High-precision temperature control forming method for TRB bearing ring forging
By setting multiple temperature measurement points in the cooling zone, the cooling intensity and conveying speed are monitored in real time and dynamically adjusted, solving the problem of uneven cooling of forgings in traditional forging processes. This achieves uniform hardness and consistent metallographic structure in the forgings, thus improving the quality of bearing rings.
Patent Information
- Application Number
- CN202611303753.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional forging processes involve rudimentary cooling control of forgings, resulting in uneven hardness distribution, localized stress concentration, and uneven metallographic structure within the forgings, making it difficult to meet the quality requirements of high-precision bearing rings.
Multiple temperature measurement points are set up in the cooling zone to monitor the temperature change rate in real time. By adjusting the cooling intensity and conveying speed through dynamic closed-loop control, the cooling rate of each section is ensured to be within the target range. Combined with double heating and isothermal annealing processes, the entire process of forging quality control is achieved.
This achieved uniformity in hardness and consistency in metallographic structure of the forgings, improved the pass rate of ultrasonic testing, and met the quality requirements of high-precision bearing rings.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of bearing ring forging technology, and particularly relates to a high-precision TRB bearing ring forging temperature-controlled forming method. Background Technology
[0002] TRB bearing rings, as precision transmission components, have extremely high requirements for dimensional accuracy, metallographic uniformity, and internal quality. During the forging process of bearing rings, the forgings need to undergo controlled cooling after rolling to eliminate internal stress, refine grains, and obtain the expected hardness distribution, thus preparing the microstructure for the subsequent isothermal annealing process.
[0003] Traditional forging processes employ relatively crude methods for cooling forgings after rolling and expanding, typically using fixed airflow or a single variable-speed air cooling system. This means that the cooling intensity and forging conveyor speed remain constant throughout the cooling process, or are only adjusted independently in an open-loop manner, lacking real-time monitoring and feedback control of the actual cooling rate. Because the temperature decay characteristics of forgings differ across cooling zones and initial temperatures fluctuate from batch to batch, fixed-parameter cooling methods struggle to adapt to changing working conditions. This can easily lead to overcooling or undercooling in different sections of the cooling zone, resulting in defects such as uneven hardness distribution, localized stress concentration, and excessive network carbides within the forging. Furthermore, the lack of precise control over the final cooling temperature results in unstable temperature conditions before the forging enters the isothermal annealing process, directly affecting the uniformity of the subsequent annealed microstructure. This leads to low ultrasonic testing pass rates, making it difficult to meet the quality requirements of high-precision bearing rings. Summary of the Invention
[0004] To address the problems in the prior art, the present invention proposes the following technical solution: This invention provides a high-precision temperature-controlled forging method for TRB bearing rings, comprising the following steps: S1. Forging: The billet is heated to the forging temperature and then forged into a ring forging. S2. Temperature measurement point layout: The annular forging is sent into the cooling zone, and the first temperature measurement point, the second temperature measurement point, ..., the nth temperature measurement point are set sequentially along the length of the cooling zone, where n≥3, and the temperature measurement points are distributed at equal intervals. S3. Temperature Monitoring and Cooling Rate Calculation: Real-time acquisition of temperature values T1, T2, ..., T at each temperature measurement point. n Calculate the rate of temperature change V between adjacent temperature measurement points. i = (T i -T i+1 ) / Δt, where Δt is the time it takes for the forging to move from the i-th temperature measuring point to the (i+1)-th temperature measuring point; S4. Cooling rate comparison and dynamic adjustment: The measured temperature change rate V of each segment is compared and adjusted. iand compared with the preset target temperature change rate V0; When V i >V0, the cooling intensity of the cooling zone is reduced and the conveying speed of the forgings is increased simultaneously, so that V i falls back within the allowable deviation range of V0; When V i <V0, the cooling intensity of the cooling zone is increased and the conveying speed of the forgings is reduced simultaneously, so that V i rises within the allowable deviation range of V0; When V i is within the allowable deviation range of V0, the current cooling intensity and conveying speed are kept unchanged; S5, circularly controlling until the final cooling reaches the standard: repeating S3~S4 until the final cooling temperature of the forgings reaches the target temperature when the forgings leave the cooling zone.
[0005] As a preference of the above technical solution, the cooling zone is an air cooling line, the cooling intensity is achieved by adjusting the air supply volume of the air cooling line, and the conveying speed of the forgings is achieved by adjusting the rotation speed of the transmission motor of the air cooling line.
[0006] As a preference of the above technical solution, in step S4, the "simultaneously reducing the cooling intensity of the cooling zone and increasing the conveying speed of the forgings" refers to: gradually reducing the air supply volume with a step length of 10% of the current air supply volume, and simultaneously gradually increasing the rotation speed with a step length of 5% of the current rotation speed, and entering the next level after the temperature reading is stable after each level of adjustment; the "simultaneously increasing the cooling intensity of the cooling zone and reducing the conveying speed of the forgings" refers to: gradually increasing the air supply volume with a step length of 10% of the current air supply volume, and simultaneously gradually reducing the rotation speed with a step length of 5% of the current rotation speed, and entering the next level after the temperature reading is stable after each level of adjustment.
[0007] As a preference of the above technical solution, in step S4, the allowable deviation range is ±15% of V0.
[0008] As a preference of the above technical solution, in step S5, the target temperature is 650℃~720℃.
[0009] As a preference of the above technical solution, in step S1, the "heating the billet to the forging temperature and then forming it into a ring forging by forging" specifically includes: S1-1 primary heating and preforming: heating the bearing steel material section to the initial forging temperature, and forming a preformed billet through upsetting, punching, bottom cutting and end face flattening; S1-2 secondary heating: heating the preformed billet again to the same initial forging temperature; S1-3 rolling final forming: feeding the preformed billet after secondary heating into a numerical control radial-axial ring rolling machine for rolling forming to obtain a ring forging.
[0010] As a preferred embodiment of the above technical solution, the initial forging temperature mentioned in S1-1 and S1-2 is 1150℃~1200℃.
[0011] As a preferred embodiment of the above technical solution, step S5 further includes: S6. Isothermal Annealing: The cooled forgings are loaded into an annealing furnace for isothermal annealing. The annealing temperature is controlled by a closed-loop thermocouple in the furnace. After annealing, the hardness and metallographic structure of the forgings are tested.
[0012] The beneficial effects of this invention are as follows: (1) This invention achieves dynamic closed-loop precise control of the entire forging cooling process by sequentially setting multiple temperature measurement points in the cooling zone and collecting the temperature values of each point in real time, calculating the temperature change rate between adjacent temperature measurement points, comparing the measured temperature change rate of each segment with the target temperature change rate, and synchronously adjusting the cooling intensity and forging conveying speed of the cooling zone based on the comparison results. The above monitoring and adjustment process is repeated until the final cooling temperature reaches the target, thus realizing dynamic closed-loop precise control of the entire forging cooling process. This scheme forms multiple temperature monitoring sections at different locations in the cooling zone, calculates the cooling rate in segments rather than relying solely on a single final cooling temperature, and can accurately identify the specific cooling rate deviation of each segment during the cooling process of the forging. It can then adjust the cooling intensity and conveying speed of the corresponding segments accordingly, thereby stabilizing the cooling rate of each segment within the target range, effectively avoiding overcooling or undercooling, and significantly improving the hardness uniformity and metallographic consistency of the forging.
[0013] (2) This invention sets the cooling zone as an air-cooled line to adjust the cooling intensity by adjusting the air volume and the forging conveying speed by adjusting the speed of the drive motor. It adopts a step-by-step adjustment method, and after each adjustment, the temperature reading is stabilized before entering the next level. Combined with the setting of the allowable deviation range, the matching relationship between the cooling intensity and the conveying speed is always coordinated during the adjustment process, avoiding temperature oscillation caused by large-scale sudden adjustment. The adjustment process is smooth and controllable, and converges quickly, which has good industrial practicality and operability.
[0014] (3) By controlling the final cooling target temperature within the furnace loading temperature window of isothermal annealing, the forging can directly enter the annealing process when it leaves the cooling zone, avoiding energy waste and uneven structure caused by reheating after excessive cooling; at the same time, in conjunction with the double heating forging process, after completing upsetting, punching, bottom cutting and flat end face pre-forming by heating once, it is heated again to the same initial forging temperature, so that the billet eliminates local temperature drop before entering the ring rolling mill, ensuring uniform deformation and consistency of structure during the rolling process; then, through the isothermal annealing process controlled by thermocouple closed loop in the annealing furnace, the spheroidization of carbides and the full release of stress are completed at the precise annealing temperature, forming a full-process quality control from forging, controlled cooling to annealing, comprehensively improving the hardness uniformity, metallographic structure level and ultrasonic testing pass rate of the forging. Detailed Implementation
[0015] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments.
[0016] To address the problem in traditional cooling control where inconsistent phase transformation paths occur in different parts of the forging due to deviations in cooling rates at different stages, leading to localized hardness fluctuations and poor microstructure uniformity, this invention achieves precise control of the cooling path through segmented monitoring and synchronous reverse adjustment. This ensures that all parts of the forging undergo the same phase transformation path, thereby achieving synergistic optimization of hardness uniformity and microstructure consistency at the microstructural level. This invention sequentially sets multiple temperature measurement sections along the cooling zone, dividing the cooling zone into continuous temperature monitoring intervals. It acquires the actual temperature change rate of the forging within each interval, thereby accurately locating the specific segment and direction of the cooling rate deviation. When the measured cooling rate is too high in a certain segment, the cooling intensity is reduced to decrease the temperature drop in that segment, while the conveying speed is increased to shorten the residence time. These two actions work together to bring the cooling rate of that segment back to the target range. When the measured cooling rate is too low, the cooling intensity is increased to increase the cooling driving force, while the conveying speed is decreased to extend the residence time. These two actions work together to raise the cooling rate of that segment to the target range. The synchronous and reverse adjustment of cooling intensity and conveying speed allows the cooling intensity to control the temperature drop of the forging per unit time, and the conveying speed to control the residence time of the forging in each segment. These two actions complement each other in the time dimension, decoupling the cooling rate control from the final cooling temperature. By repeatedly performing the above segmented monitoring, comparison, and step-by-step adjustment, the cooling rate of each segment gradually converges to the target deviation range, and the final cooling temperature synchronously stabilizes at the target value. The aforementioned control process ensures that each section of the forging passes through its respective temperature range at a preset cooling rate. This means that austenite decomposition occurs within the preset temperature window, the undercooling of pearlite transformation in each part tends to be consistent, and the pearlite lamellar spacing and carbide particle size distribution tend to be uniform. The stability of the final cooling temperature further guarantees the consistency of the microstructure of the forging before entering the isothermal annealing process. Based on this, the isothermal annealing process completes the spheroidization of carbides at a precise annealing temperature. Since the controlled cooling stage has provided a uniform precursor microstructure for each part, the carbide dissolution-precipitation kinetics in each part tends to be consistent during annealing. The spheroidized carbide particles have uniform size and distribution, ultimately achieving synergistic optimization of hardness uniformity and microstructure consistency at the entire process level.
[0017] It should be noted that in the cyclic control process of steps S3 to S5 in the following embodiments, the Δt is re-measured in real time according to the current conveying speed in each cycle, instead of using the initial measurement value; the "stable temperature reading" in step S4 means that the temperature difference between two adjacent samplings does not exceed ±2℃; when there are cooling speed sections that are higher and lower than the target range at the same time, the section with the largest percentage deviation from the target value is the priority adjustment target.
[0018] Example 1
[0019] This embodiment provides a high-precision temperature-controlled forming method for forging TRB bearing rings, applied to the forging of NP611293 model TRB bearing rings, specifically including the following steps.
[0020] S1. Forging and shaping: NP611293 type TRB bearing steel bar (grade SUJ2) was selected and sawn into segments weighing 2.8 kg each. The segments were placed in a natural gas heating furnace and heated to the initial forging temperature of 1180℃ at a heating rate of 10℃ / min, and held for 15 min. The heated segments were then removed and fed into a forging press, where they were sequentially upset (upset ratio 2.0, forged outer diameter 130 mm), punched (punch diameter 50 mm), undercut (removing 8 mm of the outer layer), and flattened (height 45 mm after flattening) to form a preform.
[0021] The preformed billet is placed back into the natural gas heating furnace and heated to 1180℃, and held for 10 minutes. The preformed billet after the second heating is then fed into a CNC radial axial rolling mill, with a rolling ratio of 1.8 and a rolling speed of 2.5 mm / s, to roll and form a ring forging (outer diameter 172 mm, inner diameter 95 mm, height 38 mm).
[0022] S2. Temperature measurement point layout: The rolled and expanded annular forging is fed into the air-cooling line cooling zone. Temperature measuring points 1, 2, and 3 are sequentially set along the length of the air-cooling line (n=3), with a spacing of 1.5m between each point. The first measuring point is located at the inlet of the air-cooling line, the second at the middle (1.5m from the inlet), and the third at 1.5m before the outlet (3.0m from the inlet). All measuring points use type K thermocouples (accuracy ±1.0℃), with a temperature acquisition frequency of 1 time / second.
[0023] S3. Temperature monitoring and cooling rate calculation: After the annular forging enters the air-cooling cooling zone, temperature monitoring is initiated. The measured time Δt1 for the forging to move from the first temperature measuring point to the second temperature measuring point is 12 seconds, and the measured time Δt2 for moving from the second temperature measuring point to the third temperature measuring point is also 12 seconds. Real-time temperature values at the three measuring points are collected: T1 = 820℃, T2 = 740℃, and T3 = 700℃. The rate of temperature change between adjacent measuring points is calculated. V1=(T1-T2) / Δt1=(820-740) / 12=80 / 12≈6.67℃ / s; V2=(T2-T3) / Δt2=(740-700) / 12=40 / 12≈3.33℃ / s.
[0024] S4. Cooling rate comparison and dynamic adjustment: Based on the continuous cooling transformation curve of the bearing ring steel (SUJ2) for model NP611293, the target temperature change rate V0 is set to 4.50℃ / s, and the allowable deviation range of V0 is ±15%, that is, the lower limit of the actual cooling rate is 3.83℃ / s and the upper limit is 5.18℃ / s.
[0025] Initial state: Air supply volume 2800m³ 3 / h, rotation speed 1200r / min, V1=6.67℃ / s (too high), V2=3.33℃ / s (slightly below the lower limit of 3.83℃).
[0026] Round 1: V1 is predominantly high, so the air supply volume will be reduced from 2800m³ / h. 3 / h is reduced to 2520m in 10% increments. 3 / h, while increasing the rotational speed from 1200r / min to 1260r / min in 5% increments.
[0027] After adjustment, T1=790℃, T2=735℃, T3=698℃; V1=(790-735) / 12≈4.58℃ / s (meets the standard). V2=(735-698) / 12≈3.08℃ / s (too low).
[0028] Round 2: V2 is too low, reduce the air supply from 2520m³ / h 3 / h increased to 2772m in 10% increments. 3 / h, while reducing the rotational speed from 1260r / min to 1197r / min in 5% increments.
[0029] After adjustment, T1=798℃, T2=740℃, and T3=695℃. V1=(798-740) / 12≈4.83℃ / s (meets the standard). V2 = (740 - 695) / 12 = 3.75℃ / s (close to the lower limit of 3.83℃); Round 3: V2 is still slightly low, so the air supply volume will be reduced from 2772m³ / h. 3 / h increased to 3049m in 10% increments. 3 / h, while reducing the rotational speed from 1197r / min to 1137r / min in 5% increments.
[0030] After adjustment, T1=805℃, T2=748℃, and T3=700℃. V1=(805-748) / 12=4.75℃ / s (meets the standard). V2=(748-700) / 12=4.00℃ / s (meets the standard).
[0031] After three rounds of adjustment, V1=4.75℃ / s and V2=4.00℃ / s, both within the range of 3.83~5.18℃ / s, indicating that the adjustment is complete.
[0032] S5. Circulation control until final cooling meets the standard: After the above adjustments are completed, the forging continues to move forward in the air-cooling line. Steps S3 to S4 are repeated cyclically to continuously monitor and control the entire cooling process of the forging. When the forging leaves the cooling zone, the final cooling temperature T3 = 700℃, which meets the final cooling temperature requirement, and the forging leaves the air-cooling line cooling zone.
[0033] S6. Isothermal annealing: The cooled forgings are loaded into the annealing furnace with a loading weight of 1500 kg and a loading height of 800 mm. The annealing temperature is controlled by a closed-loop thermocouple in the furnace: heated to 780 °C at a heating rate of 80 °C / h, held for 4 h, and then cooled in the furnace to 650 °C at a cooling rate of 30 °C / h, and then air-cooled after being removed from the furnace.
[0034] Example 2
[0035] This embodiment provides a high-precision temperature-controlled forming method for forging TRB bearing rings, applied to the forging of NP611293 model TRB bearing rings, specifically including the following steps.
[0036] S1. Forging and shaping: The blank is loaded into a natural gas heating furnace and heated to the initial forging temperature of 1150℃, and held for 18 minutes. After the forging press completes upsetting, punching, bottom trimming, and end face flattening, the preform is reheated to 1150℃ and held for 12 minutes. The reheated preform is then fed into a CNC radial-axial ring rolling mill for rolling and forming to obtain a ring forging.
[0037] S2. Temperature measurement point layout: Similar to Example 1, n=3, and the distance between each temperature measuring point is 1.5m.
[0038] S3. Temperature monitoring and cooling rate calculation: The measured time Δt1 for the forging to move from the first temperature measuring point to the second temperature measuring point was 12 seconds, and the measured time Δt2 for moving from the second temperature measuring point to the third temperature measuring point was also 12 seconds. The temperature values at each measuring point were: T1 = 810℃, T2 = 735℃, and T3 = 680℃. Calculations: V1=(810-735) / 12=75 / 12=6.25℃ / s; V2=(735-680) / 12=55 / 12≈4.58℃ / s.
[0039] S4. Cooling rate comparison and dynamic adjustment: V0 = 4.50℃ / s, with an allowable deviation range of 3.83℃ / s to 5.18℃ / s.
[0040] Initial state: Air supply volume 2800m³ 3 / h, rotation speed 1200r / min, V1=6.25℃ / s (too high), V2=4.58℃ / s (meets the standard).
[0041] Round 1: Only V1 is too high, so the air supply volume will be reduced from 2800m³ / h. 3 / h is reduced to 2520m in 10% increments. 3 / h, while increasing the rotational speed from 1200r / min to 1260r / min in 5% increments.
[0042] After adjustment, T1=785℃, T2=715℃, and T3=672℃. V1=(785-715) / 12≈5.83℃ / s (slightly high) V2=(715-672) / 12≈3.58℃ / s (too low); Round 2: Continue to address the high V1 level, reducing the air supply volume from 2520m³ / h. 3 / h was reduced to 2268m in 10% increments. 3 / h, while increasing the rotational speed from 1260r / min to 1323r / min in 5% increments.
[0043] After adjustment, T1=762℃, T2=695℃, and T3=668℃. V1=(762-695) / 12≈5.58℃ / s (too high). V2=(695-668) / 12=2.25℃ / s (too low).
[0044] Round 3: Increase the air supply volume from 2268m³ 3 / h increased to 2495m in 10% increments. 3 / h, while reducing the rotational speed from 1323r / min to 1257r / min in 5% increments.
[0045] After adjustment, T1=768℃, T2=700℃, and T3=670℃. V1=(768-700) / 12≈5.67℃ / s (too high). V2=(700-670) / 12=2.50℃ / s (too low).
[0046] The S3~S4 closed-loop adjustment is then continuously executed in a loop until all sections of the line V iAfter stabilizing in the range of 3.83℃ / s to 5.18℃ / s, it enters S5.
[0047] S5 cycle control until final cooling reaches the target: The S3~S4 cycle is executed continuously to monitor and control the entire cooling process of the forging. When the forging leaves the cooling zone, the final cooling temperature T3 = 680℃, which meets the final cooling temperature requirement.
[0048] S6 Isothermal Annealing: The cooled forgings are loaded into the annealing furnace with a loading weight of 1500 kg and a loading height of 800 mm. The annealing temperature is controlled by a closed-loop thermocouple in the furnace: heated to 780 °C at a heating rate of 80 °C / h, held for 4 h, and then cooled in the furnace to 650 °C at a cooling rate of 30 °C / h, and then air-cooled after being removed from the furnace.
[0049] Example 3
[0050] This embodiment provides a high-precision temperature-controlled forming method for forging TRB bearing rings, applied to the forging of NP611293 model TRB bearing rings, specifically including the following steps.
[0051] S1. Forging and shaping: The material section is loaded into a natural gas heating furnace and heated to the initial forging temperature of 1200℃, and held at that temperature for 12 minutes. After the forging press completes upsetting, punching, bottom trimming, and end face flattening, the preformed billet is reheated to 1200℃ and held at that temperature for 8 minutes. The preformed billet after the second heating is sent to a CNC radial-axial ring rolling mill for rolling and forming to obtain a ring forging.
[0052] S2. Temperature measurement point layout: Similar to Example 1, n=3, and the distance between each temperature measuring point is 1.5m.
[0053] S3. Temperature monitoring and cooling rate calculation: The measured time Δt1 for the forging to move from the first temperature measuring point to the second temperature measuring point was 12 seconds, and the measured time Δt2 for moving from the second temperature measuring point to the third temperature measuring point was also 12 seconds. The temperature values at each measuring point were: T1 = 840℃, T2 = 760℃, and T3 = 720℃. Calculations: V1=(840-760) / 12=80 / 12≈6.67℃ / s; V2=(760-720) / 12=40 / 12≈3.33℃ / s.
[0054] S4. Cooling rate comparison and dynamic adjustment: V0 = 4.50℃ / s, with an allowable deviation range of 3.83℃ / s to 5.18℃ / s.
[0055] Initial state: Air supply volume 2800m³ 3 / h, rotation speed 1200r / min, V1=6.67℃ / s (too high), V2=3.33℃ / s (slightly below the lower limit).
[0056] Round 1: Increase the air supply from 2800m³ 3 / h is reduced to 2520m in 10% increments. 3 / h, the rotational speed was increased from 1200r / min to 1260r / min in 5% increments.
[0057] After adjustment, T1=810℃, T2=740℃, and T3=710℃. V1=(810-740) / 12≈5.83℃ / s (too high). V2=(740-710) / 12=2.50℃ / s (too low); Round 2: Increase the air supply from 2520m³ 3 / h was reduced to 2268m in 10% increments. 3 / h, the rotational speed was increased from 1260r / min to 1323r / min in 5% increments.
[0058] After adjustment, T1=785℃, T2=718℃, and T3=695℃. V1=(785-718) / 12≈5.58℃ / s (slightly high) V2=(718-695) / 12≈1.92℃ / s (too low); Round 3: Increase the air supply volume from 2268m³ 3 / h increased to 2495m in 10% increments. 3 / h, the rotational speed was reduced from 1323 r / min to 1257 r / min in 5% increments.
[0059] After adjustment, T1=790℃, T2=720℃, and T3=698℃. V1=(790-720) / 12≈5.83℃ / s (slightly high). V2=(720-698) / 12≈1.83℃ / s (too low).
[0060] After three rounds of adjustments, the system enters a continuous closed-loop adjustment phase until it reaches the target and then enters S5.
[0061] S5. Circulation control until final cooling meets the standard: The S3-S4 cycle is continuously executed to monitor and control the entire cooling process of the forging. When the forging leaves the cooling zone, the final cooling temperature T3 = 720℃, which meets the final cooling temperature requirement.
[0062] S6. Isothermal annealing: The cooled forgings are loaded into the annealing furnace with a loading weight of 1500 kg and a loading height of 800 mm. The annealing temperature is controlled by a closed-loop thermocouple in the furnace: heated to 780 °C at a heating rate of 80 °C / h, held for 4 h, and then cooled in the furnace to 650 °C at a cooling rate of 30 °C / h, and then air-cooled after being removed from the furnace.
[0063] Example 4
[0064] This embodiment provides a high-precision temperature-controlled forming method for forging TRB bearing rings, applied to the forging of NP611293 model TRB bearing rings, specifically including the following steps.
[0065] S1. Forging and shaping: The blank is loaded into a natural gas heating furnace and heated to the initial forging temperature of 1160℃, and held for 16 minutes. After the forging press completes upsetting, punching, bottom trimming, and end face flattening, the preform is reheated to 1160℃ and held for 11 minutes. The preform after secondary heating is then fed into a CNC radial-axial ring rolling mill for rolling and forming to obtain a ring forging.
[0066] S2. Temperature measurement point layout: Temperature measuring points 1, 2, 3, 4, and 5 are set sequentially along the length of the air-cooling line, i.e., n=5, with a spacing of 1.0m between each measuring point. The first measuring point is set at the inlet of the air-cooling line, and the fifth measuring point is set at the outlet of the air-cooling line.
[0067] S3. Temperature monitoring and cooling rate calculation: The time it takes for the forging to move from the first temperature measuring point to the second temperature measuring point is Δt1 = 8 seconds; the time from the second to the third temperature measuring point is Δt2 = 8 seconds; the time from the third to the fourth temperature measuring point is Δt3 = 8 seconds; and the time from the fourth to the fifth temperature measuring point is Δt4 = 8 seconds. The initial temperatures at each measuring point are: T1 = 840℃, T2 = 790℃, T3 = 750℃, T4 = 720℃, and T5 = 700℃. Calculate the initial temperature change rate for each segment: V1=(840-790) / 8=50 / 8=6.25℃ / s; V2=(790-750) / 8=40 / 8=5.00℃ / s; V3=(750-720) / 8=30 / 8=3.75℃ / s; V4=(720-700) / 8=20 / 8=2.50℃ / s.
[0068] S4. Cooling rate comparison and dynamic adjustment: V0 = 4.50℃ / s, with an allowable deviation range of 3.83℃ / s to 5.18℃ / s.
[0069] Initial state: Air supply volume 2800m³3 / h, rotation speed 1200r / min, V1=6.25℃ / s (too high), V2=5.00℃ / s (meets standard), V3=3.75℃ / s (too low), V4=2.50℃ / s (too low).
[0070] Round 1: Increase the air supply from 2800m³ 3 / h is gradually reduced to 2520m in increments of 10% of the current value. 3 The rotational speed is increased from 1200 r / min to 1260 r / min in increments of 5% of the current value. After each adjustment, the temperature reading is allowed to stabilize before proceeding to the next adjustment.
[0071] After adjustment, T1=810℃, T2=760℃, T3=725℃, T4=695℃, and T5=675℃. V1=(810-760) / 8=6.25℃ / s (still too high). V2=(760-725) / 8=4.38℃ / s (meets the standard). V3=(725-695) / 8=3.75℃ / s (too low). V4 = (695-675) / 8 = 2.50℃ / s (too low).
[0072] Round 2: Continue to increase the air supply from 2520m³ 3 / h is gradually reduced to 2268m in increments of 10% of the current value. 3 / h, the speed is gradually increased from 1260r / min to 1323r / min in increments of 5% of the current value.
[0073] After adjustment, T1=785℃, T2=735℃, T3=700℃, T4=670℃, and T5=655℃. V1=(785-735) / 8=6.25℃ / s (still too high). V2=(735-700) / 8=4.38℃ / s (meets the standard). V3=(700-670) / 8=3.75℃ / s (too low). V4 = (670-655) / 8 = 1.88℃ / s (too low).
[0074] Round 3: Continue to increase the air supply volume from 2268m³ 3 / h is gradually reduced to 2041m in increments of 10% of the current value. 3 / h, the speed is gradually increased from 1323r / min to 1389r / min in increments of 5% of the current value.
[0075] After adjustment, T1=765℃, T2=715℃, T3=685℃, T4=660℃, and T5=648℃. V1=(765-715) / 8=6.25℃ / s (too high). V2=(715-685) / 8=3.75℃ / s (too low). V3=(685-660) / 8=3.13℃ / s (too low). V4 = (660-648) / 8 = 1.50℃ / s (too low).
[0076] After three rounds of adjustments, the system enters a continuous closed-loop adjustment phase until it reaches the target and then enters S5.
[0077] S5. Circulation control until final cooling meets the standard: The S3-S4 cycle is continuously executed to monitor and control the entire cooling process of the forging. When the forging leaves the cooling zone, the final cooling temperature T5 = 650℃, which meets the final cooling temperature requirement.
[0078] S6. Isothermal annealing: The cooled forgings are loaded into the annealing furnace with a loading weight of 1500 kg and a loading height of 800 mm. The annealing temperature is controlled by a closed-loop thermocouple in the furnace: heated to 780 °C at a heating rate of 80 °C / h, held for 4 h, and then cooled in the furnace to 650 °C at a cooling rate of 30 °C / h, and then air-cooled after being removed from the furnace.
[0079] Comparative Example 1 (adjusting only air volume, not speed) The difference between this comparative example and Example 1 is that in S4, only the air supply volume is adjusted (adjusted step by step in 10% increments), and the speed of the drive motor remains constant at 1200 r / min throughout the entire process, without being adjusted synchronously with the air supply volume.
[0080] The initial state is the same as in Example 1: air supply volume 2800m³ 3 / h, rotation speed 1200r / min, T1=820℃, T2=740℃, T3=700℃, V1=6.67℃ / s, V2=3.33℃ / s.
[0081] Round 1: Only V1 is slightly high, air supply volume increased from 2800m³ / h 3 / h decreased to 2520m 3 / h, rotation speed remains unchanged at 1200 r / min. After adjustment, V1 = 4.33℃ / s (meets standard), V2 = 3.33℃ / s (too low); Round 2: V2 is too low, air supply volume reduced from 2520m³ / h 3 / h increased to 2772m 3 / h, rotational speed remains constant. After adjustment, V1 = 4.67℃ / s (meets standard), V2 = 3.83℃ / s (meets standard); Round 3: Continue to increase the air supply to 3049m³. 3 / h, rotational speed remains constant. After adjustment, V1 = 4.75℃ / s (meets standard), V2 = 4.17℃ / s (meets standard), but T1, T2, and T3 all continue to increase overall; Round 4: Maintain air supply at 3049m³ 3 The speed and rotational speed remain unchanged at 1200 r / min; monitoring continues.
[0082] T1=818℃, T2=762℃, T3=708℃, V1 = 4.67℃ / s (compliant), V2 = 4.50℃ / s (compliant), but the overall temperature continues to rise by about 8~10℃ compared to the initial state, and the final cooling temperature T3 is close to 710℃, with a clear upward trend. Because the conveying speed is constant, adjusting the air supply alone cannot maintain a stable temperature distribution throughout the entire process during long-term operation.
[0083] Comparative Example 2 (fixed parameters, no adjustment) The difference between this comparative example and Example 1 is that step S4 is omitted, there is no dynamic adjustment, and the air supply volume and speed remain fixed throughout the process.
[0084] Initial settings: Air supply volume 3000m³ 3 / h, rotation speed 1200r / min (fixed throughout).
[0085] After the forgings enter the air-cooling line, the temperatures are T1=820℃, T2=740℃, and T3=700℃. V1=(820-740) / 12=6.67℃ / s (higher than the upper limit of 5.18℃). V2=(740-700) / 12=3.33℃ / s (below the lower limit of 3.83℃).
[0086] Continue collecting data: T1=810℃, T2=725℃, T3=678℃. V1=(810-725) / 12=7.08℃ / s (still higher than the upper limit). V2=(725-678) / 12=3.92℃ / s (meets the standard).
[0087] Continue collecting temperatures: T1=800℃, T2=710℃, T3=660℃. V1=(800-710) / 12=7.50℃ / s (continuously high). V2=(710-660) / 12=4.17℃ / s (meets the standard).
[0088] Throughout the cooling process, V1 consistently failed to reach the target range of 3.83~5.18℃ / s, and V1 remained consistently high, indicating that the fixed parameter scheme could not cope with the actual temperature changes of the forging during the cooling process.
[0089] Performance testing The performance of the forgings obtained in each embodiment and comparative example was tested. The test items included: Hardness testing: A Brinell hardness tester with a load of 187.5 kg and a steel ball diameter of 2.5 mm was used. Six measuring points were evenly distributed around the circumference of the forging. The average hardness and range (the difference between the maximum and minimum values) were calculated to evaluate the uniformity of hardness.
[0090] Metallographic structure testing: Samples were taken from the same cross section of the forging, and after grinding, polishing, and etching with 4% nitric acid alcohol solution, the microstructure was observed using an optical microscope, and the spheroidization level was evaluated in accordance with the SEP 1520 standard.
[0091] Ultrasonic flaw detection: Each forging is 100% inspected using an ultrasonic flaw detector, and the pass rate is recorded.
[0092] The test results are shown in Table 1:
[0093] Table 1 The test results show that the hardness range of each embodiment was controlled within 9 HB to 11 HB, the spheroidization level was 2 to 3, and the ultrasonic flaw detection pass rate was above 97.2%. All performance indicators were significantly better than the two comparative examples. Comparative Example 1, due to its constant conveying speed, could not maintain long-term stability of the temperature distribution throughout the process by simply adjusting the air supply volume. The hardness range widened to 30 HB, the spheroidization level coarsened to 4, and the ultrasonic flaw detection pass rate dropped to 86.5%. Comparative Example 2, due to the lack of any dynamic adjustment throughout the process, resulted in a completely uncontrolled cooling process for the forgings. The hardness range reached 38 HB, and coarse pearlite and localized bainite appeared in the microstructure. The ultrasonic flaw detection pass rate was only 78.8%. These results demonstrate that the closed-loop control method of this invention, which sets multiple temperature measurement points in the air-cooling line, calculates the cooling rate of each section in real time, and synchronously adjusts the air supply volume and conveying speed step by step, can effectively improve the hardness uniformity, metallographic quality, and internal density of forgings, and the ultrasonic flaw detection pass rate is significantly higher than that of traditional methods.
[0094] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it.
Claims
1. A high-precision TRB bearing ring forging temperature-controlled forming method, characterized in that, Includes the following steps: S1. Forging: The billet is heated to the forging temperature and then forged into a ring forging. S2. Temperature measurement point layout: The annular forging is sent into the cooling zone, and the first temperature measurement point, the second temperature measurement point, ..., the nth temperature measurement point are set sequentially along the length of the cooling zone, where n≥3, and the temperature measurement points are distributed at equal intervals. S3, temperature monitoring and cooling rate calculation: real-time acquisition of temperature values T1, T2,..., Tn of each temperature measurement point n , calculation of the temperature change rate V between adjacent temperature measurement points i = (T i -T i+1 ) / Δt, where Δt is the time for the forging to move from the ith temperature measurement point to the i+1th temperature measurement point; S4. Cooling rate comparison and dynamic adjustment: The measured temperature change rate V of each segment is compared and adjusted. i Compare with the preset target temperature change rate V0; When V i When V > V0, simultaneously reduce the cooling intensity of the cooling zone and increase the forging conveyor speed, so that V i It falls back to within the allowable deviation range of V0; When V i When V < V0, simultaneously increase the cooling intensity of the cooling zone and reduce the forging conveyor speed, so that V i Rise to within the allowable deviation range of V0; When V i When within the allowable deviation range of V0, maintain the current cooling intensity and conveying speed unchanged; S5. Cyclic control until final cooling reaches the target temperature: Repeat S3~S4 until the final cooling temperature reaches the target temperature when the forging leaves the cooling zone.
2. The high-precision TRB bearing ring forging temperature-controlled forming method according to claim 1, characterized in that, The cooling zone is an air-cooled line, and the cooling intensity is achieved by adjusting the air supply volume of the air-cooled line. The forging conveying speed is achieved by adjusting the speed of the drive motor of the air-cooled line.
3. The high-precision TRB bearing ring forging temperature-controlled forming method according to claim 1, characterized in that, In step S4, simultaneously reducing the cooling intensity of the cooling zone and increasing the forging conveying speed means: gradually reducing the air supply volume in increments of 10% of the current air supply volume, while gradually increasing the rotation speed in increments of 5% of the current rotation speed, and proceeding to the next level after the temperature reading stabilizes after each adjustment. The simultaneous increase in cooling intensity of the cooling zone and reduction in forging conveying speed refers to: gradually increasing the air supply volume in increments of 10% of the current air supply volume, while gradually decreasing the rotation speed in increments of 5% of the current rotation speed, and proceeding to the next level after the temperature reading stabilizes at each adjustment.
4. The high-precision TRB bearing ring forging temperature-controlled forming method according to claim 1, characterized in that, In step S4, the allowable deviation range is ±15% of V0.
5. The high-precision TRB bearing ring forging temperature-controlled forming method according to claim 1, characterized in that, In step S5, the target temperature is 650℃~720℃.
6. The high-precision TRB bearing ring forging temperature-controlled forming method according to claim 1, characterized in that, In step S1, the step of heating the billet to the forging temperature and then forging it into a ring forging specifically includes: S1-1 Primary heating and preforming: The bearing steel section is heated to the initial forging temperature, and then upsetting, punching, bottom cutting and flattening are performed to form a preform. S1-2 Secondary heating: The preformed billet is reheated to the same initial forging temperature; S1-3 Rolling and Expanding Final Forming: The preformed billet after secondary heating is fed into a CNC radial and axial rolling mill for rolling and expanding to obtain a ring forging.
7. The high-precision TRB bearing ring forging temperature-controlled forming method according to claim 1, characterized in that, The initial forging temperature mentioned in S1-1 and S1-2 is 1150℃~1200℃.
8. The high-precision TRB bearing ring forging temperature-controlled forming method according to claim 1, characterized in that, Step S5 is followed by: S6. Isothermal Annealing: The cooled forgings are loaded into an annealing furnace for isothermal annealing. The annealing temperature is controlled by a closed-loop thermocouple in the furnace. After annealing, the hardness and metallographic structure of the forgings are tested.