A moire fringe prevention micro-nano metal shielding net weaving method
By employing surface treatment, laser sintering, and eutectic bonding processes on micro/nano copper-tin-phosphorus alloy wires, combined with low-temperature rolling and stress-relief annealing, the balance between high light transmittance, broadband shielding, and moiré fringe suppression in micro/nano metal shielding meshes has been resolved, achieving a synergistic improvement in both efficient electromagnetic shielding and optical performance.
Patent Information
- Application Number
- CN202611375738.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to achieve a balance between high light transmittance, broadband shielding, and moiré fringe suppression in micro-nano metal shielding meshes. Furthermore, the periodic spatial distribution characteristics at the nodes of traditional plain weave are prone to interference and have high contact resistance, making it difficult to meet the large-format production requirements of high-transmittance electromagnetic shielding bulletproof transparent parts.
Micro-nano copper-tin-phosphorus alloy wires are used for surface degreasing and activation treatment. After warp and weft interlacing, pulsed laser dot matrix sintering treatment is performed and SnBi alloy powder is sprayed to form a eutectic bonding structure. Combined with low temperature rolling and stress relief annealing treatment, non-periodic node morphology is constructed to eliminate periodic high profile protrusions.
While maintaining high light transmittance and wide-band electromagnetic shielding effectiveness, it effectively suppresses the generation of moiré fringes, improves the joint strength and conductivity continuity of nodes, and ensures the structural stability and optical transmittance of the shielding mesh.
Smart Images

Figure CN123149336A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of electromagnetic protection functional materials technology, and more specifically, it relates to a method for weaving a micro / nano metal shielding mesh to prevent moiré patterns. Background Technology
[0002] Micro-nano metal shielding meshes, due to their combination of high light transmittance and excellent electromagnetic shielding properties, have been widely used in high-end transparent protection scenarios such as aerospace cockpit canopies and automotive optoelectronic sensor windows. Among them, the plain weave process has become the mainstream manufacturing route for metal shielding meshes due to its advantages such as high mesh uniformity, strong mechanical stability, and adaptability to large-format mass production. To address the moiré fringe interference problem that easily occurs during use, the existing mainstream suppression solutions mostly adopt methods such as randomizing the planar pattern of the mesh and laying irregularly shaped wires to alleviate display interference by disrupting the planar periodic spatial frequency of the mesh. Related technologies have been applied on a large scale in the field of consumer electronics touch control.
[0003] However, the related technologies all focus on the design optimization of the mesh planar pattern, without addressing the physical structure control at the plain weave nodes. Among them, the randomized pattern design has poor compatibility with the mature plain weave process in the screen industry, making it difficult to adapt to the large-format production needs of high-transmittance electromagnetic shielding bulletproof transparent parts. At the same time, the double-layer high-profile protrusions formed by the physical intersection of warp and weft threads at the traditional plain weave nodes still have periodic spatial distribution characteristics, which easily form a fixed phase difference with the display pixel array. Moreover, the high node contact resistance limits the improvement of shielding effectiveness, and it is always impossible to achieve a balance between high light transmittance, broadband shielding, and moiré fringe suppression. Summary of the Invention
[0004] To address the problem that the design optimization of related technologies using mesh planar patterns makes it impossible to achieve a balance between high light transmittance, broadband shielding, and moiré stripe suppression, this application provides a micro / nano metal shielding mesh weaving method for preventing moiré stripes.
[0005] This application provides a method for weaving micro / nano metal shielding mesh to prevent moiré patterns, employing the following technical solution: A method for weaving a micro / nano metallic shielding mesh to prevent moiré patterns includes the following steps: S1. The micro-nano copper-tin-phosphorus alloy wire is subjected to surface degreasing and activation treatment to obtain the wire material to be woven. S2. The filament to be woven is woven in a plain weave pattern to obtain a primary mesh blank with mesh areas and node areas. S3. The node region of the initial mesh blank is subjected to pulsed laser dot matrix sintering treatment, and SnBi alloy powder is sprayed into the node region to form a eutectic bonding structure of the warp and weft wires in the node region, thereby obtaining a transition mesh with continuous node conductivity. S4. The transition mesh is subjected to low-temperature rolling and stress-relief annealing treatments in sequence to obtain a micro-nano metal shielding mesh that is resistant to moiré patterns.
[0006] By adopting the above technical solution, the high conductivity and toughness of micro-nano copper-tin-phosphorus alloy wires are used as the matrix to construct a uniform mesh skeleton with plain weave. Metallurgical bonding of the node area is used to replace physical intersections, thereby eliminating periodic high-profile protrusions. While maintaining the compatibility of the plain weave process, this method controls the micro-morphology of the nodes to disrupt the spatial frequency consistency between the mesh surface and the pixel array of the display screen, thereby suppressing the generation of moiré fringes while ensuring high light transmittance and wide-band electromagnetic shielding effectiveness.
[0007] Preferably, step S1 further includes tension annealing of the micro-nano copper-tin-phosphorus alloy wire: the annealing tension is 5~15cN, the annealing temperature is 300~500℃, the wire feeding speed is 1~3m / min, and a pretreated wire with a grain size of 1~5μm and an elongation of ≥15% is obtained.
[0008] By adopting the above technical solution, axial tension is applied and heat treatment is performed during the movement of the micro-nano copper-tin-phosphorus alloy wire. The internal grain boundaries of the wire are reorganized, forming fine and uniform recrystallized grains, which improves the uniformity of the mechanical properties of the wire. The online tension annealing treatment eliminates the residual internal stress generated in the wire during the drawing process, making it less prone to brittle fracture in the subsequent bending and weaving process. At the same time, the elongation is controlled within an appropriate range to ensure the compactness of the weaving nodes and the dimensional stability of the subsequent rolling process.
[0009] Preferably, in step S1, the tin mass fraction in the micro-nano copper-tin-phosphorus alloy wire is 0.1%–0.5%, the phosphorus mass fraction is 0.01%–0.1%, and the balance is copper, with a diameter of 8–12 μm; the surface degreasing is performed by ultrasonic cleaning with a sodium carbonate solution of 5%–10% by volume, the ultrasonic power is 200–400 W, and the cleaning time is 3–8 min; the activation treatment is performed by argon-oxygen mixed plasma etching, the volume flow ratio of argon to oxygen is 4:(1–2), the etching power is 80–120 W, and the etching time is 1–3 min. After treatment, the surface roughness Ra of the filament to be woven is 0.05–0.2 μm, and the surface contact angle is ≤30°.
[0010] By adopting the above technical solution, the tin element in the copper-tin-phosphorus alloy improves the creep resistance of the wire, and the trace phosphorus element acts as a deoxidizer to purify the surface of the wire; alkaline ultrasonic cleaning removes drawing grease, and plasma etching removes the original oxide layer while introducing a controllable micro-nano-scale rough structure on the surface of the wire; this roughened surface increases the specific surface area and reduces the surface contact angle, so that the molten SnBi alloy powder in the subsequent steps can be fully wetted and spread, and a strong metallurgical bonding interface can be established.
[0011] Preferably, in step S2, the warp yarn arrangement density of the plain weave is 600~800 mesh, the weft yarn arrangement density is 600~800 mesh, the warp yarn tension fluctuation is controlled within ±0.5cN during the weaving process, the weft yarn tension fluctuation is controlled within ±0.3cN, and the mesh uniformity deviation of the obtained initial mesh blank is ≤2%.
[0012] By adopting the above technical solution, high-mesh plain weave forms a precise mesh array, providing a basic guarantee for shielding effectiveness; then, the tension fluctuation of the warp and weft yarns is controlled at the moment of weaving to avoid wrinkling of the mesh surface or deformation of the mesh caused by uneven tension; high-precision tension control keeps the mesh size consistent, which is conducive to uniform light transmission to improve imaging quality, and at the same time provides a stable focal length reference for subsequent laser dot matrix sintering, ensuring that each node receives uniform energy input.
[0013] Preferably, in step S3, the laser wavelength of the pulsed laser dot matrix sintering is 1064nm, the spot diameter is 0.8 to 1.2 times the diameter of the wire, the pulse width is 0.1 to 1ms, the pulse energy is 0.5 to 2mJ, the processing time interval between adjacent nodes is 10 to 50ms, and the scanning path only covers the node area.
[0014] By adopting the above technical solution, near-infrared lasers are selected and absorbed by the metal surface. By matching the spot diameter to the wire diameter, energy is localized. The short pulse width setting concentrates energy at the node overlap in a very short time, instantly reaching the melting temperature of SnBi alloy, avoiding thermal damage or annealing softening to the surrounding copper wire substrate. The dot matrix scanning path confines heat to the micro-region of the node, preventing the heat-affected zone from spreading and causing a decrease in the overall strength of the mesh.
[0015] Preferably, in step S3, the mass ratio of bismuth to tin in the SnBi alloy powder is (57~59):(41~43), the particle size is 1~3μm, the spray flow rate is 5~20mg / s, the preheating temperature of the alloy powder during spraying is 100~130℃, and the thickness of the eutectic bonding layer formed with the warp and weft wires after melting is 0.5~1.5μm; the profile height of the node region of the obtained transition mesh is 1.1~1.3 times the diameter of the wire.
[0016] By adopting the above technical solution, a bismuth-tin alloy with a specific mass ratio forms a low-melting-point eutectic system, which melts rapidly under laser action and spreads and wets the surface of copper wire; the preheated alloy powder reduces the heat load of laser energy and prevents the powder from splashing due to excessive temperature difference; the molten liquid alloy fills the micro-pits on the surface of the wire and the overlapping gaps of the warp and weft wires under the action of capillary force, and forms a dense eutectic bonding layer after cooling; this low-profile bonding structure connects the originally physically contacting double-layer wires into a whole, reduces the actual height of the node, destroys the periodic spatial distribution characteristics of the equal height and equal spacing of the traditional plain weave nodes, and blocks the conditions for the generation of moiré fringes.
[0017] Preferably, in step S3, the conductivity of the node region of the transition mesh is 90% to 98% of the conductivity of the filament body to be woven, the standard deviation of the node height within any 10mm×10mm region is ≤0.1μm, and the shear strength of the node region is ≥15MPa.
[0018] By adopting the above technical solution, the high conductivity node bonding layer eliminates the contact resistance present in traditional woven mesh, constructs a continuous and unobstructed conductive network, and ensures the shielding effectiveness of high-frequency electromagnetic waves; controlling the small standard deviation of node height keeps the mesh surface flatness at a high level, reduces light scattering to improve transmittance, and at the same time ensures that the node morphology is statistically non-periodic, so that the local node height difference cannot form a fixed phase difference with the periodic pixels of the display screen, thus achieving the effect of preventing moiré stripes at the physical level.
[0019] Preferably, in step S4, the reduction of the low-temperature rolling is 5% to 15% of the wire diameter, the surface roughness of the roll Ra is ≤0.02μm, the rolling speed is 0.5 to 2m / min, and the oxygen content of the rolling environment is ≤100ppm.
[0020] By adopting the above technical solutions, the low-temperature rolling process further compacts the eutectic bonding layer in the node area, making it more tightly bonded to the matrix. At the same time, the absolute height of the node is further reduced through slight plastic deformation, making it close to the thickness of a single layer of wire. The mirror-grade roll surface ensures that the mesh surface is not scratched again, maintaining the surface smoothness. Rolling in a low-oxygen environment prevents oxidation and discoloration of the metal surface under high temperature and high pressure, ensuring the optical transmittance and appearance quality of the final product.
[0021] Preferably, in step S4, the stress relief annealing temperature is 150~250℃, the holding time is 10~30min, the heating rate is 5~10℃ / min, and the cooling rate is 3~8℃ / min.
[0022] By adopting the above technical solution, precise stress-relieving annealing is performed after low-temperature rolling to eliminate microscopic residual stress generated during weaving, laser sintering, and rolling. Appropriate holding time and heating / cooling rate are used to avoid material performance degradation caused by temperature shock and prevent the mesh from relaxing and deforming at high temperatures. This step stabilizes the microstructure of the mesh, ensuring that the shielding mesh does not warp or spring back in size during subsequent cutting, handling, and bonding with bulletproof transparent parts, thus maintaining the long-term stability of the overall structure.
[0023] Preferably, in step S4, after low-temperature rolling and before stress-relief annealing, an argon-hydrogen mixed gas plasma cleaning is also included, wherein the volume flow ratio of argon to hydrogen is 1:(1~2), the cleaning power is 50~100W, and the cleaning time is 3~8min.
[0024] By adopting the above technical solution, the reducing properties of hydrogen are used to remove the extremely thin oxide film generated during the rolling process under plasma excitation, restoring a clean and active metal surface. Argon is used as a protective gas and sputtering ion source to assist in cleaning the physically adsorbed impurity particles on the surface. This cleaning process occurs before annealing, ensuring that the metal surface is in a highly active state during subsequent heat treatment, promoting atomic diffusion and grain boundary migration, further improving the node bonding strength, and avoiding the impact of oxide inclusions on shielding performance and light transmittance.
[0025] In summary, this application has the following beneficial effects: 1. Because this application uses plain weave to construct the mesh skeleton and uses the metallurgical bonding structure of the node area to replace the physical cross-over of the wire, the periodic high profile protrusions are eliminated; and the node morphology presents a non-periodic distribution, which blocks the conditions for generating a fixed phase difference with the display pixel array, thereby achieving the suppression of moiré fringes while ensuring high light transmittance and wide-band electromagnetic shielding effectiveness.
[0026] 2. In this application, a pretreatment process combining online tension annealing and surface micro-roughening activation is preferred. Since heat treatment eliminates residual internal stress inside the wire and roughening the surface improves the wetting and spreading ability of low melting point alloys, the mechanical ductility and joint strength of the wire are improved simultaneously, laying a structural foundation for subsequent precision weaving and low profile rolling.
[0027] 3. In this application, a node construction process using localized pulsed laser sintering combined with eutectic alloy powder filling is preferred. Since the laser energy is precisely limited to the warp and weft wire overlap, combined with the capillary filling effect of molten metal, the conductivity continuity of the node is reconstructed in the low heat-affected zone. This process reduces the node contact resistance to improve shielding effectiveness, while disrupting the spatial frequency consistency of the braided mesh through the low-profile bonding layer, thus achieving a synergistic effect of moiré resistance and high shielding.
[0028] 4. The method of this application, through the combination of low-temperature rolling and stress-relief annealing processes, further compacts the joint layer and reduces the thickness of the mesh while eliminating residual stress generated during processing; as the flatness and structural stability of the mesh are improved, warping deformation during subsequent composite use is avoided, thus obtaining the reliability suitable for high-transmittance electromagnetic shielding bulletproof transparent parts. Attached Figure Description
[0029] Figure 1 A flowchart illustrating a method for weaving a micro / nano metallic shielding mesh to prevent moiré patterns, as proposed in this application; Figure 2 This is a schematic diagram showing the test results of the optical and electrical performance of the embodiments and comparative examples in this application; Figure 3 This is a schematic diagram showing the test results of the nodal shear strength in the embodiments and comparative examples of this application; Figure 4 This is a schematic diagram showing the test results of the bending resistance of the embodiments and comparative examples in this application. Detailed Implementation
[0030] The present application will be further described in detail below with reference to the accompanying drawings and embodiments.
[0031] Technical concept: This application discloses a method for weaving a micro / nano metallic shielding mesh to prevent moiré patterns. The method includes the following steps: S1, surface degreasing and activation treatment of micro / nano copper-tin-phosphorus alloy wires to obtain the wire material to be woven; S2, weaving the wire material into a plain weave pattern to obtain a primary mesh blank with mesh areas and node areas; S3, pulsed laser dot-array sintering treatment of the node areas of the primary mesh blank, while simultaneously spraying SnBi-based alloy powder into the node areas, so that the warp and weft wires in the node areas form a eutectic bonding structure, obtaining a transition mesh with continuous node conductivity; S4, sequentially subjecting the transition mesh to low-temperature rolling and stress-relief annealing treatments to obtain a micro / nano metallic shielding mesh to prevent moiré patterns.
[0032] This application uses plain weave to construct the mesh skeleton and uses the metallurgical bonding structure of the node area to replace the physical cross-over of the wire material, thereby eliminating periodic high profile protrusions; while the node morphology presents a non-periodic distribution, blocking the conditions for generating a fixed phase difference with the display pixel array, thereby achieving the suppression of moiré fringes while ensuring high light transmittance and wide-band electromagnetic shielding effectiveness.
[0033] Example 1: This example provides a method for weaving a micro / nano metal shielding mesh to prevent moiré stripes, including the following steps: S1. The micro-nano copper-tin-phosphorus alloy wire is subjected to surface degreasing and activation treatment to obtain the wire material to be woven.
[0034] The micro-nano copper-tin-phosphorus alloy wire has a tin mass fraction of 0.1%, a phosphorus mass fraction of 0.01%, and the balance is copper, with a diameter of 8μm. Surface degreasing is performed using a 5% sodium carbonate solution with ultrasonic cleaning at a power of 200W for 8 minutes. Activation treatment is achieved using argon-oxygen mixed plasma etching at a volume flow ratio of 4:1, an etching power of 80W, and an etching time of 3 minutes. After treatment, the surface roughness Ra of the filament to be woven is 0.05μm, and the surface contact angle is 30°. Before step S1, the micro-nano copper-tin-phosphorus alloy wire undergoes tension annealing at a tension of 5cN, an annealing temperature of 300℃, and a wire feed speed of 1–3 m / min to obtain a pre-treated filament with a grain size of 1–5μm and an elongation ≥15%.
[0035] S2. The filaments to be woven are interwoven in a plain weave pattern to obtain a primary mesh blank with mesh areas and node areas.
[0036] Among them, the warp yarn arrangement density of plain weave is 600 mesh, the weft yarn arrangement density is 600 mesh, the warp yarn tension fluctuation is controlled within ±0.5cN during the weaving process, the weft yarn tension fluctuation is controlled within ±0.3cN, and the mesh uniformity deviation of the resulting raw mesh blank is ≤2%.
[0037] S3. The node region of the initial mesh blank is subjected to pulsed laser dot matrix sintering treatment, and SnBi alloy powder is sprayed into the node region to form a eutectic bonding structure of the warp and weft wires in the node region, thus obtaining a continuous conductive transition mesh.
[0038] The pulsed laser sintering process uses a laser wavelength of 1064 nm, a spot diameter 0.8 times the wire diameter, a pulse width of 0.1 ms, a pulse energy of 0.5 mJ, a processing time interval of 50 ms between adjacent nodes, and a scanning path that only covers the node region. The SnBi alloy powder has a bismuth to tin mass ratio of 57:41, a particle size of 1 μm, a spray flow rate of 5 mg / s, a preheating temperature of 100℃ during spraying, and a eutectic bonding layer thickness of 0.5 μm formed with the warp and weft wires after melting. The height of the node region profile of the resulting transition mesh is 1.1 times the wire diameter, the conductivity of the node region is 90% of the conductivity of the woven wire body, the standard deviation of the node height within any 10 mm × 10 mm region is ≤0.1 μm, and the shear strength of the node region is ≥15 MPa.
[0039] S4. The transition mesh is subjected to low-temperature rolling and stress-relieving annealing treatments in sequence to obtain a micro-nano metal shielding mesh that prevents moiré stripes.
[0040] The process includes: a reduction of 5% of the wire diameter in low-temperature rolling, a roll surface roughness Ra≤0.02μm, a rolling speed of 0.5m / min, and an oxygen content of ≤100ppm in the rolling environment; a stress-relieving annealing temperature of 150℃, a holding time of 10min, a heating rate of 5℃ / min, and a cooling rate of 3℃ / min; and argon-hydrogen mixed gas plasma cleaning after low-temperature rolling and before stress-relieving annealing, with an argon to hydrogen volume flow ratio of 1:1, a cleaning power of 50W, and a cleaning time of 8min.
[0041] Example 2: This example provides a method for weaving a micro / nano metal shielding mesh to prevent moiré patterns, including the following steps: S1. The micro-nano copper-tin-phosphorus alloy wire is subjected to surface degreasing and activation treatment to obtain the wire material to be woven.
[0042] The micro-nano copper-tin-phosphorus alloy wire contains 0.3% tin and 0.05% phosphorus by mass, with the balance being copper, and has a diameter of 10 μm. Surface degreasing is performed using a 7.5% sodium carbonate solution with ultrasonic cleaning at a power of 300 W for 5.5 min. Activation treatment is achieved using argon-oxygen mixed plasma etching at a volume flow ratio of 4:1.5, an etching power of 100 W, and an etching time of 2 min. After treatment, the surface roughness Ra of the filament to be woven is 0.125 μm, and the surface contact angle is 15°. Before step S1, the micro-nano copper-tin-phosphorus alloy wire undergoes tension annealing at a tension of 10 cN, an annealing temperature of 400℃, and a wire feed speed of 2 m / min to obtain a pre-treated filament with a grain size of 3 μm and an elongation ≥15%.
[0043] S2. The filaments to be woven are interwoven in a plain weave pattern to obtain a primary mesh blank with mesh areas and node areas.
[0044] The plain weave has a warp density of 700 mesh and a weft density of 700 mesh. During the weaving process, the warp tension fluctuation is controlled within ±0.5 cN and the weft tension fluctuation is controlled within ±0.3 cN. The mesh uniformity deviation of the resulting raw mesh blank is ≤1%.
[0045] S3. The node region of the initial mesh blank is subjected to pulsed laser dot matrix sintering treatment, and SnBi alloy powder is sprayed into the node region to form a eutectic bonding structure of the warp and weft wires in the node region, thus obtaining a continuous conductive transition mesh.
[0046] The pulsed laser sintering process used a laser wavelength of 1064 nm, a spot diameter 1.0 times the wire diameter, a pulse width of 0.55 ms, a pulse energy of 1.25 mJ, a processing time interval of 30 ms between adjacent nodes, and a scanning path that only covered the node region. The SnBi alloy powder had a bismuth to tin mass ratio of 58:42, a particle size of 2 μm, a jet flow rate of 12.5 mg / s, a preheating temperature of 115℃ during jetting, and a eutectic bonding layer thickness of 1.0 μm formed with the warp and weft wires after melting. The height of the node region profile of the resulting transition mesh was 1.2 times the wire diameter, the conductivity of the node region was 94% of the conductivity of the woven wire body, the standard deviation of the node height within any 10 mm × 10 mm region was ≤0.05 μm, and the shear strength of the node region was ≥22 MPa.
[0047] S4. The transition mesh is subjected to low-temperature rolling and stress-relieving annealing treatments in sequence to obtain a micro-nano metal shielding mesh that prevents moiré stripes.
[0048] The process includes: a reduction of 10% of the wire diameter in low-temperature rolling, a roll surface roughness Ra≤0.01μm, a rolling speed of 1.25m / min, and an oxygen content of ≤50ppm in the rolling environment; a stress-relieving annealing temperature of 200℃, a holding time of 20min, a heating rate of 7.5℃ / min, and a cooling rate of 5.5℃ / min; and an argon-hydrogen mixed gas plasma cleaning process after low-temperature rolling and before stress-relieving annealing, with an argon to hydrogen volume flow rate ratio of 1:1.5, a cleaning power of 75W, and a cleaning time of 5.5min.
[0049] Example 3: This example provides a method for weaving a micro / nano metal shielding mesh to prevent moiré patterns, including the following steps: S1. The micro-nano copper-tin-phosphorus alloy wire is subjected to surface degreasing and activation treatment to obtain the wire material to be woven.
[0050] The micro-nano copper-tin-phosphorus alloy wire has a tin mass fraction of 0.5%, a phosphorus mass fraction of 0.1%, and the balance is copper, with a diameter of 12μm. Surface degreasing is performed using a 10% sodium carbonate solution with ultrasonic cleaning at a power of 400W for 3 minutes. Activation treatment is achieved using argon-oxygen mixed plasma etching at a volume flow ratio of 4:2, an etching power of 120W, and an etching time of 1 minute. After treatment, the surface roughness Ra of the filament to be woven is 0.2μm, and the surface contact angle is ≤30°. Before step S1, the micro-nano copper-tin-phosphorus alloy wire undergoes tension annealing at a tension of 15cN, an annealing temperature of 500℃, and a wire feed speed of 3m / min to obtain a pre-treated filament with a grain size of 5μm and an elongation ≥15%.
[0051] S2. The filaments to be woven are interwoven in a plain weave pattern to obtain a primary mesh blank with mesh areas and node areas.
[0052] Among them, the warp yarn arrangement density of plain weave is 800 mesh, the weft yarn arrangement density is 800 mesh, the warp yarn tension fluctuation is controlled within ±0.5cN during the weaving process, the weft yarn tension fluctuation is controlled within ±0.3cN, and the mesh uniformity deviation of the resulting raw mesh blank is ≤0.5%.
[0053] S3. The node region of the initial mesh blank is subjected to pulsed laser dot matrix sintering treatment, and SnBi alloy powder is sprayed into the node region to form a eutectic bonding structure of the warp and weft wires in the node region, thus obtaining a continuous conductive transition mesh.
[0054] The pulsed laser sintering process uses a laser wavelength of 1064 nm, a spot diameter 1.2 times the wire diameter, a pulse width of 1.0 ms, a pulse energy of 2.0 mJ, a processing time interval of 10 ms between adjacent nodes, and a scanning path that only covers the node region. The SnBi alloy powder has a bismuth to tin mass ratio of 59:43, a particle size of 3 μm, a spray flow rate of 20 mg / s, a preheating temperature of 130℃ during spraying, and a eutectic bonding layer thickness of 1.5 μm formed with the warp and weft wires after melting. The height of the node region profile of the resulting transition mesh is 1.3 times the wire diameter, the conductivity of the node region is 98% of the conductivity of the woven wire body, the standard deviation of the node height within any 10 mm × 10 mm region is ≤0.01 μm, and the shear strength of the node region is ≥30 MPa.
[0055] S4. The transition mesh is subjected to low-temperature rolling and stress-relieving annealing treatments in sequence to obtain a micro-nano metal shielding mesh that prevents moiré stripes.
[0056] The process includes: a reduction of 15% of the wire diameter in low-temperature rolling, a roll surface roughness Ra≤0.01μm, a rolling speed of 2m / min, and an oxygen content of ≤10ppm in the rolling environment; a stress-relieving annealing temperature of 250℃, a holding time of 30min, a heating rate of 10℃ / min, and a cooling rate of 8℃ / min; and argon-hydrogen mixed gas plasma cleaning after low-temperature rolling and before stress-relieving annealing, with an argon to hydrogen volume flow ratio of 1:2, a cleaning power of 100W, and a cleaning time of 3min.
[0057] Comparative Example 1: This comparative example refers to the content of Example 1, except that the micro-nano copper-tin-phosphorus alloy wire does not contain phosphorus, that is, the mass fraction of phosphorus is 0%, and the rest is the same as Example 1.
[0058] Comparative Example 2: This comparative example refers to the content of Example 1, except that the activation treatment is omitted in step S1, only surface degreasing and cleaning are performed, and argon-oxygen mixed plasma etching is not performed. The rest of the content is the same as Example 1.
[0059] Comparative Example 3: This comparative example refers to the content of Example 1, except that the warp yarn arrangement density of the plain weave in step S2 is 400 mesh and the weft yarn arrangement density is 400 mesh, and the rest is the same as Example 1.
[0060] Comparative Example 4: This comparative example refers to the content of Example 1, except that in step S3, the scanning path of the pulsed laser dot matrix sintering covers the entire mesh surface, rather than just the node area. The rest of the content is the same as in Example 1.
[0061] Comparative Example 5: This comparative example refers to the content of Example 1, except that SnBi alloy powder was not sprayed into the node area in step S3. Instead, the warp and weft wires were directly sintered together by pulsed laser. The rest of the content is the same as in Example 1.
[0062] Comparative Example 6: This comparative example refers to the content of Example 1, except that the stress relief annealing process is omitted in step S4, and natural cooling is only performed after low-temperature rolling. The rest of the content is the same as that of Example 1.
[0063] Performance testing Sample preparation: The micro-nano metal shielding meshes prepared in each example and comparative example were cut into 100mm×100mm square samples. The surface of the samples was wiped with anhydrous ethanol to remove the attached contaminants. Then, the samples were placed in an environment with a temperature of 23℃ and a relative humidity of 50% for 24 hours to eliminate the interference of environmental temperature and humidity fluctuations on the test results. After the pretreatment was completed, each sample was numbered and marked for later use.
[0064] Moiré fringe rating test: The test sample is flatly attached to one side of the display surface of a standard LCD screen. The screen is loaded with a full white test image. Under a D65 standard light source with an illuminance of 1000lx, five testers with normal vision observe the interference between the sample and the pixel array of the display screen from the frontal view and within a ±30° viewing angle. The moiré fringe rating is evaluated according to a four-level standard: no visible fringes, slightly visible and not affecting observation, obviously visible and affecting observation, and severely visible and obscuring the image. This test method is a routine visual evaluation method in this field.
[0065] Electromagnetic shielding effectiveness test: The test sample is cut to fit the size of the coaxial transmission line test fixture and installed between the test ports of the vector network analyzer. A full-band scan is performed in the frequency range of 10kHz to 18GHz, and the difference between the incident electromagnetic wave power and the transmitted electromagnetic wave power is recorded simultaneously. The minimum value of the full-band is taken as the electromagnetic shielding effectiveness value of the sample. This test is performed in accordance with GB / T 30142-2013 Method for measuring the shielding effectiveness of planar electromagnetic shielding materials.
[0066] Visible light transmittance test: The test sample is cut into a regular 50mm×50mm sample and placed in the integrating sphere test port of the UV-Vis spectrophotometer. The spectrum is scanned in the visible light wavelength range of 400nm~700nm. The average transmittance of the scanned band is taken as the visible light transmittance test result of the sample. This test is performed according to the integrating sphere method of GB / T 25273-2025 Determination of Haze and Transmittance of Thin Films for Liquid Crystal Displays.
[0067] Node conductivity testing: The sample to be tested is fixed on the insulating base of the four-probe test stage. The spacing of the four probes is adjusted to 1500μm. First, the probe group is aligned with the wire body area away from the node, and the resistivity of the wire body is measured. Then, the probe group is aligned with the node area, and the resistivity of the node area is measured under the same test current conditions. The ratio of the resistivity of the node area to the resistivity of the wire body is calculated to obtain the relative value of node conductivity. This test is performed in accordance with GB / T 351-2019 Method for Measurement of Resistivity of Metallic Materials.
[0068] Nodal shear strength testing: The test sample is fixed on a precision fixture on a micromechanical testing table. A diamond flat-head indenter with a tip diameter of 50μm is used to apply a uniform downward load to the center of a single nodal area. The load-displacement curve is recorded in real time. The peak load at which the nodal fails is extracted and divided by the actual joint area of the nodal to calculate the shear strength value of the nodal. This test is performed in accordance with GB / T 228.1-2021 Metallic materials, tensile testing - Part 1: Basic principles of mechanical testing methods at room temperature, using the micromechanical indenter shear method.
[0069] Mesh surface flatness test: The test sample is laid flat on the stage of the white light interferometer. Ten 10mm×10mm test areas are randomly selected on the sample surface. The surface morphology of each area is scanned. The arithmetic mean and standard deviation of the height of all nodes in each area are recorded. The average of the standard deviations of the ten areas is taken as the evaluation index of mesh surface flatness. The smaller the standard deviation, the higher the mesh surface flatness. This test is performed in accordance with the morphology test principle of geometric tolerance test and verification of product geometric technical specifications in GB / T 1958-2017.
[0070] Bending resistance test: The test sample is cut into strips of 100mm×20mm and installed on a reciprocating bending tester with a mandrel diameter of 5mm. It is bent 180° at a frequency of 30 times / min. After every 100 bends, the electromagnetic shielding effectiveness and visible light transmittance of the sample are tested. The decay rate of the performance relative to the initial value is calculated. When the decay rate of any performance exceeds 10%, the test is stopped. The cumulative number of bends is recorded as the evaluation index of bending resistance. This test is performed in accordance with the basic principles of fatigue test of GB / T15248-2008 Axial constant amplitude low cycle fatigue test method for metallic materials, using the reciprocating bending self-test method.
[0071] Table 1: Moiré Fringe Grades and Optical and Electrical Properties
[0072] Table 2: Node electrical conductivity and mechanical properties
[0073] Table 3: Mesh morphology and structural stability
[0074] Table 4: Service Reliability and Bending Resistance
[0075] Example Conclusion: Combined with Examples 1-3 and Comparative Example 1 and Table 2, it can be seen that the presence of phosphorus in the micro-nano copper-tin-phosphorus alloy wire has an impact on the metallurgical bonding quality of the nodes. As a surface-active element, phosphorus can effectively purify the oxide film on the surface of the wire and promote the diffusion of interfacial atoms, thereby significantly improving the bonding strength and conductivity continuity of the node region, which confirms the influence of alloy composition design on the construction of high-performance shielding networks.
[0076] As can be seen from Examples 1-3 and Comparative Example 2, and Tables 2 and 3, the micro-nano-scale rough structure introduced by the surface activation treatment significantly improves the physicochemical properties of the wire surface. This structure not only increases the specific surface area, but also reduces the surface contact angle of the molten metal, allowing the low-melting-point alloy powder to be fully wetted and spread under the action of capillary force, thereby reducing the standard deviation of node height and improving shear strength, demonstrating the influence of the pretreatment process on the subsequent node construction.
[0077] As can be seen from Examples 1-3 and Comparative Example 3, and Tables 1 and 3, the dense mesh structure formed by high-mesh-count plain weave is a prerequisite for achieving a balance between optical and electromagnetic performance. The high-density weave on the substrate that ensures uniform light transmission, combined with the subsequent low-profile processing of the nodes, effectively destroys the conditions for interference between the mesh and the pixel array of the display screen, verifying the influence of precision weaving technology on suppressing moiré fringes.
[0078] As can be seen from Examples 1-3 and Comparative Example 4, and Tables 2 and 4, the localized energy control process of pulsed laser dot matrix sintering can avoid large-area thermal damage to the wire matrix by precisely limiting the laser energy to the micro-region of the node, thus maintaining the overall mechanical properties and structural stability of the mesh. This low-heat-input processing mode is the guarantee for achieving high-precision forming and long-term service of micro-nano wire mesh.
[0079] Combining Examples 1-3 and Comparative Example 5 with Tables 1 and 2, it can be seen that the eutectic filling effect of SnBi alloy powder establishes a synergistic mechanism between preventing moiré fringes and improving shielding effectiveness. While the molten alloy forms a low-profile continuous conductive path in the gaps of the filling nodes, it eliminates the interference source of periodic high-profile protrusions in the woven mesh, proving the role of the node integrated construction process in achieving multifunctional integration.
[0080] As can be seen from Examples 1-3 and Comparative Example 6, and Tables 3 and 4, the stress relief annealing process has an impact on eliminating work hardening and residual stress. This process effectively releases the microscopic internal stress generated during weaving, sintering and rolling, improves the flatness and fatigue resistance of the mesh surface, and ensures the geometric stability and long-term reliability of the shielding mesh in subsequent composite and complex environments.
[0081] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A method for weaving a micro / nano metallic shielding mesh to prevent moiré stripes, characterized in that, Includes the following steps: S1. The micro-nano copper-tin-phosphorus alloy wire is subjected to surface degreasing and activation treatment to obtain the wire material to be woven. S2. The filament to be woven is woven in a plain weave pattern to obtain a primary mesh blank with mesh areas and node areas. S3. The node region of the initial mesh blank is subjected to pulsed laser dot matrix sintering treatment, and SnBi alloy powder is sprayed into the node region to form a eutectic bonding structure of the warp and weft wires in the node region, thereby obtaining a transition mesh with continuous node conductivity. S4. The transition mesh is subjected to low-temperature rolling and stress-relief annealing treatments in sequence to obtain a micro-nano metal shielding mesh that is resistant to moiré patterns.
2. The method for weaving a micro / nano metal shielding mesh to prevent moiré stripes according to claim 1, characterized in that, In step S1, tension annealing of the micro-nano copper-tin-phosphorus alloy wire is also included: the annealing tension is 5~15cN, the annealing temperature is 300~500℃, the wire feeding speed is 1~3m / min, and a pretreated wire with a grain size of 1~5μm and an elongation of ≥15% is obtained.
3. The method for weaving a micro / nano metal shielding mesh to prevent moiré patterns according to claim 1, characterized in that, In step S1, the tin mass fraction in the micro-nano copper-tin-phosphorus alloy wire is 0.1%–0.5%, the phosphorus mass fraction is 0.01%–0.1%, and the balance is copper, with a diameter of 8–12 μm. The surface degreasing is performed by ultrasonic cleaning with a sodium carbonate solution of 5%–10% by volume, with an ultrasonic power of 200–400 W and a cleaning time of 3–8 min. The activation treatment is performed by argon-oxygen mixed plasma etching, with an argon to oxygen volume flow rate ratio of 4:(1–2), an etching power of 80–120 W, and an etching time of 1–3 min. After the treatment, the surface roughness Ra of the filament to be woven is 0.05–0.2 μm, and the surface contact angle is ≤30°.
4. The method for weaving a micro / nano metal shielding mesh to prevent moiré patterns according to claim 1, characterized in that, In step S2, the warp yarn arrangement density of plain weave is 600~800 mesh, the weft yarn arrangement density is 600~800 mesh, the warp yarn tension fluctuation during weaving is controlled within ±0.5cN, the weft yarn tension fluctuation is controlled within ±0.3cN, and the mesh uniformity deviation of the obtained initial mesh blank is ≤2%.
5. The method for weaving a micro / nano metallic shielding mesh to prevent moiré stripes according to claim 1, characterized in that, In step S3, the laser wavelength of the pulsed laser dot matrix sintering is 1064nm, the spot diameter is 0.8 to 1.2 times the diameter of the wire, the pulse width is 0.1 to 1ms, the pulse energy is 0.5 to 2mJ, the processing time interval between adjacent nodes is 10 to 50ms, and the scanning path only covers the node area.
6. The method for weaving a micro / nano metal shielding mesh to prevent moiré stripes according to claim 1, characterized in that, In step S3, the mass ratio of bismuth to tin in the SnBi alloy powder is (57~59):(41~43), the particle size is 1~3μm, the spray flow rate is 5~20mg / s, the preheating temperature of the alloy powder during spraying is 100~130℃, and the thickness of the eutectic bonding layer formed with the warp and weft wires after melting is 0.5~1.5μm; the profile height of the node region of the obtained transition mesh is 1.1~1.3 times the diameter of the wire.
7. The method for weaving a micro / nano metal shielding mesh to prevent moiré patterns according to claim 1, characterized in that, In step S3, the conductivity of the node area of the transition mesh is 90% to 98% of the conductivity of the filament body to be woven, the standard deviation of the node height in any 10mm×10mm area is ≤0.1μm, and the shear strength of the node area is ≥15MPa.
8. The method for weaving a micro / nano metal shielding mesh to prevent moiré patterns according to claim 1, characterized in that, In step S4, the reduction in low-temperature rolling is 5% to 15% of the wire diameter, the surface roughness of the rolls Ra ≤ 0.02 μm, the rolling speed is 0.5 to 2 m / min, and the oxygen content of the rolling environment is ≤ 100 ppm.
9. The method for weaving a micro / nano metal shielding mesh to prevent moiré patterns according to claim 1, characterized in that, In step S4, the stress relief annealing temperature is 150~250℃, the holding time is 10~30min, the heating rate is 5~10℃ / min, and the cooling rate is 3~8℃ / min.
10. The method for weaving a micro / nano metal shielding mesh to prevent moiré stripes according to claim 1, characterized in that, In step S4, after low-temperature rolling and before stress-relief annealing, there is also argon-hydrogen mixed gas plasma cleaning, in which the volume flow ratio of argon to hydrogen is 1:(1~2), the cleaning power is 50~100W, and the cleaning time is 3~8min.