cryogenic jetting pressure, same punching speed);
[0101] 2. For each punching operation, the timing coordination control module records the maximum value during the shearing process. Value, denoted as ;
[0102] 3. Remove the stamped pole piece and use an optical microscope or 3D profilometer to measure the tear band width ratio of the cross section (the wider the tear band, the more ductile fracture components there are). Set a passing standard, such as the tear band ratio must be less than or equal to 5%.
[0103] 4. Among all the trial blanking samples that meet the qualification standards, extract the smallest one. value;
[0104] 5. Multiply this minimum value by a safety factor (e.g., 0.8~0.9) to determine the final threshold for production. This means that as long as the actual calculated value... Exceeding this threshold can statistically guarantee that over 99% of the product cross-sections meet the smoothness standard for brittle fracture.
[0105] The beneficial effects of this embodiment: Existing technology believes that as long as the surface temperature of the steel pole is confirmed to drop below the ductile-brittle transition temperature (DBTT) by infrared thermometry, it is simply equivalent to the material having met the conditions for brittle fracture, and then the punching command is directly issued. This is an open-loop empirical control. This solution: adopts a multi-dimensional and dynamic judgment logic, believing that in the millisecond-level punching transient process, low temperature only provides a possibility. The actual brittle fracture is the result of the coupling of cold penetration, stress loading, and constraint state in time and space. This solution upgrades the judgment standard from a single temperature target to a multi-dimensional dynamic prediction of the effect of triggering brittle fracture, and controls the punching process according to the prediction results.
[0106] Furthermore, this scheme introduces a cryogenic embrittlement penetration attenuation factor and adopts an exponential decay model to accurately quantify the degree of discount on the overall effective embrittlement capability when the surface is cold and the center is hot. By introducing a strain rate-induced embrittlement gain factor, it quantifies the degree to which the embrittlement-promoting effect is obtained when the punching speed is fast and the material dislocations do not have time to move. This is beneficial for achieving the effect of multi-dimensional dynamic prediction to trigger brittle fracture.
[0107] Example 3: This example should be understood as including all the features of any of the foregoing examples, and further improving upon them. It also includes supplementing the above examples with more specific equipment models and size parameters, and provides a comparative example between this solution and the prior art.
[0108] In this embodiment, the blank to be punched is a large-sized thick steel electrode blank, made of Q235B low-carbon steel or SPCC cold-rolled steel. The blank has dimensions of 80mm × 45mm and a thickness of 6.0mm, with a perimeter of 180mm to 220mm for the punching outline. The blank surface is degreased and dried before entering the punching station. Because the steel thick electrode material has a body-centered cubic crystal structure, it exhibits a ductile-brittle transition at low temperatures. Therefore, a localized transient cryogenic embrittlement module can induce the area to be sheared to enter a state dominated by brittle fracture before punching. Copper, aluminum, or copper-aluminum composite electrodes are not considered preferred materials in this embodiment.
[0109] The frame and drive module utilize a closed-type dual-point servo press as the load-bearing and driving foundation. The selected equipment model is a JH36-250 closed-type dual-point press or an equivalent tonnage servo hydraulic press, with a nominal pressure of 2500kN, a slide stroke of 180mm, a slide speed adjustment range of 20mm / s to 180mm / s, and an effective worktable size of 900mm × 600mm. The upper die mounting base is connected to the slide via a T-slot and a locating key, while the lower die mounting base is fixed to the worktable via locating pins and high-strength bolts. To ensure the relative positional accuracy between the punch and die during large-size thick pole blanking, the slide repeatability accuracy of the frame and drive module is controlled within ±0.015mm, and the worktable flatness is controlled within 0.03mm / 500mm.
[0110] The large-size thick electrode precision blanking die module includes an upper die base, a lower die base, a punch, a die, a blank holder structure, a guide structure, and a blank positioning and support structure. The upper and lower die bases are made of 45# steel with a hardness of HRC28–32 after quenching and tempering. The punch and die are made of Cr12MoV or DC53 cold work die steel, with a hardness of HRC58–62 after vacuum quenching and deep cryogenic tempering. The punch cutting edge radius is 0.02mm–0.05mm, and the die cutting edge radius is 0.03mm–0.06mm. For a 6.0mm thick steel electrode blank, the single-sided blanking clearance between the punch and die is set to 0.06mm–0.12mm, preferably 0.09mm. This clearance ensures that the fracture surface after low-temperature embrittlement can expand along the predetermined shear band, while avoiding excessive clearance that could lead to secondary tearing and increased burrs.
[0111] The blanking structure employs a combination of annular blanking plates and segmented holding blocks. The annular blanking plate is arranged around the blanking contour, with a 0.3mm–0.5mm wide annular holding band on the lower surface of the blanking plate in contact with the blank. The segmented holding blocks are arranged along the long side of the contour and in the rounded corner transition area, with each segmented holding block provided with holding force by an independent spring or nitrogen spring. The total blanking force is set to 80kN–120kN, preferably 100kN. This blanking structure suppresses blank warping, shifting, and edge bulging under low-temperature spraying and blanking loads, ensuring that the shearing band aligns with the low-temperature action area.
[0112] The guiding structure employs a combination of four guide post and guide sleeve pairs and two sets of lateral guide slider pairs. The guide post diameter is 40mm, the inner hole clearance of the guide sleeve is 0.008mm~0.015mm, and the guiding length of the lateral guide slider pairs is not less than 80mm. The guiding structure ensures that the offset of the punch relative to the die during the downward movement does not exceed 0.02mm, thereby avoiding problems such as uneven local clearance, widening of local tear bands, and decreased perpendicularity of the cross-section when punching large-sized thick pole posts with long contours.
[0113] The blank positioning and support structure includes two 8mm diameter positioning pins, two lateral limiting blocks, four support pads, and a contour-fitting support surface. The positioning pins engage with the pre-set positioning holes in the blank. The lateral limiting blocks define the blank's position in the feeding and lateral directions. The support pads support the non-punching areas of the blank, and the contour-fitting support surface is arranged around the outer edge of the contour to be punched. This structure ensures that the punch shearing center, die cutting edge center, liquid nitrogen jetting center, and cold flow convergence cover confinement center maintain a coaxial or contour-corresponding relationship, with center deviation controlled within 0.1mm.
[0114] The localized transient cryogenic embrittlement module includes a liquid nitrogen storage and supply unit, a cryogenic delivery pipeline, an annular distribution chamber, and a micro-nozzle array. The liquid nitrogen storage and supply unit uses a 175L self-pressurized liquid nitrogen tank, with a working pressure set between 0.35MPa and 0.55MPa, preferably 0.45MPa. The cryogenic delivery pipeline uses a DN8 vacuum-insulated stainless steel flexible hose with an outer cold-insulating sheath, and the total pipeline length is controlled within 2.5m. The cryogenic control valve uses a cryogenic solenoid valve or a cryogenic pneumatic angle seat valve, with a valve response time of less than 20ms. The annular distribution chamber is made of 316L stainless steel and is located around the periphery of the die cutting edge; the distribution chamber has a rectangular cross-section of 6mm × 8mm or a circular cross-section with an inner diameter of 8mm.
[0115] The micro-nozzle array is arranged circumferentially along the shearing contour of the thick electrode post, with 24 to 36 nozzles, preferably 32. Each micro-nozzle has a nozzle diameter of 0.3 mm to 0.5 mm, preferably 0.4 mm; the angle between the nozzle axis and the billet surface is 25° to 40°, preferably 30°; and the distance from the nozzle outlet to the billet surface is 6 mm to 10 mm, preferably 8 mm. The micro-nozzle array is divided into four spray zones, corresponding to the two long and two short sides of the thick electrode post contour. Each zone is connected to the annular distribution chamber by an independent branch, and the flow rate is adjusted through a throttling orifice or a micro-pressure regulating valve, ensuring that the liquid nitrogen spray volume in the long side region is 10% to 20% higher than that in the short side region. This compensates for the temperature unevenness caused by the larger heat capacity and longer cooling path in the long contour region.
[0116] Before the punching action begins, the timing coordination control module controls the opening of the cryogenic solenoid valve, allowing liquid nitrogen to enter the annular distribution chamber through the cryogenic delivery pipeline. The liquid nitrogen is then sprayed onto the shearing area by a micro-nozzle array in a circumferentially surrounding and locally converging manner. The cryogenic spray advance is set to 180ms–260ms before the punch contacts the billet, preferably 220ms; the liquid nitrogen spray duration is set to 250ms–420ms, preferably 320ms; and the liquid nitrogen consumption per punch is 6g–12g, preferably 9g. After cryogenic spraying, the surface temperature of the shearing strip drops from room temperature (20℃) to -120℃–-160℃, preferably to around -140℃, causing the thick steel pole shearing strip to be in a cryogenic embrittlement state at the moment of punching.
[0117] The double-layer flow-guiding and reheating anti-frost shield module includes an inner cold flow converging shield and an outer reheating and flow-guiding shield. The inner cold flow converging shield is made of thin-walled 304 stainless steel with a thickness of 1.5mm to 2.0mm, and a confining flow-guiding surface facing the die opening area is provided on the inner side. The gap between the confining flow-guiding surface and the blank surface is 3mm to 5mm, preferably 4mm. The lower edge of the cold flow converging shield is 2mm to 4mm away from the outer side of the die cutting edge, forming a semi-enclosed local low-temperature spray space, so that the liquid nitrogen spray preferentially acts on the shear band area, reducing the diffusion of cold flow to the feeding area and the die body.
[0118] An outer rewarming guide shroud is fitted over the cold flow convergence shroud, forming an annular rewarming air channel with a width of 5mm to 8mm between them. The rewarming guide shroud is equipped with two rewarming gas inlets, four rewarming gas outlets, two mist outlets, and an annular condensation guide groove. The rewarming gas outlets face the die opening area and the area adjacent to the thick electrode section, with an outlet angle of 20° to 35°, preferably 25°. The condensation guide groove is 3mm to 5mm wide, with a 1° to 3° drainage slope at the bottom to drain the condensate generated during the rewarming process to the outside of the die, preventing condensate from entering the die cutting edge area.
[0119] The drying and rewarming gas supply module includes a drying gas source, a filter and pressure reducing valve, a pressure stabilizing tank, gas pipelines, and a control valve assembly. The drying gas source is selected from dried compressed air or dried nitrogen, with a dew point not exceeding -40℃ and a supply pressure of 0.4MPa to 0.6MPa. The pressure stabilizing tank has a volume of 3L to 5L, and the rewarming gas working pressure is 0.15MPa to 0.25MPa, preferably 0.2MPa; the rewarming gas flow rate is 80L / min to 120L / min, preferably 100L / min. The rewarming gas temperature is 25℃ to 40℃, preferably 35℃. After punching, the timing-coordinated control module starts the rewarming airflow 10mm after the punch returns to the upper surface of the billet, with a rewarming duration of 1.5s to 2.5s, preferably 2.0s. The dry rewarming airflow enters the rewarming outlet along the rewarming air passage, blowing around the mold opening, the area adjacent to the thick electrode section, and the area where low-temperature fog accumulates, thus achieving fog removal, frost prevention, and local rewarming.
[0120] The timing-coordinated control module consists of a PLC controller, a stroke detection unit, a temperature detection unit, a pressure detection unit, and an actuator valve group. The PLC controller is either a Siemens S7-1200 or a Mitsubishi FX5U series controller. The stroke detection unit uses a magnetic scale, photoelectric sensor, or servo encoder, with a stroke detection resolution of no less than 0.01mm. The temperature detection unit uses a high-speed infrared temperature probe with a response time of less than 1ms and a temperature range of -200℃ to 200℃. The pressure detection unit includes a liquid nitrogen pipeline pressure sensor and a rewarming gas pressure sensor. The control flow follows the sequence of "pre-punch cooling to induce brittleness—high-rigidity shearing during punching—post-punch guiding and rewarming": when the punch descends to a distance of 8mm to 12mm from the upper surface of the billet, liquid nitrogen injection is activated; after the punch enters the billet and completes shearing separation, liquid nitrogen injection is deactivated; after the punch returns and leaves the upper surface of the billet, the rewarming gas flow is activated; when the temperature in the die area rises above 0℃ and there is no obvious cold mist residue, the rewarming gas flow is deactivated.
[0121] The following is a comparison between this solution and existing technologies:
[0122] Comparative Example 1: Comparison of cross-sectional quality between room temperature punching and local transient cryogenic embrittlement punching.
[0123] The test conditions were as follows: the blank material was a Q235B steel thick pole with a thickness of 6.0 mm and an external dimension of 80 mm × 45 mm; the blanking speed was 120 mm / s; the blanking gap was 0.09 mm / side; and the number of samples per group was 50 pieces. Comparative Example 1 used room temperature blanking and did not set up a local transient deep cryogenic embrittlement module.
[0124] The following is a comparison table between this scheme and Comparative Example 1 in terms of cross-sectional quality. Figure 3 The corresponding effect images are shown below (to avoid excessive differences in the images of different comparison items, some comparison items are not shown in the images):
[0125]
[0126] The data in the table shows that, under the same material, thickness, and blanking clearance conditions, room temperature blanking mainly relies on the punch and die to forcibly shear the thick electrode material. The material undergoes significant plastic flow before fracture, resulting in large collapse angles, tear bands, and burrs. This proposed solution uses a liquid nitrogen micro-nozzle array to perform localized transient deep cryogenic treatment on the shear band before blanking. This rapidly cools the surface of the shear band on the thick steel electrode and induces a brittle fracture-dominated state. Subsequently, the punch and die complete the rigid shearing, resulting in a more concentrated fracture path, a smoother cross-section, and a significant reduction in burr height, collapse angle width, and tear band width.
[0127] Comparative Example 2: Comparison of continuous punching stability between the absence of a double-layer flow-guiding, reheating, and anti-frost cover and the presence of a double-layer flow-guiding, reheating, and anti-frost cover.
[0128] The experimental conditions were: continuous punching of 1000 steel thick pole blanks, liquid nitrogen injection pressure of 0.45 MPa, single injection time of 320 ms, and punching cycle of 6 pieces / min. Comparative Example 2 retained liquid nitrogen injection but did not include an inner cold flow containment hood and an outer reheating guide hood, employing only open injection and natural reheating. This scheme uses an inner cold flow containment hood, an outer reheating guide hood, a drying and reheating gas supply module, and a condensation guide trough.
[0129] The following table compares the stability of this scheme with that of Comparative Example 2 in the continuous punching process. Figure 4 The corresponding effect diagrams are shown below (to avoid excessive differences in the images of different comparison items, some comparison items are not shown in the diagrams).
[0130]
[0131] The data in the table shows that when only open-type liquid nitrogen injection is used, the cryogenic medium diffuses to the periphery of the mold and the feeding area, leading to increased liquid nitrogen consumption, frost formation at the die opening, cold fog retention, and a significant temperature drop in the mold body. This can easily cause problems such as unstable feeding, condensate buildup at the die opening, and burr height drift during continuous punching. This solution uses an inner cold flow converging hood to limit the liquid nitrogen jet to the vicinity of the shear zone. An outer reheating guide hood and a drying reheating gas supply module provide directional reheating and defogging to the die opening area after punching, concentrating the cooling energy in the effective processing area while preventing overcooling of the mold body and frost formation in the feeding area. This improves the stability of continuous punching and the consistency of batch processing.
[0132] The above-disclosed content is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Therefore, all equivalent technical changes made based on the description and drawings of the present invention are included within the scope of protection of the present invention. Furthermore, the elements therein can be updated as technology develops. The above units are merely examples, and those skilled in the art can adopt corresponding units according to actual needs when implementing this solution.
Claims
1. A large size thick pole post blanking system based on local transient deep cryogenic embrittlement, characterized by, include: The frame and drive module provide overall load-bearing capacity and high-load punching drive for the system; A large-size thick electrode precision blanking die module is installed on the frame and drive module and is used for positioning, holding, guiding, blanking and unloading of large-size thick electrode blanks; A localized transient cryogenic embrittlement module is arranged around the periphery of the large-size thick electrode precision stamping die module. It is used to perform localized, targeted low-temperature spraying on the working area of the large-size thick electrode precision stamping die module within a predetermined short period of time before the stamping action occurs. This causes the surface temperature of the working area to drop sharply below the brittle transition temperature of the material, thereby inducing the material to transform from a ductile fracture mode to a brittle fracture mode. The working area of the large-size thick electrode precision stamping die module is hereinafter referred to as the working area. The double-layer flow-guiding, reheating and anti-frost cover module is set around the large-size thick pole precision punching die module and around the local transient deep cryogenic embrittlement module. It is used to limit and concentrate the low-temperature jet during the low-temperature jetting stage, and to guide the flow, reheat, de-fog and prevent frost in the working area and its surrounding area after punching. The drying and rewarming gas supply module is connected to the double-layer flow-guiding rewarming and anti-frost cover module and is used to provide a drying and rewarming airflow to the double-layer flow-guiding rewarming and anti-frost cover module. The timing coordination control module is connected to the frame and drive module, the local transient cryogenic embrittlement module and the drying and reheating gas supply module respectively, and is used to control the opening and closing coordination of the local transient cryogenic injection and the reheating airflow according to the timing of the punching stroke. The large-size thick pole precision blanking die module includes an upper die base, a lower die base, a punch, a die cavity, a blanking structure, a guiding structure, and a blank positioning support structure. The local transient deep cryogenic embrittlement module includes a low-temperature medium source, a low-temperature delivery pipeline, an annular distribution cavity, and a micro-nozzle array. The double-layer flow guiding and reheating anti-frost cover module includes a cold flow convergence cover located on the inner side and a reheating flow guiding cover located on the outer side. The cold flow convergence cover and the periphery of the working area form a locally confined spray space, and the reheating flow guiding cover and the cold flow convergence cover form an annular or circumferentially connected reheating air passage. The timing coordination control module controls the local transient cryogenic embrittlement module to perform transient injection before the punch enters the working area, and controls the drying and reheating gas supply module to deliver a drying and reheating gas flow to the reheating gas channel after the punch completes the punching.
2. A system for blanking of large size thick pole pieces based on local transient cryogenic embrittlement as claimed in claim 1 wherein, The frame and drive module include a frame body, a slider drive mechanism, an upper die mounting base, and a lower die mounting base. The frame body is used to withstand the large punching force during the punching process of large-size thick pole posts. The slider drive mechanism is used to drive the upper die mounting base to reciprocate in a predetermined direction to ensure that the punch performs closed punching with high rigidity and high repeatability relative to the die.
3. A system for blanking of large size thick pole pieces based on local transient deep cryogenic embrittlement as claimed in claim 1 wherein, The pressing structure in the large-size thick electrode precision blanking die module includes one or more combinations of pressing plate, pressing ring or partitioned pressing component. The pressing structure is used to apply a stable pressing force to the surface of the blank before the large-size thick electrode blank is blanked. The guiding structure includes a guide post and guide sleeve pair, a guide slider pair, or a composite guide pair. The guiding structure is used to ensure the accuracy of the cutting edge clearance between the punch and the die and the motion stability during the large-contour punching process. The blank positioning support structure is used to support large-sized thick pole blanks and define the relative positional relationship between the blanking area and the punch, die and local low-temperature spraying area.
4. A system for blanking of large size thick pole pieces based on local transient deep cryogenic embrittlement as claimed in claim 1 wherein, The cryogenic medium source in the local transient cryogenic embrittlement module is a liquid nitrogen storage and supply unit, the cryogenic delivery pipeline is a cold-insulating delivery pipeline, the annular distribution cavity is located around the die cutting edge, and the micro-nozzle array is arranged around the periphery of the large-size thick pole blank to be sheared and inclined towards the working area, so as to spray the cryogenic medium into the working area in a circumferentially surrounding and locally converging manner, so that the blank enters a cryogenic embrittlement state for a short time before punching.
5. A system for blanking of large size thick pole pieces based on local transient deep cryogenic embrittlement as claimed in claim 1 wherein, The micro-nozzle array adopts a multi-nozzle partition structure, with each partition nozzle module connected to the annular distribution cavity. The multi-nozzle partition structure includes at least two sets of nozzle units arranged along the length and circumferential direction of the electrode profile. Each nozzle unit points to the working area with a predetermined tilt angle and a predetermined convergence direction to adapt to the characteristics of large-size thick electrode profiles with long profiles, large shear circumference, and high local heat capacity, ensuring the uniformity of low-temperature action along the entire punching profile.
6. A system for blanking of large size thick pole pieces based on local transient deep cryogenic embrittlement as claimed in claim 1 wherein, The cold flow convergence cover in the double-layer flow guiding and reheating anti-frost cover module is located near the die cutting edge. The cold flow convergence cover has a confined flow guiding surface facing the die opening area. The confined flow guiding surface, together with the outer periphery of the die cutting edge and the outer periphery of the working area, forms a semi-enclosed low-temperature spraying space, which is used to make the low-temperature medium sprayed by the local transient deep cryogenic embrittlement module act on the working area preferentially. The reheating guide hood in the double-layer flow guiding reheating anti-frost cover module is sleeved on the outside of the cold flow convergence cover, and the two form a ring or circumferentially connected reheating air channel. The reheating guide hood is provided with a reheating gas inlet, a flow guiding slope, and a reheating gas outlet facing the die area and the edge area of the thick electrode post. The reheating guide hood is used to transport the dry reheating airflow along a predetermined direction to the periphery of the cutting edge, above the die, and the area adjacent to the cross section of the thick electrode post blank after the blanking is completed. The double-layer flow-guiding reheating and anti-frost cover module also includes a mist vent and a condensation guide channel. The mist vent is used to discharge the low-temperature mist formed around the die opening during the punching process of large-size thick pole posts, and the condensation guide channel is used to directionally discharge the condensate formed during the reheating process.
7. A system for blanking of large size thick pole pieces based on local transient deep cryogenic embrittlement as claimed in claim 1 wherein, The drying and rewarming gas supply module includes a drying gas source, a pressure stabilizing unit, a gas supply pipeline, and a control valve group. The drying gas source is a dry air source or a dry nitrogen source. The pressure stabilizing unit is used to stabilize the rewarming gas flow pressure. The control valve group is used to provide intermittent or continuous rewarming gas flow to the rewarming gas channel under the control of the timing coordination control module.
8. A system for blanking of large size thick pole pieces based on local transient deep cryogenic embrittlement as claimed in claim 1 wherein, The timing-coordinated control module includes a stroke detection unit, a timing control unit, and an execution unit connected to the local transient cryogenic embrittlement module and the drying and reheating gas supply module. The stroke detection unit is used to detect the motion stages of the punch approaching the thick pole blank, starting shearing, and completing the punching separation. The timing control unit is used to control the start time of cryogenic injection, the duration of injection, the end time of injection, and the start and stop times of reheating airflow according to the motion stages, so as to form a coordinated workflow of short-term pre-punching cryogenic embrittlement, high-rigidity punching during punching, and post-punching guiding reheating and demisting.
9. A system for blanking of large size thick pole pieces based on local transient deep cryogenic embrittlement as claimed in claim 1 wherein, The system's workflow includes the following steps: S1. After the large-size thick electrode blank enters the punching station, the blank positioning and support structure completes the positioning and support, and the pressing structure stably presses the thick electrode blank above the die. S2, the timing coordination control module controls the liquid nitrogen to enter the annular distribution cavity through the cold-insulating delivery pipeline according to the punch stroke state, and then spray it into the working area along the shearing contour of the large-size thick pole by the micro-nozzle array; S3, the thick electrode blank changes from ductile fracture mode to brittle fracture mode; S4, the punch enters the thick pole blank under the guidance of the guide structure, and completes rigid shearing separation with the die; S5. After the punching is completed, the timing coordination control module controls the low temperature injection to be turned off or reduced, and at the same time starts the drying and reheating gas supply module. The drying airflow enters the outer reheating guide shroud, is guided by the reheating air passage and the guide slope, and blows towards the die area and the area adjacent to the thick pole section to quickly complete the defogging, anti-frost and local reheating. S6, residual mist is discharged from the mist outlet, and condensate is discharged from the condensate guide channel.
Citation Information
Patent Citations
Lifting type continuous blanking battery pole block forming method
CN120828085A