A forging processing method of a TiB directional reinforced high-temperature titanium alloy blade forging
By employing a multi-stage collaborative forging method, the problem of random distribution and difficulty in maintaining directional microstructure in TiB particle-reinforced titanium matrix composites during forging was solved. This method achieved axially oriented distribution of TiB particles, improving the high-temperature performance and dimensional accuracy of blade forgings, and is suitable for the preparation of high-temperature structural components for aero-engines.
Patent Information
- Application Number
- CN202611612306.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-24
AI Technical Summary
Existing TiB particle-reinforced titanium matrix composites suffer from performance degradation during forging due to random TiB particle distribution, difficulty in maintaining oriented microstructure, and uneven temperature distribution in large-size billets. This makes it difficult to meet the requirements for high-temperature structural components in next-generation aero-engines.
A multi-stage synergistic control forging method is adopted, including billet forging, directional upsetting and drawing above the Tβ phase transformation point, precision forging of bars and die forging, to ensure that TiB particles are oriented along the axial direction and inherited into the blade forging. By controlling the consistency of heating temperature and deformation direction, the precipitation of primary α phase and grain boundary migration interference are avoided.
It achieves the directional distribution of TiB particles along the bearing direction of the blade, significantly improving the high-temperature performance and dimensional accuracy of the blade forging. It is suitable for the preparation of various specifications of bars and blade forgings, meeting the requirements of long service life and high reliability of high-temperature structural components for aero-engines.
Smart Images

Figure CN123149347A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal material forging technology, specifically to a forging process for large-diameter bars of titanium-based composite material with TiB directional arrangement. Background Technology
[0002] High-temperature titanium alloys are widely used in high-temperature structural components such as compressor blades and discs in aero-engines due to their excellent high-temperature strength, good oxidation resistance, and low density. However, with the continuous increase in the thrust-to-weight ratio of aero-engines, the operating temperature and stress of blades continue to rise. Traditional homogeneous titanium alloys still suffer from insufficient creep resistance and decreased fatigue performance under extreme high-temperature environments, making it difficult to meet the long service life and high reliability requirements of next-generation aero-engines.
[0003] TiB particle-reinforced titanium matrix composites possess higher high-temperature strength, creep resistance, and elastic modulus. The TiB reinforcing phase exhibits good interfacial bonding with the titanium matrix and matches its coefficient of thermal expansion, making it an important pathway to improve the performance of high-temperature titanium alloy components. However, existing TiB particle-reinforced titanium matrix composites face the following prominent problems during forging: (1) TiB particles are randomly distributed and oriented. During conventional forging (especially upsetting, free drawing, and die forging), TiB particles are redistributed with the flow of metal and are randomly oriented. They cannot form an effective reinforcing effect in the load-bearing direction of the component, which means that the high-temperature performance potential of the material cannot be fully realized.
[0004] (2) The oriented structure is difficult to maintain in multiple passes and multiple heat treatments. Existing technologies usually only achieve the initial orientation of TiB particles in a certain deformation stage (such as billet making or bar making). However, in subsequent deformation processes, if the deformation temperature is not properly controlled, such as deformation below the Tβ phase transformation point, the precipitation of the primary α phase and grain boundary migration will disrupt the oriented arrangement of TiB particles, causing the oriented structure to become disordered or even disappear, and it cannot be inherited to the final forging.
[0005] (3) Uneven temperature distribution across large billet cross sections leads to TiB orientation deflection. For large bar and blade forgings, the billet cross section is large. If the heating regime is not reasonable, there is a large temperature difference between the core and the surface of the billet. During deformation, the metal flow is uneven, which causes the TiB particles to deflect in orientation, resulting in a decrease in orientation and an increase in performance dispersion. Summary of the Invention
[0006] The purpose of this invention is to provide a forging method for TiB-oriented reinforced high-temperature titanium alloy blade forgings, using the following technical solution: A forging method for TiB-oriented reinforced high-temperature titanium alloy blade forgings includes the following steps: Step 1: Forging the billet; The TiB-reinforced high-temperature titanium alloy ingot is heated to 1050℃~1150℃ and held for 8h~16h before being forged into a billet. The forging ratio of the billet forging is not less than 4, and the billet is obtained. Step 2: Directional upsetting; The billet is heated to 20°C to 50°C above the Tβ phase transformation point of the alloy, and then upset and reverse drawing deformation is performed to form a forging billet. The forging ratio of the directional upset drawing is not less than 4, so that the TiB particles are oriented along the axial direction of the billet. Step 3: Precision forging of the bar; The forging billet is heated to 10°C to 30°C above the Tβ phase transformation point of the alloy, and formed in 2 to 4 heats on a precision forging machine to produce a bar. The TiB particles in the bar are kept parallel to the axial direction of the bar. Step 4: Die forging; The bar is heated to 10°C to 30°C above the Tβ phase transformation point of the alloy, and pre-forged and final-forged on a die forging machine to obtain a TiB-oriented reinforced high-temperature titanium alloy blade forging. The TiB particles in the blade forging are oriented along the blade bearing direction. In particular, the deformation temperatures in steps two, three, and four are all above the Tβ phase transformation point of the alloy, so that the axially oriented distribution of the TiB particles formed in step two can be maintained and inherited into the blade forging during the deformation process in steps three and four.
[0007] The preferred embodiment of the forging method for TiB-oriented reinforced high-temperature titanium alloy blade forging is as follows: in step three, the specification of the bar is Φ30mm~Φ150mm; the distribution of TiB particles in the bar is parallel to the axial direction of the bar.
[0008] The preferred embodiment of the forging method for TiB directional reinforced high-temperature titanium alloy blade forging is as follows: in steps two, three, and four, before each forging pass, the billet is heated and held at a heating coefficient η = 0.2 min / mm to 0.5 min / mm. After reaching the holding time, the billet is removed from the furnace and covered with asbestos. Then, it is returned to the furnace and reheated to the set temperature and held for 10 min to 15 min before the forging process is performed again.
[0009] The preferred embodiment of the forging method for TiB-oriented reinforced high-temperature titanium alloy blade forging is that, in step two, the upsetting direction of each heat treatment is consistent with the elongation direction of the previous heat treatment, so that the deformation of each heat treatment forms an elongation flow along the axial direction of the billet, thereby strengthening the axial orientation of TiB particles.
[0010] The preferred embodiment of the forging process of the TiB-oriented reinforced high-temperature titanium alloy blade forging is that, in step four, the final forging temperature during die forging is not lower than the Tβ phase transformation point of the alloy, so as to avoid deformation below the Tβ phase transformation point that would lead to disordered directional distribution of TiB particles.
[0011] The preferred embodiment of the forging method for a TiB-oriented reinforced high-temperature titanium alloy blade forging is that, in step four, the axial direction of the bar is consistent with the bearing direction of the blade forging, so that the directional distribution direction of the TiB particles is parallel to the bearing direction of the blade forging.
[0012] The principle of this invention is as follows: When deformed above the Tβ phase transformation point, the alloy is in a single-phase β region, and TiB particles rearrange themselves oriented along with the flow of the β matrix metal. Since there is no precipitation of the primary α phase or grain boundary obstruction, once the TiB particles are oriented along the deformation direction, as long as subsequent deformation is controlled above the Tβ phase transformation point and the flow direction remains consistent, this oriented structure can be inherited stepwise without disorder. Accordingly, this invention establishes and maintains the axial oriented distribution of TiB particles through multi-stage synergistic control—ingot casting—β-region oriented upsetting—β-region precision forging—β-region die forging, ultimately aligning it with the blade's load-bearing direction.
[0013] Beneficial effects:
[0014] 1. This invention employs multi-stage synergistic control, including ingot casting, directional upsetting above the Tβ phase transformation point, precision forging, and die forging (pre-forging and final forging), to ensure the axial distribution of TiB particles along the bar stock. This directional microstructure is inherited in the blade forging, thus fully leveraging the reinforcing effect of the TiB phase in the blade's load-bearing direction. The room temperature tensile strength, high-temperature creep life, and creep resistance of the blade forging along the load-bearing direction are significantly superior to those of conventional forgings with randomly oriented TiB.
[0015] 2. In this invention, upsetting and reversing elongation deformation are performed at 20℃~50℃ above the Tβ phase transformation point, with a forging ratio of not less than 4. In this temperature range, the β phase is completely softened, and TiB particles are easily oriented axially with the metal flow. The high forging ratio ensures sufficient deformation accumulation and improves the directionality and uniformity of the reinforcing phase distribution.
[0016] 3. During the forging process, the heating coefficient η = 0.2 min / mm ~ 0.5 min / mm. After reaching the holding time, the billet is taken out of the furnace and covered with asbestos. It is then returned to the furnace and reheated to the set temperature and held for 10 min ~ 15 min before forging. This effectively reduces the temperature difference of the billet cross section, avoids uneven local deformation that could lead to TiB orientation deflection, and ensures stable batch performance.
[0017] 4. This invention can guarantee the forming quality and dimensional accuracy of complex blade profiles while preserving the TiB oriented structure. It is suitable for the preparation of bar stock of various specifications from Φ30mm to Φ150mm and blade forgings of different sizes, and is especially suitable for the engineering preparation of high-temperature titanium-based composite material structural parts. Attached Figure Description
[0018] Figure 1 This is a schematic diagram of the three-dimensional microstructure of the blade forging; Figure 2 This is a schematic diagram of the TiB directional enhancement process. Detailed Implementation
[0019] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the appendices in the embodiments of the present invention will be described below. Figures 1-2 The specific embodiments of the present invention will be described in detail below. Those skilled in the art can make appropriate adjustments without departing from the spirit of the invention. The following embodiments illustrate the present invention in more detail, but do not limit the invention in any way. In the following examples, all raw materials used were TiB-reinforced high-temperature titanium alloy ingots, wherein the TiB reinforcing phase content was 0.5wt%~2.0wt%, and the balance was Ti and alloying elements such as Al, Sn, Zr, Mo, Nb, Si, etc. The ingots were prepared by consumable melting. The Tβ phase transformation point of each alloy was determined by metallographic method or differential scanning calorimetry.
[0020] Example 1
[0021] The measured Tβ phase transformation point of the TiB-reinforced high-temperature titanium alloy ingot was 1015℃. A forging method for TiB-oriented reinforced high-temperature titanium alloy blade forgings includes the following steps: Step 1: Forging the billet; The TiB-reinforced high-temperature titanium alloy ingot was heated to 1100℃, held at a heating coefficient η=0.3min / mm for 12h, then removed from the furnace and covered with asbestos. It was then returned to the furnace, reheated to 1100℃ and held for 12min, and then forged into a billet. The forging ratio of the billet forging was 4.5 to obtain the billet. Step 2: Directional upsetting; The billet is heated to 40°C above the Tβ phase transformation point, i.e., 1055°C. After holding at this temperature with a heating coefficient η=0.3min / mm, it is removed from the furnace, covered with asbestos, and then returned to the furnace to be reheated to 1055°C and held for 12 minutes. Upsetting and reversing drawing deformation are then performed. The upsetting direction of each heat is consistent with the drawing direction of the previous heat. The forging ratio of the directional upsetting and drawing is 4.2, forming a forged billet. The TiB particles are oriented along the axial direction of the billet. Step 3: Precision forging of the bar; The forging billet is heated to 20°C above the Tβ phase transformation point, i.e., 1035°C, and formed in three passes on a precision forging machine to produce a Φ80mm bar. The TiB particles in the bar are kept parallel to the axial direction of the bar. Step 4: Die forging; The bar is heated to 20°C above the Tβ phase transformation point, i.e., 1035°C, and pre-forged and final-forged on a die forging machine. The final forging temperature during die forging is not lower than the Tβ phase transformation point of 1015°C. The axial direction of the bar is consistent with the bearing direction of the blade forging, thus obtaining a TiB oriented reinforced high-temperature titanium alloy blade forging.
[0022] The TiB in the obtained blade forgings is oriented axially, i.e., in the direction of blade bearing, and the microstructure is uniform. Sampling and testing along the bearing direction showed that the tensile strength at 600℃ was 720MPa, and the creep rupture life at 600℃ / 350MPa was greater than 100h, which is about 15% and more than 1 times higher than that of conventionally forged blades with random orientation, respectively.
[0023] Example 2
[0024] The same TiB-reinforced high-temperature titanium alloy ingot with the same composition as in Example 1 was used, with a Tβ phase transformation point of 1010℃.
[0025] A forging method for TiB-oriented reinforced high-temperature titanium alloy blade forgings includes the following steps: Step 1: Forging the billet; The ingot is heated to 1050℃, held at the temperature for 10 hours with a heating coefficient η=0.2min / mm, then removed from the furnace, covered with asbestos, returned to the furnace, reheated to 1050℃ and held for 10 minutes, and then forged into a billet with a forging ratio of 4.0. Step 2: Directional upsetting; The billet is heated to 30°C above the Tβ phase transformation point, i.e., 1040°C, and then upset and reverse elongation deformation is performed. The upsetting direction of each heat is consistent with the elongation direction of the previous heat. The forging ratio is 4.0, forming a forged billet. Step 3: Precision forging of the bar; The forging billet is heated to 10°C above the Tβ phase transformation point, i.e., 1020°C, and then formed in two passes on a precision forging machine to produce a Φ30mm bar. Step 4: Die forging; The bar stock is heated to 10°C above the Tβ phase transformation point, i.e., 1020°C, and then pre-forged and final-forged on a die forging machine. The final forging temperature is not lower than the Tβ phase transformation point to obtain the blade forging.
[0026] The resulting blade forgings exhibited good TiB directional reinforcement, with a creep rupture life of over 100 hours at 600℃ along the load-bearing direction, verifying the applicability of this method to small-diameter bars.
[0027] Comparative Example 1 Using an ingot with the same composition as in Example 1, after completing the initial forging according to step one of Example 1, the billet was heated to 20°C below the Tβ phase transformation point, i.e., 995°C, for upsetting and reversible drawing. The remaining steps were the same as in Example 1. The resulting blade forging exhibited random TiB particle orientation, a tensile strength of 630 MPa at 600°C, and a creep rupture life of less than 50 hours at 600°C / 350 MPa, significantly lower than that of Example 1.
[0028] Comparative Example 2 Using the same process as in Example 1, except that the final forging temperature in step four was controlled to 10°C below the Tβ phase transformation point, i.e., 1005°C. In the resulting blade forging, although TiB was already oriented in the bar stage, the precipitation of the primary α phase during the final forging process disrupted the oriented distribution of TiB. The TiB orientation in the bearing direction of the blade decreased by about 40%, and the 600°C creep life was reduced by about 50% compared to Example 1.
[0029] As can be seen from the above embodiments and comparative examples: (1) In Examples 1-2, the deformation temperatures of steps 2, 3 and 4 are all above the Tβ phase transformation point. With the control that the upsetting direction and the drawing direction are consistent in each fire, the axial orientation distribution of TiB particles is established and inherited to the bearing direction of the blade forging step by step, and the high temperature performance is significantly improved. (2) Comparative Example 1 shows that if the reversal deformation is carried out below the Tβ phase transition point, the TiB directional structure cannot be established and the blade performance drops significantly, proving that the deformation above the Tβ phase transition point throughout the process is the fundamental guarantee of the effectiveness of the present invention. (3) Comparative Example 2 shows that if the final forging temperature is lower than the Tβ phase transformation point, the established directional structure will be disordered, proving the necessity of the present invention to limit the final forging temperature to not be lower than the Tβ phase transformation point.
[0030] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Those skilled in the art can make various modifications and improvements without departing from the spirit and scope of the present invention.
Claims
1. A forging method for TiB-oriented reinforced high-temperature titanium alloy blade forgings, characterized in that, Includes the following steps: Step 1: Forging the billet; The TiB-reinforced high-temperature titanium alloy ingot is heated to 1050℃~1150℃ and held for 8h~16h before being forged into a billet. The forging ratio of the billet forging is not less than 4, and the billet is obtained. Step 2: Directional upsetting; The billet is heated to 20°C to 50°C above the Tβ phase transformation point of the alloy, and then upset and reverse drawing deformation is performed to form a forging billet. The forging ratio of the directional upset drawing is not less than 4, so that the TiB particles are oriented along the axial direction of the billet. Step 3: Precision forging of the bar; The forging billet is heated to 10°C to 30°C above the Tβ phase transformation point of the alloy, and formed in 2 to 4 heats on a precision forging machine to produce a bar. The TiB particles in the bar are kept parallel to the axial direction of the bar. Step 4: Die forging; The bar is heated to 10°C to 30°C above the Tβ phase transformation point of the alloy, and pre-forged and final-forged on a die forging machine to obtain a TiB-oriented reinforced high-temperature titanium alloy blade forging. The TiB particles in the blade forging are oriented along the blade bearing direction. In particular, the deformation temperatures in steps two, three, and four are all above the Tβ phase transformation point of the alloy, so that the axially oriented distribution of the TiB particles formed in step two can be maintained and inherited into the blade forging during the deformation process in steps three and four.
2. The forging method for a TiB-oriented reinforced high-temperature titanium alloy blade forging as described in claim 1, characterized in that: In step three, the specifications of the rod are Φ30mm~Φ150mm; the TiB particles in the rod are distributed parallel to the axial direction of the rod.
3. The forging method for a TiB-oriented reinforced high-temperature titanium alloy blade forging as described in claim 1, characterized in that: In steps two, three, and four, the billet is heated and kept warm at a heating coefficient η = 0.2 min / mm to 0.5 min / mm before each deformation. After the holding time is reached, the billet is taken out of the furnace and covered with asbestos. Then it is returned to the furnace and reheated to the set temperature and held for 10 min to 15 min before the forging process of that heat is carried out again.
4. The forging method for a TiB-oriented reinforced high-temperature titanium alloy blade forging as described in claim 1, characterized in that: In step two, the upsetting direction of each heat treatment is consistent with the elongation direction of the previous heat treatment, so that the deformation of each heat treatment forms an elongation flow along the axial direction of the billet, thereby strengthening the directional arrangement of TiB particles along the axial direction.
5. The forging method for a TiB-oriented reinforced high-temperature titanium alloy blade forging as described in claim 1, characterized in that: In step four, the final forging temperature during die forging is not lower than the Tβ phase transformation point of the alloy, so as to avoid deformation below the Tβ phase transformation point that would cause disordered directional distribution of TiB particles.
6. The forging method for a TiB-oriented reinforced high-temperature titanium alloy blade forging as described in claim 1, characterized in that: In step four, the axial direction of the bar is aligned with the bearing direction of the blade forging, so that the directional distribution direction of the TiB particles is parallel to the bearing direction of the blade forging.