A method for forging a large-size bar of an ultrafine-grained high-temperature titanium alloy
By combining water quenching above the β phase transformation point, low-temperature water quenching in the two-phase region, and two large-ratio forging deformations in the two-phase region, the problem of uneven microstructure in large-size high-temperature titanium alloy bars was solved, achieving a uniform ultrafine grain structure and improved performance.
Patent Information
- Application Number
- CN202611612305.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies make it difficult to achieve a uniform ultrafine grain structure in large-size high-temperature titanium alloy bars, resulting in large differences between the core and surface structures, which easily leads to mixed grains and coarse grains, making it difficult to meet the batch consistency requirements of high-reliability components.
The process employs a combination of water quenching above the β-phase transformation point, low-temperature water quenching in the two-phase region, and two large-ratio forging deformations in the two-phase region. This includes heating, heat preservation, water quenching, and multiple upsetting and drawing deformations to ensure that the microstructure is completely transformed into the β-phase before rapid cooling and uniform deformation, combined with appropriate heating coefficients and heat preservation time control.
A uniform equiaxed ultrafine grain structure with an average grain size of 300~400nm was obtained, eliminating mixed grains and coarse grains, improving the uniformity of the structure and batch consistency of the bar, and enhancing high-temperature strength, creep resistance and fatigue performance.
Smart Images

Figure CN123149346A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of titanium alloy pressure processing technology, specifically to a forging method for large-diameter bars of ultrafine-grained high-temperature titanium alloy. Background Technology
[0002] High-temperature titanium alloys are widely used in aerospace, energy, and chemical industries due to their excellent high-temperature strength, good creep resistance, and corrosion resistance. As engineering components develop towards larger sizes, lighter weights, and higher performance, higher requirements are being placed on the microstructure uniformity and grain refinement of large-size high-temperature titanium alloy bars.
[0003] Ti-Al-Sn-Zr-Mo-Si series high-temperature titanium alloys can be used at temperatures above 550~600℃ and are key materials for aero-engines. However, these alloys have a high degree of alloying, high high-temperature deformation pressure, and poor process plasticity. After casting, the grains are coarse. Conventional forging processes can usually only refine the grains to the micron level. Moreover, in large cross-sections, there is a large difference between the core and surface microstructure, which easily produces color mixing and coarse grains, retaining large original β grain boundaries, resulting in performance fluctuations and making it difficult to meet the batch consistency requirements of high-reliability components. Therefore, it is of great significance to develop a forging method that can achieve a uniform ultrafine grain structure in large-size titanium alloy bars. Summary of the Invention
[0004] The purpose of this invention is to provide a forging method for large-diameter ultrafine-grained high-temperature titanium alloy bars, employing the following technical solution: A forging method for large-diameter bars of ultrafine-grained high-temperature titanium alloy, wherein the high-temperature titanium alloy is a Ti-Al-Sn-Zr-Mo-Si system high-temperature titanium alloy, comprising the following steps: Step 1: Heat the alloy ingot to 1050~1150℃, hold for 10~60h and then forge it. The total forging ratio should not be less than 4. High-temperature deformation breaks up the coarse structure in the casting state and makes it homogenized. The holding time is matched with the cross-sectional size of the ingot to ensure the casting heat penetration and prevent forging cracks caused by the temperature difference between the core and the surface.
[0005] Step 2: Heat the billet obtained in Step 1 to 10~100℃ above the β phase transformation point, hold for 2~8h and then water quench to room temperature; after the microstructure is completely transformed into the β phase, it is rapidly cooled by water quenching, and the billet obtains high-density dislocations and other crystal defects, and the driving force for recrystallization refinement is sufficient, providing microstructure conditions for the large forging ratio deformation in Step 3.
[0006] Step 3: The billet obtained in Step 2 is subjected to three-stage upsetting and drawing deformation at 30~50℃ below the β phase transformation point, with a total forging ratio of not less than 8 and a final forging temperature of not less than 850℃; Step 4: Heat the billet obtained in Step 3 to 10~30℃ below the β phase transformation point, hold for 2h~6h, and then water quench to room temperature; Step 5: The billet obtained in Step 4 is subjected to three-stage upsetting and drawing deformation at 150~200℃ below the β phase transformation point, with a total forging ratio of not less than 8 and a final forging temperature of not less than 700℃, and is shaped to the target size. The water quenching in step two and step four, as well as the large-scale deformation of the two-phase region in steps three and five, work together to make the average grain size of the rod prepared by the method 300~400nm, and the original β grain boundaries in the macroscopic metallographic structure indistinguishable.
[0007] The preferred embodiment of the forging method for large-size ultrafine-grained high-temperature titanium alloy bars is as follows: in steps three and five, the holding time for each heating is t1 = η1 × δ1, where δ1 is the minimum cross-sectional size of the forging billet in millimeters, and η1 is the heating coefficient, which is 0.3~0.5 mm / min. Forging is then performed after the billet is removed from the furnace.
[0008] The preferred embodiment of the forging method for large-diameter ultrafine-grained high-temperature titanium alloy bars is that the diameter of the bars is 200~700mm.
[0009] The preferred embodiment of the forging method for large-size ultrafine-grained high-temperature titanium alloy bars is that the Ti-Al-Sn-Zr-Mo-Si series high-temperature titanium alloy is TC25G, Ti60, or Ti65.
[0010] Beneficial effects:
[0011] This invention achieves a uniform equiaxed ultrafine grain structure with an average grain size of 300–400 nm in large-size high-temperature titanium alloy bars of the Ti-Al-Sn-Zr-Mo-Si system through a combination of water quenching above the β-phase transformation point, low-temperature water quenching in the two-phase region, and two large-ratio forging deformations in the two-phase region. The original β-grain boundaries are indistinguishable on the macroscopic metallographic surface, overcoming the limitation of conventional forging processes in obtaining a uniform ultrafine grain structure. This invention is applicable to the preparation of large-size high-temperature titanium alloy bars with diameters of Φ200 mm–700 mm. The microstructure of the core and surface of the bar is uniform and consistent, eliminating mixed grains, coarse grains, and performance fluctuations, improving the uniformity of the bar microstructure and batch consistency. The bars prepared by this invention exhibit excellent comprehensive mechanical properties, with improved high-temperature strength, creep resistance, and fatigue performance. Attached Figure Description
[0012] Figure 1 This is a metallographic diagram of the billet after water quenching in Embodiment 1 of the present invention; Figure 2 This is a transmission microstructure diagram of the core of the final bar stock in Embodiment 1 of the present invention. Detailed Implementation
[0013] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the appendices in the embodiments of the present invention will be described below. Figures 1-2 The following describes in detail the specific embodiments of the present invention. Those skilled in the art can make appropriate adjustments without departing from the spirit of the invention. The following embodiments illustrate the present invention in more detail, but do not limit the present invention in any way.
[0014] Example 1
[0015] The high-temperature titanium alloy Ti65, with a composition of Ti-5.9Al-4.0Sn-3.5Zr-0.3Mo-0.4Si-0.3Nb-2.0Ta-1.0W-0.05C, was prepared by three melting processes in a vacuum arc remelting furnace, with a diameter of Φ440mm. The measured β-phase transformation point was 1045℃.
[0016] A forging method for large-diameter ultrafine-grained high-temperature titanium alloy bars includes the following steps: Step 1: Heat the alloy ingot to 1150℃ and hold it for 30 hours to ensure uniform temperature inside and outside the ingot. Then, remove it from the furnace and perform upsetting and drawing combined forging on a high-speed forging machine. The ingot is repeatedly turned over along the direction and deformed in three heats. After each heat, it is reheated to 1100℃ and the holding time is determined according to the minimum cross-sectional size of the billet. The total forging ratio is 4.5. Step 2: Heat the billet obtained in Step 1 to 1095℃, which is 50℃ above the β phase transformation point, hold for 4 hours, and transfer it to a water tank within 30 seconds after taking it out of the furnace. The whole billet is then water quenched to room temperature to obtain a billet that has undergone β phase region solution quenching treatment. Step 3: Load the billet obtained in Step 2 into an electric resistance furnace and heat it to 1015℃, which is 30℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1, where δ1 is the minimum cross-sectional dimension of the billet in this heat, in millimeters. After exiting the furnace, it is subjected to upsetting and drawing combined forging on a high-speed forging machine. Each heat is returned to the furnace and heated to 1015℃, and the holding time is re-determined according to the current minimum cross-sectional dimension of the billet. The billet undergoes three heats of deformation. The single-heat forging ratio of each heat is 2.0~2.3, the total forging ratio is 8.5, and the final forging temperature of each heat is not lower than 900℃, resulting in a fine-grained billet.
[0017] Step 4: Load the fine-grained billet obtained in Step 3 into a resistance furnace and heat it to 1025℃, which is 20℃ below the β phase transformation point. Hold it at this temperature for 4 hours. After taking it out of the furnace, transfer it to a water tank within 30 seconds and quench it in water to room temperature to obtain a billet that has undergone two-phase region heat preservation and quenching treatment.
[0018] Step 5: Load the billet obtained in Step 4 into an electric resistance furnace and heat it to 865℃, which is 180℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. After exiting the furnace, it is subjected to upsetting and drawing combined forging on a high-speed forging mill. Each forging is reheated to 865℃ and the holding time is re-determined according to the minimum cross-sectional size of the current billet. The billet undergoes three forging cycles in total. The single-forging ratio of each cycle is 2.0~2.2, and the total forging ratio is 8.2. The final forging temperature of each cycle is not lower than 800℃. After heating and holding at 750℃, the billet is shaped to Φ300mm to obtain a large-size bar.
[0019] Results: The obtained Φ300mm Ti65 large-size bar exhibited a uniform macroscopic metallographic structure from the core to the surface along the cross-section of the bar, with no traces of the original β grain boundaries observed. Samples were taken from the core, half radius, and surface, and measured by EBSD and TEM. The average grain sizes were 340nm, 330nm, and 345nm, respectively, all within the range of 300~400nm, indicating a uniform equiaxed ultrafine grain structure.
[0020] Example 2
[0021] The TC25G alloy with a composition of Ti-6.5Al-2Zr-2Sn-2Mo-1W-0.2Si was prepared by three melting processes in a vacuum arc remelting furnace, with a diameter of Φ360mm. The measured β phase transformation point was 980℃.
[0022] A forging method for large-diameter ultrafine-grained high-temperature titanium alloy bars includes the following steps: Step 1: Heat the ingot to 1120℃ and hold for 20 hours. After taking it out of the furnace, perform three-stage upsetting and drawing combined forging with a total forging ratio of 4.2 to obtain the forging billet.
[0023] Step 2: Heat the forging billet to 1040℃, which is 60℃ above the β phase transformation point, hold it at that temperature for 3 hours, and then remove it from the furnace and water quench it to room temperature.
[0024] Step 3: Heat the billet to 945℃, which is 35℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging. Each stage is reheated to 945℃ and the holding time is re-determined. The total forging ratio is 8.8. The final forging temperature of each stage is not lower than 850℃ to obtain a fine-grained billet.
[0025] Step 4: Heat the fine-grained billet to 955℃, which is 25℃ below the β phase transformation point, hold it at that temperature for 3 hours, and then remove it from the furnace and water quench it to room temperature.
[0026] Step 5: Heat the billet to 810℃, which is 170℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging. Each stage is reheated to 810℃ and the holding time is re-determined. The total forging ratio is 8.5. The final forging temperature of each stage is not lower than 720℃. Then, shape it to Φ220mm to obtain a large-size bar.
[0027] Results: The obtained Φ220mm TC25G large-size bar has a uniform macroscopic metallographic structure with indistinguishable original β grain boundaries; the average grain size of the core and the surface layer are 325nm and 335nm, respectively, both within the range of 300~400nm.
[0028] Example 3
[0029] Ti60 alloy with the composition Ti-5.8AL-4Sn-3.5Zr-0.4Mo-0.4Nb-1.0Ta-0.4Si-0.06C was prepared by three melting processes in a vacuum arc remelting furnace, with a diameter of Φ500mm. The measured β phase transformation point was 1040℃.
[0030] Step 1: Heat the ingot to 1150℃ and hold for 35 hours. After taking it out of the furnace, perform three-stage upsetting and drawing combined forging with a total forging ratio of 4.4 to obtain the forging billet.
[0031] Step 2: Heat the forging billet to 1100℃, which is 60℃ above the β phase transformation point, hold it at that temperature for 4 hours, and then remove it from the furnace and water quench it to room temperature.
[0032] Step 3: Heat the billet to 1000℃, which is 40℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging with a total forging ratio of 8.6. The final forging temperature of each stage is not lower than 900℃ to obtain a fine-grained billet.
[0033] Step 4: Heat the fine-grained billet to 1020℃, which is 20℃ below the β phase transformation point, hold it at this temperature for 4 hours, and then remove it from the furnace and water quench it to room temperature.
[0034] Step 5: Heat the billet to 860℃, which is 180℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging with a total forging ratio of 8.3. The final forging temperature of each stage is not lower than 750℃. Then shape it to Φ650mm to obtain a large-size bar.
[0035] Results: The obtained Φ650mm Ti60 large-size bar has a uniform macroscopic metallographic structure with indistinguishable original β grain boundaries; the average grain size of the core and the surface layer are 350nm and 340nm, respectively, both within the range of 300~400nm.
[0036] Comparative Example 1 The same Ti65 alloy ingots of the same batch and specifications as in Example 1 were used, with a diameter of Φ440mm and a measured β-phase transformation point of 1045℃. The specific steps are as follows: Step 1: Heat the ingot to 1150℃ and hold for 30 hours. After taking it out of the furnace, perform three-stage upsetting and drawing combined forging with a total forging ratio of 4.5 to obtain the forging billet. Step 2: Heat the forging billet to 1095℃, which is 50℃ above the β phase transformation point, hold it at that temperature for 4 hours, and then water quench it to room temperature after taking it out of the furnace. Step 3: Heat the billet to 1015℃, which is 30℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging with a total forging ratio of 8.5. The final forging temperature of each stage is not lower than 900℃ to obtain a fine-grained billet. Step 4: The fine-grained billet obtained in Step 3 is directly placed into an electric resistance furnace and heated to 865℃ without water quenching, which is 180℃ below the β phase transformation point. After holding for a period of t1=0.4δ1, it is taken out of the furnace and subjected to the three-stage upsetting and drawing combined forging process in Step 5. The total forging ratio is 8.2, and the final forging temperature of each stage is not lower than 800℃. Then it is shaped to Φ300mm to obtain a large-size bar.
[0037] Results: The obtained rods were measured by EBSD and TEM. The average grain sizes of the core, half radius and surface were 160 μm, 150 μm and 140 μm, respectively. They were micron-scale structures and no ultrafine grain structure of 300~400 nm was obtained. Local mixed crystals were also visible in the core.
[0038] Comparative Example 2 The same Ti65 alloy ingots of the same batch and specifications as in Example 1 were used, with a diameter of Φ440mm and a measured β-phase transformation point of 1045℃. The specific steps are as follows: Step 1: Heat the ingot to 1150℃ and hold for 30 hours. After taking it out of the furnace, perform three-stage upsetting and drawing combined forging with a total forging ratio of 4.5 to obtain the forging billet. Step 2: Heat the forging billet to 1095℃, which is 50℃ above the β phase transformation point, hold it at that temperature for 4 hours, and then water quench it to room temperature after taking it out of the furnace. Step 3: Heat the billet to 1015℃, which is 30℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging with a total forging ratio of 8.5. The final forging temperature of each stage is not lower than 900℃ to obtain a fine-grained billet. Step 4: Heat the fine-grained billet to 1025℃, which is 20℃ below the β phase transformation point, hold it at that temperature for 4 hours, and then water quench the entire billet to room temperature after it is taken out of the furnace. Step 5: Heat the billet to 1010℃, which is 35℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging with a total forging ratio of 8.2. The final forging temperature of each stage is not lower than 900℃. Then shape it to Φ300mm to obtain a large-size bar.
[0039] Results: The obtained rods were measured by EBSD and TEM. The average grain sizes of the core, half radius and surface were 130 μm, 120 μm and 120 μm, respectively, which are micron-scale structures. No ultrafine grain structure of 300~400 nm was obtained.
[0040] Comparative Example 3 The same Ti65 alloy ingots of the same batch and specifications as in Example 1 were used, with a diameter of Φ440mm and a measured β-phase transformation point of 1045℃. The specific steps are as follows: Step 1: Heat the ingot to 1150℃ and hold for 30 hours. After taking it out of the furnace, perform three-stage upsetting and drawing combined forging with a total forging ratio of 4.5 to obtain the forging billet. Step 2: The forged billet obtained in Step 1 is directly placed into a resistance furnace and heated to 1015℃, which is 30℃ below the β phase transformation point, without undergoing solution quenching in the β phase region. After holding for a period of t1=0.4δ1, it is taken out of the furnace and subjected to the three-stage upsetting and drawing combined forging process in Step 3. The total forging ratio is 8.5, and the final forging temperature of each stage is not lower than 900℃, resulting in a fine-grained billet. Step 3: Heat the fine-grained billet to 1025℃, which is 20℃ below the β phase transformation point, hold it at that temperature for 4 hours, and then water quench the entire billet to room temperature after it is taken out of the furnace. Step 4: Heat the billet to 865℃, which is 180℃ below the β phase transformation point. The holding time is determined according to t1=0.4δ1. Perform three-stage upsetting and drawing combined forging with a total forging ratio of 8.2. The final forging temperature of each stage is not lower than 800℃. Then shape it to Φ300mm to obtain a large-size bar.
[0041] Results: The macroscopic metallographic structure of the obtained rod showed residual coarse original β grain boundary traces, and the structure of the core and the surface was not uniform. According to EBSD and TEM measurements, the average grain size of the core was 320 μm, the average grain size at 1 / 2 radius was 190 μm, and the average grain size of the surface was 120 μm. The difference in grain size between the core and the surface was obvious, and a uniform 300~400 nm ultrafine grain structure was not obtained.
[0042] The results of Examples 1-3 show that, using the process of the present invention, large-diameter bars with a diameter of Φ200 mm or more can be prepared from Ti-Al-Sn-Zr-Mo-Si series high-temperature titanium alloys Ti65, TC25G, and Ti60. The macroscopic microstructure is uniform, the original β grain boundaries are indistinguishable, and the average grain size is 300-400 nm. The results of Comparative Examples 1-3 show that omitting the water quenching steps in steps two and four, or changing the deformation temperature in step five from 150-200℃ below the β phase transformation point to a conventional two-phase region temperature, cannot obtain the aforementioned uniform ultrafine grain structure.
[0043] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Those skilled in the art can make various modifications and improvements without departing from the spirit and scope of the present invention.
Claims
1. A forging method for large-diameter bars of ultrafine-grained high-temperature titanium alloy, wherein the high-temperature titanium alloy is a Ti-Al-Sn-Zr-Mo-Si series high-temperature titanium alloy, characterized in that: Includes the following steps: Step 1: Heat the alloy ingot to 1050~1150℃, hold it for 10~60h, and then forge it. The total forging ratio should not be less than 4. Step 2: Heat the billet obtained in Step 1 to 10~100℃ above the β phase transformation point, hold for 2~8 hours, and then water quench to room temperature; Step 3: The billet obtained in Step 2 is subjected to three-stage upsetting and drawing deformation at 30~50℃ below the β phase transformation point, with a total forging ratio of not less than 8 and a final forging temperature of not less than 850℃; Step 4: Heat the billet obtained in Step 3 to 10~30℃ below the β phase transformation point, hold for 2h~6h, and then water quench to room temperature; Step 5: The billet obtained in Step 4 is subjected to three-stage upsetting and drawing deformation at 150~200℃ below the β phase transformation point, with a total forging ratio of not less than 8 and a final forging temperature of not less than 700℃, and is shaped to the target size. The water quenching in step two and step four, as well as the large-scale deformation of the two-phase region in steps three and five, work together to make the average grain size of the rod prepared by the method 300~400nm, and the original β grain boundaries in the macroscopic metallographic structure indistinguishable.
2. The forging method for large-diameter ultrafine-grained high-temperature titanium alloy bars according to claim 1, characterized in that: In steps three and five, the holding time for each heating is t1 = η1 × δ1, where δ1 is the minimum cross-sectional dimension of the forging billet in millimeters, and η1 is the heating coefficient, which is 0.3~0.5 mm / min.
3. The forging method for large-diameter ultrafine-grained high-temperature titanium alloy bars according to claim 1, characterized in that: The diameter of the rod is 200~700mm.
4. The forging method for large-diameter ultrafine-grained high-temperature titanium alloy bars according to claim 1, characterized in that: The Ti-Al-Sn-Zr-Mo-Si series high-temperature titanium alloy is TC25G, Ti60, or Ti65.