A cold heading process for thin-walled parts with through holes

By heat treatment of raw materials, multi-station progressive cold heading and cyclic annealing, a grid structure of alternating ferrite and pearlite is formed, which solves the problem of insufficient mechanical strength of thin-walled deep-hole parts and improves the toughness and mechanical properties of the material.

CN123149351APending Publication Date: 2026-11-24ZHEJIANG DONGRUI MACHINERY IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611204035.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing cold heading methods for thin-walled deep-hole parts, as the number of extrusions increases, the metal flow space becomes limited, leading to uneven material flow and defects such as uneven wall thickness and hole wall cracks, resulting in poor mechanical properties.

Method used

The raw materials are heat-treated to form a nano-bainitic structure. Combined with multi-station progressive cold heading and cyclic annealing, a grid structure of alternating ferrite and pearlite is formed. The structure is further strengthened by quenching. The process steps are optimized to improve the mechanical strength of the material.

Benefits of technology

It effectively solves the problem of insufficient mechanical strength of thin-walled parts with through holes, improves material toughness, avoids cracking, and ensures reduced friction and improved mechanical properties during the molding process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to a kind of thin-walled parts with hole cold heading process, belong to part processing technical field.The thin-walled parts with hole cold heading process disclosed in the present application, specific steps are as follows: raw material heat treatment-coarse block-multi-station progressive cold heading forming-cyclic annealing-thin-walled parts with hole after quenching are obtained.By heat treatment, material forms nano bainite structure, improves the toughness of material, and under the action of multi-station cold heading forming, equiaxed grain is elongated along the direction of maximum principal deformation, forms the fiber structure of ferrite and pearlite alternately, and after cyclic annealing, regularized lamellar pearlite is formed, and with ferrite, it constitutes grid structure for the structural mechanical strength of material, finally after quenching, it is further strengthened, can effectively solve the problem of insufficient mechanical strength of thin-walled parts with hole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of parts processing technology and relates to a cold heading process for thin-walled parts with through holes. Background Technology

[0002] Thin-walled parts refer to components with a relatively small ratio between their wall thickness and length, diameter, or overall size. They are characterized by their lightweight structure and complex shape. They are used in applications such as aircraft engine casings, lightweight automotive parts, and precision instrument housings. Their structural design and manufacturing require high precision, and demand high mechanical stability during processing. Therefore, the forming of thin-walled tubular parts must consider both the deep hole and thin wall characteristics, which can lead to defects such as uneven wall thickness, irregular cross-sections, and even hole wall cracks.

[0003] Current methods for cold heading thin-walled deep-hole parts involve multiple extrusions to form the thin-walled deep holes. However, as the number of extrusions increases, the thin-walled cavity becomes increasingly narrow, the metal flow space becomes extremely limited, and the friction between the metal and the cavity wall increases significantly. This easily leads to uneven material flow, resulting in localized thin walls, low hole wall quality, and poor mechanical properties of the thin-walled parts. Therefore, this invention proposes a cold heading process for thin-walled parts with through holes, further optimizing the process steps based on existing technologies. Summary of the Invention

[0004] This invention relates to a cold heading process for thin-walled parts with through holes, belonging to the field of parts processing technology. The specific steps of the cold heading process for thin-walled parts with through holes disclosed in this invention are: raw material heat treatment—rough upsetting—multi-station progressive cold heading—cyclic annealing—quenching to obtain the thin-walled part with through holes. Heat treatment induces a nano-bainitic microstructure in the material, improving its toughness. Under the action of multi-station cold heading, equiaxed grains are elongated along the direction of maximum principal deformation, forming a fibrous structure of alternating ferrite and pearlite. Cyclic annealing forms regularized lamellar pearlite, which, together with ferrite, constitutes a mesh structure, contributing to the material's structural mechanical strength. Finally, quenching further strengthens the material, effectively solving the problem of insufficient mechanical strength in thin-walled parts with through holes.

[0005] The objective of this invention can be achieved through the following technical solutions: A cold heading process for a thin-walled part with a through hole, the cold heading process specifically including the following steps: (1) The raw materials are put into a heating furnace for heat treatment, and then air-cooled to room temperature to obtain pretreated materials; (2) The pretreated material is axially upset to obtain a cylindrical blank; (3) The blank is placed into the mold cavity of the cold heading machine, and the punch continuously extrudes and shapes the blank through 5 stations to obtain the initial product of thin-walled part with through hole; (4) The initial product of the thin-walled part with through hole is placed in a heating furnace for cyclic annealing, and then cooled to room temperature in a cold extraction liquid to obtain the thin-walled part with through hole.

[0006] Further, the specific steps of the heat treatment in step (1) are as follows: the raw material is heated to 1000-1100℃ and kept at that temperature for 30-50 minutes, then taken out and placed in a salt bath furnace at 220-260℃ for 2-3 hours, then heated to 600-700℃ and kept at that temperature for 3 hours, then air-cooled to room temperature, then heated to 850-880℃ in a heating furnace and kept at that temperature for 30 minutes, then taken out and placed in a salt bath furnace at 200-230℃ for 24 hours.

[0007] Furthermore, the elemental mass percentages of the raw materials are: C 0.6-0.7%, Si 0.3-0.6%, Mn 1.4-1.65%, P 0.01-0.025%, S 0.005-0.01%, Cr 0.04-0.068%, Cu 0.089-0.16%, with the remainder being Fe.

[0008] Furthermore, the blank in step (2) has a specification of Φ16mm×32mm.

[0009] Further, the five stations in step (3) are specifically divided into: station 1 is for denting, station 2 is for compound extrusion, and stations 3, 4 and 5 are for thin-wall elongation forming. The continuous extrusion speed is 70-78 mm / s, and the continuous extrusion temperature is 40-60℃.

[0010] Furthermore, the mold cavity in step (3) undergoes phosphating treatment. The specific steps are as follows: a layer of phosphating solution is brushed onto the cavity of the mold and dried at 75-80°C, and then a layer of sodium stearate saponification solution is brushed onto the cavity and dried at 80-90°C. The phosphating solution is composed of phosphoric acid, zinc oxide, nitric acid, copper carbonate, sodium nitrate and water in a ratio of 41:27.5:22.5:3:38:100.

[0011] Further, the specific steps of the cyclic annealing in step (4) are as follows: the initial product of the thin-walled part with through hole is heated to 700-710℃ and held for 2-3 minutes, then cooled to 680-690℃ and held for 8-10 minutes, and then heated to 700-710℃ and held for 2-3 minutes, wherein the heating and cooling rate is 1-1.5℃ / min.

[0012] Furthermore, the cooling rate in step (4) is 5-8℃ / s, and the wall thickness of the thin-walled part with through holes is 1-3mm.

[0013] The beneficial effects of this invention are: This invention uses a series of steps—raw material heat treatment, rough upsetting, multi-station progressive cold heading, cyclic annealing, and quenching—to obtain thin-walled parts with through holes. The heat treatment first refines the microstructure of the material by temperature control, forming nano-bainite, which greatly improves the toughness of the material and prevents cracking during the cold heading process. At the same time, the mold cavity is phosphated and lubricated to reduce the friction coefficient of the material in the mold cavity. This avoids the problem that lubrication treatment on the material surface would cause deformation during the cold heading process and damage the lubrication layer, thus increasing friction. By utilizing the multi-station cold heading process, nano-bainite is elongated along the direction of maximum principal deformation of equiaxed grains, forming a fibrous structure of alternating nano-bainitic ferrite laths and refined carbides. After cyclic annealing, regularized lamellar pearlite is formed, which, together with ferrite, constitutes a grid structure, contributing to the mechanical strength of the material. Finally, quenching further strengthens the material, effectively solving the problem of insufficient mechanical strength in thin-walled parts with through holes. Detailed Implementation

[0014] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with embodiments, is provided below.

[0015] The sodium stearate saponification solution involved in this invention has a mass fraction of 10%, a phosphoric acid mass fraction of 75%, and a nitric acid mass fraction of 68%. Example 1

[0016] A cold heading process for a thin-walled part with a through hole, the cold heading process specifically including the following steps: (1) The raw materials are put into a heating furnace for heat treatment, and then air-cooled to room temperature to obtain pretreated materials; (2) The pretreated material is axially upset to obtain a cylindrical blank; (3) The blank is placed into the mold cavity of the cold heading machine, and the punch continuously extrudes and shapes the blank through 5 stations to obtain the initial product of thin-walled part with through hole; (4) The initial product of the thin-walled part with through hole is placed in a heating furnace for cyclic annealing, and then cooled to room temperature in a cold extraction liquid to obtain the thin-walled part with through hole.

[0017] The specific steps of heat treatment in step (1) are as follows: the raw material is heated to 1000℃ and kept at that temperature for 30 minutes. It is then taken out and placed in a salt bath furnace at 220℃ for 2 hours. Then, the temperature is raised to 600℃ and kept at that temperature for 3 hours. It is then air-cooled to room temperature. Next, the temperature is raised to 850℃ in a heating furnace and kept at that temperature for 30 minutes. It is then taken out and placed in a salt bath furnace at 200℃ for 24 hours.

[0018] The elemental mass percentages of the raw materials are: C 0.6%, Si 0.3%, Mn 1.4%, P 0.01%, S 0.005-0.01%, Cr 0.04%, Cu 0.089%, with the remainder being Fe.

[0019] The blank in step (2) has a specification of Φ16mm×32mm.

[0020] The five stations in step (3) are specifically divided into: station 1 is for denting, station 2 is for compound extrusion, and stations 3, 4 and 5 are for thin-walled elongation forming. The continuous extrusion speed is 70 mm / s and the continuous extrusion temperature is 40°C.

[0021] The mold cavity in step (3) is subjected to phosphating treatment. The specific steps are as follows: a layer of phosphating solution is brushed onto the cavity of the mold and dried at 75°C, and then a layer of sodium stearate saponification solution is brushed onto the cavity and dried at 80°C. The phosphating solution is composed of phosphoric acid, zinc oxide, nitric acid, copper carbonate, sodium nitrate and water in a ratio of 41:27.5:22.5:3:38:100.

[0022] The specific steps of the cyclic annealing in step (4) are as follows: the initial product of the thin-walled part with through hole is heated to 700℃ and held for 2 minutes, then cooled to 680℃ and held for 8 minutes, and then heated to 700℃ and held for 2 minutes. The heating and cooling rates are 1℃ / min.

[0023] The cooling rate in step (4) is 5°C / s, and the wall thickness of the thin-walled part with through holes is 1mm. Example 2

[0024] A cold heading process for a thin-walled part with a through hole, the cold heading process specifically including the following steps: (1) The raw materials are put into a heating furnace for heat treatment, and then air-cooled to room temperature to obtain pretreated materials; (2) The pretreated material is axially upset to obtain a cylindrical blank; (3) The blank is placed into the mold cavity of the cold heading machine, and the punch continuously extrudes and shapes the blank through 5 stations to obtain the initial product of thin-walled part with through hole; (4) The initial product of the thin-walled part with through hole is placed in a heating furnace for cyclic annealing, and then cooled to room temperature in a cold extraction liquid to obtain the thin-walled part with through hole.

[0025] The specific steps of heat treatment in step (1) are as follows: the raw material is heated to 1050℃ and kept at that temperature for 40 minutes. It is then taken out and placed in a salt bath furnace at 240℃ for 2.5 hours. Then, the temperature is raised to 650℃ and kept at that temperature for 3 hours. It is then air-cooled to room temperature. Next, the temperature is raised to 865℃ in a heating furnace and kept at that temperature for 30 minutes. It is then taken out and placed in a salt bath furnace at 215℃ for 24 hours.

[0026] The elemental mass percentages of the raw materials are: C 0.65%, Si 0.45%, Mn 1.55%, P 0.018%, S 0.007%, Cr 0.05%, Cu 0.1%, with the remainder being Fe.

[0027] The blank in step (2) has a specification of Φ16mm×32mm.

[0028] The five stations in step (3) are specifically divided into: station 1 is for denting, station 2 is for compound extrusion, and stations 3, 4 and 5 are for thin-wall elongation forming. The continuous extrusion speed is 74 mm / s and the continuous extrusion temperature is 50°C.

[0029] The mold cavity in step (3) is subjected to phosphating treatment. The specific steps are as follows: a layer of phosphating solution is brushed onto the cavity of the mold and dried at 77°C, and then a layer of sodium stearate saponification solution is brushed onto the cavity and dried at 85°C. The phosphating solution is composed of phosphoric acid, zinc oxide, nitric acid, copper carbonate, sodium nitrate and water in a ratio of 41:27.5:22.5:3:38:100.

[0030] The specific steps of the cyclic annealing in step (4) are as follows: the initial product of the thin-walled part with through hole is heated to 705℃ and held for 2 minutes, then cooled to 685℃ and held for 9 minutes, and then heated to 705℃ and held for 2 minutes. The heating and cooling rates are 1.2℃ / min.

[0031] The cooling rate in step (4) is 6.5℃ / s, and the wall thickness of the thin-walled part with through holes is 2mm. Example 3

[0032] A cold heading process for a thin-walled part with a through hole, the cold heading process specifically including the following steps: (1) The raw materials are put into a heating furnace for heat treatment, and then air-cooled to room temperature to obtain pretreated materials; (2) The pretreated material is axially upset to obtain a cylindrical blank; (3) The blank is placed into the mold cavity of the cold heading machine, and the punch continuously extrudes and shapes the blank through 5 stations to obtain the initial product of thin-walled part with through hole; (4) The initial product of the thin-walled part with through hole is placed in a heating furnace for cyclic annealing, and then cooled to room temperature in a cold extraction liquid to obtain the thin-walled part with through hole.

[0033] The specific steps of heat treatment in step (1) are as follows: the raw material is heated to 1100℃ and kept at that temperature for 50 minutes. It is then taken out and placed in a salt bath furnace at 260℃ for 3 hours. Then, the temperature is raised to 700℃ and kept at that temperature for 3 hours. It is then air-cooled to room temperature. Next, the temperature is raised to -880℃ in a heating furnace and kept at that temperature for 30 minutes. It is then taken out and placed in a salt bath furnace at 230℃ for 24 hours.

[0034] The elemental mass percentages of the raw materials are: C 0.7%, Si 0.6%, Mn 1.65%, P 0.025%, S 0.01%, Cr 0.068%, Cu 0.16%, with the remainder being Fe.

[0035] The blank in step (2) has a specification of Φ16mm×32mm.

[0036] The five stations in step (3) are specifically divided into: station 1 is for denting, station 2 is for compound extrusion, and stations 3, 4 and 5 are for thin-wall elongation forming. The continuous extrusion speed is 78 mm / s and the continuous extrusion temperature is 60°C.

[0037] The mold cavity in step (3) is subjected to phosphating treatment. The specific steps are as follows: a layer of phosphating solution is brushed onto the cavity of the mold and dried at 80°C, and then a layer of sodium stearate saponification solution is brushed onto the cavity and dried at 90°C. The phosphating solution is composed of phosphoric acid, zinc oxide, nitric acid, copper carbonate, sodium nitrate and water in a ratio of 41:27.5:22.5:3:38:100.

[0038] The specific steps of the cyclic annealing in step (4) are as follows: the initial product of the thin-walled part with through hole is heated to 710℃ and held for 3 minutes, then cooled to 690℃ and held for 10 minutes, and then heated to 710℃ and held for 3 minutes. The heating and cooling rates are 1.5℃ / min.

[0039] The cooling rate in step (4) is 8°C / s, and the wall thickness of the thin-walled part with through holes is 3mm.

[0040] Comparative Example 1 Based on Example 2, a cold heading process for a thin-walled part with a through hole is provided, which specifically includes the following steps: (1) The raw materials are put into a heating furnace for heat treatment, and then air-cooled to room temperature to obtain pretreated materials; (2) The pretreated material is axially upset to obtain a cylindrical blank; (3) The blank is placed into the mold cavity of the cold heading machine, and the punch continuously extrudes and shapes the blank through 5 stations to obtain the initial product of thin-walled part with through hole; (4) The initial product of the thin-walled part with through hole is placed in a heating furnace for cyclic annealing, and then cooled to room temperature in a cold extraction liquid to obtain the thin-walled part with through hole.

[0041] The specific steps of the heat treatment in step (1) are as follows: heat the raw material to 865℃ and keep it at that temperature for 30 minutes, then take it out and put it into a salt bath furnace at 215℃ and keep it at that temperature for 24 hours.

[0042] The elemental mass percentages of the raw materials are: C 0.65%, Si 0.45%, Mn 1.55%, P 0.018%, S 0.007%, Cr 0.05%, Cu 0.1%, with the remainder being Fe.

[0043] The blank in step (2) has a specification of Φ16mm×32mm.

[0044] The five stations in step (3) are specifically divided into: station 1 is for denting, station 2 is for compound extrusion, and stations 3, 4 and 5 are for thin-wall elongation forming. The continuous extrusion speed is 74 mm / s and the continuous extrusion temperature is 50°C.

[0045] The mold cavity in step (3) is subjected to phosphating treatment. The specific steps are as follows: a layer of phosphating solution is brushed onto the cavity of the mold and dried at 77°C, and then a layer of sodium stearate saponification solution is brushed onto the cavity and dried at 85°C. The phosphating solution is composed of phosphoric acid, zinc oxide, nitric acid, copper carbonate, sodium nitrate and water in a ratio of 41:27.5:22.5:3:38:100.

[0046] The specific steps of the cyclic annealing in step (4) are as follows: the initial product of the thin-walled part with through hole is heated to 705℃ and held for 2 minutes, then cooled to 685℃ and held for 9 minutes, and then heated to 705℃ and held for 2 minutes. The heating and cooling rates are 1.2℃ / min.

[0047] The cooling rate in step (4) is 6.5℃ / s, and the wall thickness of the thin-walled part with through holes is 2mm.

[0048] Comparative Example 2 Based on Example 2, a cold heading process for a thin-walled part with a through hole is provided, which specifically includes the following steps: (1) The raw materials are put into a heating furnace for heat treatment, and then air-cooled to room temperature to obtain pretreated materials; (2) The pretreated material is axially upset to obtain a cylindrical blank; (3) The blank is placed into the mold cavity of the cold heading machine, and the punch continuously extrudes and shapes the blank through 5 stations to obtain the initial product of thin-walled part with through hole; (4) The initial product of the thin-walled part with through hole is placed in a heating furnace for cyclic annealing, and then cooled to room temperature in a cold extraction liquid to obtain the thin-walled part with through hole.

[0049] The specific steps of heat treatment in step (1) are as follows: the raw material is heated to 1050℃ and kept at that temperature for 40 minutes. It is then taken out and placed in a salt bath furnace at 240℃ for 2.5 hours. Then, the temperature is raised to 650℃ and kept at that temperature for 3 hours. It is then air-cooled to room temperature. Next, the temperature is raised to 865℃ in a heating furnace and kept at that temperature for 30 minutes. It is then taken out and placed in a salt bath furnace at 215℃ for 24 hours.

[0050] The elemental mass percentages of the raw materials are: C 0.65%, Si 0.45%, Mn 1.55%, P 0.018%, S 0.007%, Cr 0.05%, Cu 0.1%, with the remainder being Fe.

[0051] The blank in step (2) has a specification of Φ16mm×32mm.

[0052] The blank in step (2) is first subjected to phosphating treatment. The specific steps are as follows: a layer of phosphating solution is brushed onto the surface of the blank and dried at 77°C, and then a layer of sodium stearate saponification solution is brushed onto it and dried at 85°C. The phosphating solution is composed of phosphoric acid, zinc oxide, nitric acid, copper carbonate, sodium nitrate and water in a ratio of 41:27.5:22.5:3:38:100.

[0053] The five stations in step (3) are specifically divided into: station 1 is for denting, station 2 is for compound extrusion, and stations 3, 4 and 5 are for thin-wall elongation forming. The continuous extrusion speed is 74 mm / s and the continuous extrusion temperature is 50°C.

[0054] The specific steps of the cyclic annealing in step (4) are as follows: the initial product of the thin-walled part with through hole is heated to 705℃ and held for 2 minutes, then cooled to 685℃ and held for 9 minutes, and then heated to 705℃ and held for 2 minutes. The heating and cooling rates are 1.2℃ / min.

[0055] The cooling rate in step (4) is 6.5℃ / s, and the wall thickness of the thin-walled part with through holes is 2mm.

[0056] Comparative Example 3 Based on Example 2, the continuous extrusion speed in step (3) was adjusted to 65 mm / s, while other conditions remained the same as in Example 2.

[0057] Comparative Example 4 Based on Example 2, the continuous extrusion speed in step (3) was adjusted to 85 mm / s, while other conditions remained the same as in Example 2.

[0058] Comparative Example 5 Based on Example 2, the cyclic annealing process in step (4) is removed, while other conditions remain the same as in Example 2.

[0059] Comparative Example 6 Based on Example 2, the cooling rate in step (4) was adjusted to 10°C / s, while other conditions remained the same as in Example 2.

[0060] Comparative Example 7 Based on Example 2, the cooling rate in step (4) was adjusted to 3°C / s, while other conditions remained the same as in Example 2.

[0061] Performance testing The thin-walled parts with through holes prepared in Examples 1-3 and Comparative Examples 1-7 were used as samples, and the microstructure, thickness uniformity, and crack area ratio of the samples were determined using a metallographic analyzer. The yield strength, tensile strength, and elongation of the samples were determined according to GB / T 228.1-2021. The test results are shown in Table 1.

[0062] Table 1 Test Results Sample Organizational structure Thickness uniformity and crack percentage Yield strength MPa Tensile strength (MPa) elongation % Example 1 Grid structure uniform 1232 1350 15.3 Example 2 Grid structure uniform 1249 1367 15.4 Example 3 Grid structure uniform 1227 1346 15.6 Comparative Example 1 Fiber structure Uniform, with a crack ratio of 1.53%. 893 1124 12.7 Comparative Example 2 Grid structure Uneven, with cracks accounting for 0.97%. 946 1163 12.2 Comparative Example 3 Grid structure uniform 1034 1209 17.9 Comparative Example 4 Grid structure Uneven, with cracks accounting for 1.36%. 907 1145 11.8 Comparative Example 5 Fiber structure Uniform, with a crack ratio of 2.97%. 853 1097 11.2 Comparative Example 6 Grid structure Uniform, with cracks accounting for 2.30%. 884 1100 12.3 Comparative Example 7 Grid structure uniform 1162 1264 17.2 Based on the comprehensive analysis of the data in Table 1, it can be concluded that Examples 1-3 all have a mesh structure with uniform thickness, and their yield strength and tensile strength are greater than those of Comparative Examples 1-7. Comparative Example 1: The raw material was not refined during heat treatment, and direct isothermal quenching formed nano-bainite. Subsequent cold heading and cyclic annealing hindered the formation of the mesh structure, and the fiber structure cracked under the same quenching rate, resulting in a significant reduction in mechanical properties. Comparative Example 2: The blank underwent phosphating and lubrication treatment. As the blank underwent cold heading deformation, the surface lubrication layer was damaged, leading to changes in friction and uneven thickness, resulting in cracks in thinner areas during quenching. Comparative Examples 3-4: The extrusion rate was adjusted by lowering or increasing. Lowering the rate restricted axial grain elongation, affecting the density of the mesh structure and thus reducing mechanical properties. Increasing the rate increased the stress, exceeding the grain elongation range and causing fracture, thus reducing mechanical properties. Comparative Example 5: No cyclic annealing step was performed, and the fiber structure could not transform into a mesh structure, resulting in weakened mechanical properties. Comparative Examples 6-7: The quenching rate was adjusted by raising or lowering the rate. Raising the rate exceeded the toughness range of the mesh structure, causing cracking. Lowering the rate resulted in insufficient refinement strength and weakened mechanical properties. In summary, Example 2 exhibits the best overall performance, and the mesh structure demonstrates superior mechanical strength compared to the fiber structure. This invention prepares thin-walled parts with through holes and uniform thickness with better mechanical properties through a process of raw material heat treatment, roughing, multi-station progressive cold heading, cyclic annealing, and quenching.

[0063] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A cold heading process for thin-walled parts with through holes, characterized in that, The cold heading process for the thin-walled part with through holes specifically includes the following steps: (1) The raw materials are put into a heating furnace for heat treatment, and then air-cooled to room temperature to obtain pretreated materials; (2) The pretreated material is axially upset to obtain a cylindrical blank; (3) The blank is placed into the mold cavity of the cold heading machine, and the punch continuously extrudes and shapes the blank through 5 stations to obtain the initial product of thin-walled part with through hole; (4) The initial product of the thin-walled part with through hole is placed in a heating furnace for cyclic annealing, and then cooled to room temperature in a cold extraction liquid to obtain the thin-walled part with through hole.

2. The cold heading process for a thin-walled part with a through hole according to claim 1, characterized in that, The specific steps of heat treatment in step (1) are as follows: heat the raw material to 1000-1100℃ and keep it at that temperature for 30-50 minutes, take it out and put it into a salt bath furnace at 220-260℃ and keep it at that temperature for 2-3 hours, then raise the temperature to 600-700℃ and keep it at that temperature for 3 hours, air cool it to room temperature, then raise the temperature to 850-880℃ in a heating furnace and keep it at that temperature for 30 minutes, take it out and put it into a salt bath furnace at 200-230℃ and keep it at that temperature for 24 hours.

3. The cold heading process for a thin-walled part with a through hole according to claim 1, characterized in that, The elemental mass percentages of the raw materials are: C 0.6-0.7%, Si 0.3-0.6%, Mn 1.4-1.65%, P 0.01-0.025%, S 0.005-0.01%, Cr 0.04-0.068%, Cu 0.089-0.16%, with the remainder being Fe.

4. The cold heading process for a thin-walled part with a through hole according to claim 1, characterized in that, The blank in step (2) has a specification of Φ16mm×32mm.

5. The cold heading process for a thin-walled part with a through hole according to claim 1, characterized in that, The five stations in step (3) are specifically divided into: station 1 is for denting, station 2 is for compound extrusion, and stations 3, 4 and 5 are for thin-wall elongation forming. The continuous extrusion speed is 70-78 mm / s and the continuous extrusion temperature is 40-60℃.

6. The cold heading process for a thin-walled part with a through hole according to claim 1, characterized in that, The mold cavity in step (3) is subjected to phosphating treatment. The specific steps are as follows: a layer of phosphating solution is brushed onto the cavity of the mold and dried at 75-80°C, and then a layer of sodium stearate saponification solution is brushed onto the cavity and dried at 80-90°C. The phosphating solution is composed of phosphoric acid, zinc oxide, nitric acid, copper carbonate, sodium nitrate and water in a ratio of 41:27.5:22.5:3:38:

100.

7. The cold heading process for a thin-walled part with a through hole according to claim 1, characterized in that, The specific steps of the cyclic annealing in step (4) are as follows: the initial product of the thin-walled part with through hole is heated to 700-710℃ and held for 2-3 minutes, then cooled to 680-690℃ and held for 8-10 minutes, and then heated to 700-710℃ and held for 2-3 minutes. The heating and cooling rates are 1-1.5℃ / min.

8. The cold heading process for a thin-walled part with a through hole according to claim 1, characterized in that, The cooling rate in step (4) is 5-8℃ / s, and the wall thickness of the thin-walled part with through holes is 1-3mm.