一种基于GFM1800吨径锻机大规格锻材锻透性的提升方法
By using a stepped forging method with R220 or R280 hammers on a GFM1800-ton diameter forging mill, the forging process is decomposed into multiple sections, reducing the surface temperature and using internal high temperature to break the grains, thus solving the problems of coarse grains and loose structure, and achieving high-efficiency forging penetration of large-size forgings.
Patent Information
- Application Number
- CN202611413929.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-24
AI Technical Summary
When the GFM1800-ton radial forging mill produces forgings with a diameter greater than ∮350, it exhibits coarse grains and a loose microstructure, resulting in substandard forgings.
Using R220 or R280 hammerheads, a stepped forging process with 7-9 deformation passes is performed. The forging process is broken down into multiple sections. After forging, the surface temperature of each section is reduced, and multiple forging passes are performed using the internal high temperature to break up the grains and form a wave-shaped and segmented forging method.
It improves the forging penetration of large-size forgings, solves the problems of coarse grains and loose structure, and improves production efficiency, achieving a combination of good forging penetration and high efficiency.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of forging performance improvement technology, and in particular relates to a method for improving the forging penetration of large-diameter forgings based on a GFM1800 ton-diameter forging machine. Background Technology
[0002] The GFM 1800t radial forging mill, introduced in 2010, was the world's largest radial forging equipment at the time. Its production capacity is 100,000 tons of forgings per year, including square steel, flat steel, round steel, stepped shafts, forged pipes, etc., involving multiple varieties such as carbon steel, alloy structural steel, die steel, CrNi stainless steel, and petroleum steel. The product specifications are ∮560~∮80, the maximum weight of raw materials is 10 tons, and the longest forgings that can be produced is 22m in length.
[0003] Users have increasingly higher requirements for product quality, shifting from demand in the ordinary steel market to demand in the high-end market. Not only are internal quality requirements high, but also the requirements for external dimensions (larger diameter, longer length) are more stringent. However, the upstream process of the radial forging mill lacks the support of large-scale forging. In production, when using ∮690 continuously cast round billets as raw materials to produce forgings larger than ∮350, a large number of coarse grains and loose microstructures will appear, causing flaw detection and resulting in unqualified forgings. Summary of the Invention
[0004] The purpose of this invention is to provide a method for improving the forging penetration of large-size forgings based on the GFM1800-ton radial forging machine, which solves the problem that when the GFM1800-ton radial forging machine produces forgings with a specification greater than ∮350, a large number of coarse grains and loose structure will appear, causing defects in the forgings and resulting in unqualified forgings.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill, the specific steps of which are as follows: (i) Before forging, according to the weight of the continuous casting round billet raw material and the size requirements of the finished product, the forging hammer head is replaced with R220 or R280 model, the hammer head lifting value is set from the original 10mm to 15-20mm, and production is carried out according to the stepped forging round forging method with 7-9 deformation passes. (ii) In the first to third passes, the ∮690 continuous casting round billet is forged into a straight bar of ∮600-∮480, in preparation for the stepped forging round; (III) During the 2nd to 4th forging passes, the B operating carriage moves 900-1000mm while maintaining a speed of 2-2.5m / min, leaving a peak length of 500-800mm. The forging process proceeds from ∮600-∮480 to ∮540-∮440, completing one trough forging and forming a section. Each section consists of one peak and one trough. The hammer head is opened 2-3 times consecutively, opening by 40-60mm. This process is repeated to forge the next section until the current pass is completed. (iv) During the 3rd to 5th forging passes, observe whether the head of the billet is a peak or a trough. If it is a trough, forge from ∮540-∮440 to ∮420-∮400, with the trolley moving 500-800mm to complete one section of forging. Repeat this process to forge the next section until the current pass is completed, and so on for subsequent passes. If it is a peak, forge from ∮600-∮480 to ∮540-∮440, opening the hammer head 2-3 times consecutively, opening the hammer head 40-60mm, with the trolley moving 500-800mm to complete the peak forging. The trolley then moves another 500-800mm to reach the trough, forging from ∮540-∮440 to ∮420-∮400. Repeat this process to forge the next section until the current pass is completed, and so on for subsequent passes. (v) Continue forging for the 6th to the last forging pass, and the forging is completed.
[0006] Preferably, the travel speed of the operating vehicle in (ii) and (iii) is controlled at 2-2.5 m / min.
[0007] Preferably, the deformation amount of the first forging pass in (ii) is controlled at 70-90mm.
[0008] Preferably, the forging deformation amount of each pass in the second and third passes of (ii) and (iii) is 40-70mm.
[0009] Preferably, the surface temperature of the forging material is reduced during the forging processes of (ii), (iii), (iv) and (v), with the surface temperature of the forging material reduced by 50-100°C after each pass.
[0010] Preferably, the forging deformation amount of each pass in the 4th and 5th passes in (iii) and (iv) is ≤40mm.
[0011] Preferably, the forging deformation amount of each pass from the 6th to the last pass in (v) is ≤35mm.
[0012] Preferably, the walking speed of the operating vehicle in step (v) is maintained at 2-3 m / min.
[0013] Preferably, the surface temperature of the forged material in the fifth step is as low as 800-850℃.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: This method decomposes the forging process into multiple forging sections. The temperature of each section decreases after forging. When forging the next stage, the surface temperature is low and the metal has poor fluidity, while the internal temperature is high and the metal has good fluidity, breaking down the core grains. Repeating multiple forging stages prevents internal porosity and coarse grain breakage, solves the problem of non-compliance in flaw detection after forging, improves the forging penetration of forgings with a diameter forging machine producing forgings larger than ∮350, overcomes the defects of fast forging machines having good forging penetration but slow forging speed, and diameter forging machines having fast forging speed but poor forging penetration, and achieves a combination of good forging penetration and high efficiency, forming a stepped forging round forging combination that combines wave-shaped, segmented, and low-temperature extrusion. Detailed Implementation
[0015] The technical solution of the present invention will be described in detail below with reference to the embodiments. Example 1
[0016] This embodiment uses a GFM1800-ton diameter forging machine, with ∮690 continuously cast round billets of 42CrMo as raw materials, the billet weight is 9.6t, and the forging specification is ∮350mm.
[0017] Before forging, the deformation amount for each pass is calculated according to the process requirements to ensure that the length of the forging material does not exceed 15m in the penultimate pass. If the length exceeds 15m, production is not possible (due to the limitation of the forging center hole diameter of the operating carriage). The present invention provides a method for improving the forging penetration of large-diameter forgings using a GFM1800 ton-diameter forging machine. The specific steps are as follows: (a) Before forging, according to the weight of the ∮690 continuous casting round billet raw material and the size requirements of the finished product, the forging hammer head is replaced with R220 model, and the hammer head lifting value is set from the original 10mm to 20mm. The forging is carried out in 9 deformation passes, and the production is carried out in 9-pass stepped forging round forging method.
[0018] (ii) The forging deformation amount of the first pass is controlled at 90mm, and the forging deformation amount of the second and third passes is controlled at 60mm respectively. The travel speed of the operating trolley is controlled at 2m / min. The ∮690 continuous casting round billet is forged into a ∮480 straight bar to prepare for stepped forging round.
[0019] (III) During the fourth forging pass, the deformation is controlled at 40mm. The B operating carriage moves 1000mm while maintaining a speed of 2m / min, leaving a peak length of 500mm. The forging is carried out from ∮480 to ∮440, completing one trough forging and forming a section. A section consists of one peak and one trough. The hammer is opened twice consecutively, opening by 40mm, while maintaining a speed of 2m / min. This process is repeated to forge the next section until the fourth pass is completed. During the forging process, the surface temperature of the forging material decreases, and the surface temperature of the forging material decreases by 50℃ after each pass.
[0020] (iv) During the 5th forging pass, observe whether the head of the billet is a peak or a trough. If it is a trough, forge directly from ∮440 to ∮400. The deformation amount of the 5th pass is controlled at 40mm. The operating carriage travels 500mm to complete one section of forging. The hammer head opens to 440mm twice, and the forging peak ∮480 is reduced to 440. The operating carriage travels 500mm to complete the peak forging. The operating carriage travels another 500mm to reach the trough, and ∮440 is forged to ∮400. The travel speed is maintained at 2m / min. This process is repeated to forge the next section until the 5th pass is completed. During the forging process, the surface temperature of the forging material decreases, while the core remains at a high temperature. The fluidity of the surface metal decreases, and the kinetic energy of forging is directed more towards the core. At the same time, the core grains are crushed by side compression.
[0021] (v) Continue forging until the 9th pass for round forging, and the forging is completed. The deformation of the 6th and 7th passes is controlled at 35mm and 30mm respectively. The 8th pass is an empty feed pass that incorporates the straightening process of the head. The 9th pass completes the finishing pass forging to the finished size ∮350mm. During the forging process, the walking speed is maintained at 3m / min. The surface temperature of the forged material in the finished pass is as low as 800℃. Example 2
[0022] This embodiment uses a GFM1800-ton diameter forging machine, with ∮690 continuously cast round billets of 38CrMoAl as raw materials, the billet weight is 8.4t, and the forging specification is ∮380mm.
[0023] The method for improving the forging penetration of large-diameter forgings based on a GFM1800 ton-diameter forging mill, provided by this invention, comprises the following specific steps: (a) Before forging, based on the weight of the ∮690 continuous casting round billet raw material and the size requirements of the finished product, the forging hammer head is replaced with the R280 model, and the hammer head lifting value is set from the original 10mm to 20mm. Production is carried out according to the 7-pass stepped forging round forging method.
[0024] (ii) The forging deformation amount of the first pass is controlled at 80mm, the forging deformation amount of the second pass is controlled at 70mm, the travel speed of the operating trolley is controlled at 2m / min, and the ∮690 continuous casting round billet is forged into a ∮540 straight bar to prepare for stepped forging round.
[0025] (III) During the third forging pass, the deformation is controlled at 40mm. The A operating carriage moves 1000mm while maintaining a speed of 2m / min, leaving a peak length of 500mm. The forging process is carried out from ∮540mm to ∮500mm, completing one trough forging and forming a section. Each section consists of one peak and one trough. The hammer is opened twice consecutively, opening by 40mm each time, while maintaining a speed of 2m / min. This process is repeated to forge the next section until the third pass is completed. During the forging process, the surface temperature of the forging material decreases, and the surface temperature of the forging material decreases by 50℃ after each pass.
[0026] (iv) During the fourth forging pass, observe whether the head of the billet is a peak or a trough, and let it stand for 2-3 minutes (the larger the diameter of the raw material, the slower the temperature drop, so let it stand to cool down). If it is a trough, forge directly from ∮500mm to ∮460mm. The deformation amount of the fourth pass is controlled at 40mm. The operating carriage travels 500mm to complete one section of forging. Open the hammer twice in succession. When the hammer is opened to 500mm, the forging peak ∮540mm is reduced to 500mm. The operating carriage travels 500mm to complete the peak forging. The operating carriage then travels another 500mm to reach the trough. Forge from ∮500mm to ∮460mm. The traveling speed is maintained at 2m / min. Continue in this manner to forge the next section until the fourth pass is completed.
[0027] (V) During the 5th forging pass, observe whether the head of the billet is a peak or a trough, and let it stand for 2-3 minutes (for larger billet diameters, the temperature drops slowly, so let it stand to cool down). If it is a trough, forge directly from ∮460mm to ∮420mm. The deformation amount of the 5th pass should be controlled at 40mm. The operating carriage should travel 500mm to complete one section of forging. Open the hammer head twice consecutively, opening it to 460mm. The forging peak ∮500mm should be reduced to 460mm. The operating carriage should then... After forging the 500mm wave crest, the trolley travels another 500mm to reach the wave trough, forging from ∮460mm to ∮420mm, maintaining a travel speed of 2m / min. This process is repeated to forge the next section until the 5th pass is completed. During the forging process, the surface temperature of the forging material decreases, while the core remains at a high temperature. The fluidity of the surface metal decreases, and the kinetic energy of the forging is directed more towards the core. At the same time, the core grains are crushed by side compression.
[0028] (vi) Continue forging the 6th pass. The deformation amount in the 6th pass is controlled at 70mm. The segmented stepped forging is rounded to a round bar with a diameter of ∮390mm. The straightening process of the head is incorporated into the 7th pass. The deformation amount is 10mm to complete the finishing pass forging to the finished size of ∮380mm. During the forging process, the walking speed is maintained at 2m / min. The surface temperature of the forged material in the finished pass is as low as 850℃. Example 3
[0029] This embodiment uses a GFM1800-ton diameter forging machine, with ∮690 continuously cast round billet F60 as raw material, billet weight 9.6t, and forging specification ∮400mm.
[0030] Before forging, the deformation amount and finished length for each pass are calculated and determined according to the process requirements. The method for improving the forging penetration of large-diameter forgings based on the GFM1800-ton diameter forging machine provided by this invention is adopted, and the specific steps are as follows: (a) Before forging, according to the weight of the ∮690 continuous casting round billet raw material and the size requirements of the finished product, the forging hammer head is replaced with the R280 model, and the hammer head lifting value is set from the original 10mm to 20mm. Production is carried out in a stepped forging round forging method of 6 deformation passes plus one empty feed pass (6+1).
[0031] (ii) The forging deformation in the first pass is controlled to a maximum of 90mm, and the travel speed of the operating vehicle is controlled to 2m / min. The ∮690mm continuous casting round billet is forged into a ∮600mm straight bar to prepare for stepped forging.
[0032] (III) During the second forging pass, let it stand for 4-5 minutes (the temperature drops slowly when the raw material diameter is large, so let it stand to cool down). Control the deformation to 60mm. The B operating carriage clamps and moves 1000mm, maintaining a speed of 2m / min. Leave a peak length of 500mm. Forge from ∮600mm to ∮540mm to complete one trough forging, forming a section. A section consists of one peak and one trough. Open the hammer head 3 times consecutively, opening the hammer head 60mm. Maintain a speed of 2m / min. Continue this process to forge the next section until the second pass is completed. During the forging process, the surface temperature of the forging material decreases. The surface temperature of the forging material decreases by 100℃ after the completion of this pass.
[0033] (iv) During the third forging pass, observe whether the head of the billet is a peak or a trough, and let it stand for 4-5 minutes (the larger the raw material diameter, the slower the temperature drop, so let it stand to cool down). If it is a trough, forge directly from ∮540mm to ∮480mm. The deformation amount of the third pass is controlled at 60mm. The operating carriage travels 500mm to complete one section of forging. Open the hammer head three times in a row. When the hammer head is opened to 540mm, the forging peak ∮600mm is reduced to 540mm. The operating carriage travels 500mm to complete the peak forging. The operating carriage then travels another 500mm to reach the trough. Forge from ∮540mm to ∮480mm. The traveling speed is maintained at 2m / min. Continue in this manner to forge the next section until the third pass is completed.
[0034] (V) During the fourth forging pass, observe whether the billet head is a peak or a trough, and let it stand for 2-3 minutes (larger billet diameters result in slower temperature drop, allowing it to stand and cool). If it is a trough, forge directly from ∮480mm to ∮420mm. Control the deformation amount of the fourth pass to 60mm, and move the trolley 500mm to complete one section of forging. Press the hammer open button three times consecutively to open the hammer to 480mm, and forge the peak ∮540mm to 480mm. The forging process is completed after the machine travels 500mm to the crest of the wave. The machine then travels another 500mm to the trough, forging from ∮480mm to ∮420mm. The travel speed is maintained at 2m / min. This process is repeated to forge the next section until the 4th pass is completed. During the forging process, the surface temperature of the forging material decreases, while the core remains at a high temperature. The fluidity of the surface metal decreases, and the kinetic energy of the forging is directed more towards the core. At the same time, the core grains are crushed by lateral compression.
[0035] (vi) Continue forging the 5th pass, with the deformation amount controlled at 60mm, and forge the segmented stepped forging to a round bar of ∮420mm; the deformation amount of the 6th pass is 20mm, and the finishing pass is forged to the finished size of ∮400mm. During the forging process, the walking speed is maintained at 2m / min, and the surface temperature of the finished forging is below 850℃.
[0036] (vii) Empty feeding forming pass, no deformation, forging size ∮400mm, one pass from beginning to end, the traveling speed is kept at 2m / min during the process, to perform straightness shaping and surface strengthening of the forging material.
[0037] After forging using the method of this invention, the hidden dangers of coarse grains and loose structure in the core of the continuously cast round billet are eliminated, the surface is free of defects, and the straightness and external dimensions of the finished product meet the requirements.
Claims
1. A method for improving the forging penetration of large-diameter forgings using a GFM1800-ton diameter forging mill, characterized in that, The specific steps are as follows: (i) Before forging, according to the weight of the continuous casting round billet raw material and the size requirements of the finished product, the forging hammer head is replaced with R220 or R280 model, the hammer head lifting value is set from the original 10mm to 15-20mm, and production is carried out according to the stepped forging round forging method with 7-9 deformation passes. (ii) In the first to third passes, the ∮690 continuous casting round billet is forged into a straight bar of ∮600-∮480, in preparation for the stepped forging round; (III) During the 2nd to 4th forging passes, the B operating carriage moves 900-1000mm while maintaining a speed of 2-2.5m / min, leaving a peak length of 500-800mm. The forging process proceeds from ∮600-∮480 to ∮540-∮440, completing one trough forging and forming a section. Each section consists of one peak and one trough. The hammer head is opened 2-3 times consecutively, opening by 40-60mm. This process is repeated to forge the next section until the current pass is completed. (iv) During the 3rd to 5th forging passes, observe whether the head of the billet is a peak or a trough. If it is a trough, forge from ∮540-∮440 to ∮420-∮400, with the trolley moving 500-800mm to complete one section of forging. Repeat this process to forge the next section until the current pass is completed, and so on for subsequent passes. If it is a peak, forge from ∮600-∮480 to ∮540-∮440, opening the hammer head 2-3 times consecutively, opening the hammer head 40-60mm, with the trolley moving 500-800mm to complete the peak forging. The trolley then moves another 500-800mm to reach the trough, forging from ∮540-∮440 to ∮420-∮400. Repeat this process to forge the next section until the current pass is completed, and so on for subsequent passes. (v) Continue forging for the 6th to the last forging pass, and the forging is completed.
2. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, The travel speed of the operating vehicle in (ii) and (iii) is controlled at 2-2.5 m / min.
3. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, The deformation amount of the first forging pass in (ii) is controlled at 70-90mm.
4. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, The forging deformation amount for each of the second and third passes in (ii) and (iii) is 40-70 mm.
5. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, During the forging processes described in (ii), (iii), (iv) and (v), the surface temperature of the forging material decreases, with the surface temperature of the forging material decreasing by 50-100°C after each pass.
6. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, The forging deformation amount of each pass in the 4th and 5th passes of (iii) and (iv) is ≤40mm.
7. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, In section (v), the forging deformation amount of each pass from the 6th to the last pass is ≤35mm.
8. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, The operating vehicle in (v) shall maintain a travel speed of 2-3 m / min.
9. The method for improving the forging penetration of large-diameter forgings based on a GFM1800-ton diameter forging mill according to claim 1, characterized in that, The surface temperature of the forged material in the fifth step is as low as 800-850℃.