A low porosity lost foam casting process

By employing technologies such as EPS foam bead gradient drying, double-layer coating, full-process negative pressure pouring, and segmented cooling in the lost foam casting process, the problems of high porosity and poor microstructure uniformity in castings have been solved, resulting in castings with low porosity and excellent mechanical properties, which are suitable for intelligent welding and casting integrated manufacturing.

CN123149362APending Publication Date: 2026-11-24HUNAN HECHUANG MASCH CASTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611420833.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the existing lost foam casting process, the castings have high porosity and poor microstructure uniformity, which makes it difficult to meet the requirements of intelligent welding and casting integrated manufacturing for casting density and weldability. This results in a high scrap rate and restricts the promotion and application of high-end equipment components.

Method used

EPS foam beads are used to prepare foam patterns and perform gradient drying. Double-layer composite refractory coating is applied, and the process is combined with full negative pressure pouring, layered sand filling and compaction and segmented cooling. With the help of silicon-barium-calcium composite inoculant and electromagnetic stirring, gas can be discharged in time and graphite can be evenly distributed, reducing porosity and improving the density and mechanical properties of the casting.

Benefits of technology

It significantly reduces the porosity of castings to ≤1%, has excellent graphite morphology and high pearlite content, resulting in excellent mechanical properties of castings. It is suitable for intelligent welding processing, reduces the scrap rate of castings, and meets the quality requirements of high-end equipment components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149362A_ABST
    Figure CN123149362A_ABST
Patent Text Reader

Abstract

This invention provides a low-porosity lost foam casting process, comprising: pre-foaming and steam foaming of EPS foam beads to obtain a foam pattern; gradient drying to a moisture content ≤0.2% and coating with a double-layer composite refractory coating; mixing new and recycled quartz sand to obtain binder-free dry sand; layering sand filling and applying negative pressure vibration compaction after pattern assembly; adding a silicon-barium-calcium composite inoculant and refining with electromagnetic stirring to obtain molten iron; bottom-pouring uniform pouring under full negative pressure conditions and heat preservation riser feeding; segmented cooling and solidification after pouring; sand removal, shot blasting, and low-temperature aging treatment. This invention, through the synergistic effect of gradient drying, double-layer composite coating, negative pressure compaction and negative pressure pouring, composite inoculation, and segmented cooling, achieves a casting porosity ≤1%, excellent graphite morphology, significantly improved tensile strength and hardness, and high density and good weldability, making it suitable for the production of intelligent welded casting integrated components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of casting technology, and in particular to a lost foam casting process with low porosity, which is especially suitable for the preparation of gray cast iron parts for intelligent welded casting integrated components. Background Technology

[0002] Lost foam casting, also known as solid casting or EPC process, is a casting method that uses foam plastic to make a pattern, coats the surface of the pattern with refractory coating, and then embeds it in dry sand to form a shape. When molten metal is poured in, the foam pattern is heated and vaporized, and the molten metal fills the mold and solidifies to obtain the casting. It has the advantages of high dimensional accuracy, short production cycle and smooth surface of castings, and is widely used in the production of gray cast iron parts.

[0003] However, during lost foam casting, the foam pattern vaporizes and decomposes under the high temperature of the molten metal, generating a large amount of gas. If this gas cannot be discharged from the sand mold in a timely and sufficient manner, it will be drawn into the molten metal or remain inside the casting, leading to defects such as porosity, inclusions, and cold shuts, severely affecting the density and mechanical properties of the casting. In existing lost foam casting processes, the main sources of porosity include: vaporization of residual moisture in the foam pattern during pouring; insufficient permeability of the coating layer, making it difficult for decomposed gases to escape; turbulent flow of the molten metal during pouring, resulting in air inclusions; and insufficient local negative pressure and poor gas discharge due to loose filling of the molding sand.

[0004] Meanwhile, conventional inoculation treatments can easily lead to graphite morphology deterioration, insufficient pearlite content in the matrix, and substandard mechanical properties of the castings. An unreasonable cooling regime can increase residual stress in the castings, making them prone to cracking and dimensional deviations. Most existing technologies only optimize a single stage, lacking a synergistic solution across the entire process. They cannot simultaneously achieve low porosity, good microstructure, and low residual stress, resulting in a high scrap rate and failing to meet the demands of intelligent integrated welding and casting manufacturing for high-quality gray cast iron castings. This hinders the further promotion and application of lost foam casting technology in high-end equipment components. Summary of the Invention

[0005] In view of this, the present invention proposes a low-porosity lost foam casting process, which aims to solve the problems of high porosity, poor microstructure uniformity, and difficulty in meeting the requirements of intelligent welding and casting integrated manufacturing for casting density and weldability.

[0006] The technical solution of this invention is achieved as follows: a lost foam casting process with low porosity. S1. Preparation of foam pattern: Select EPS foam beads and pre-foam, steam foaming to form foam pattern. Dry the pattern to a moisture content of ≤0.2%. Then, apply composite refractory coating to the surface of the pattern in multiple coats to form a coating. S2. Molding sand preparation and sand box pretreatment: Mix new quartz sand with recycled quartz sand to obtain binder-free dry sand, clean the sand box and spray an anti-stick coating on its inner wall and then preheat it. S3. Pattern assembly and sand compaction: Fix the dried pattern in the sand box and reserve an exhaust channel. Fill the sand box with the dry sand in layers, vibrate and apply negative pressure while filling the sand to make the molding sand compact. S4. Metal molten metal smelting and refining: Smelt according to the batch and refine with the addition of a composite inoculant to obtain molten iron; S5. Negative pressure casting: Under the condition of maintaining negative pressure throughout the process, the molten iron is poured at a uniform speed using a bottom pouring method, and the heat-insulating riser is used to continuously feed the iron. S6. Segmented cooling and solidification: After casting is completed, natural cooling is carried out first, followed by forced air cooling. The negative pressure is released after the casting drops to the specified temperature. S7. Shaking and post-treatment: Vibration shake-off separates the casting from the molding sand. After shot blasting, the casting is subjected to low-temperature aging treatment to obtain castings with low porosity.

[0007] Furthermore, the EPS foam beads have a particle size of 0.3~0.6mm and a pre-expansion density controlled at 18~22kg / m³. 3 The steam pressure for steam foaming molding is 0.12~0.15MPa, and the molding heat preservation time is 30~45s.

[0008] Furthermore, in step S1, the drying adopts a gradient drying method: the sample is placed in a constant temperature drying room, and preheated slowly at 30~40℃ for 2~3 hours, and then heated to 45~55℃ and kept at that temperature for 12~16 hours, so that the moisture content of the sample is ≤0.2%.

[0009] Further, in step S1, the composite refractory coating is a two-layer composite coating, including a top layer coating and a back layer coating; the top layer coating, by weight, includes: 70-80 parts zircon powder, 8-12 parts silica sol, 1-3 parts bentonite, 0.05-0.1 parts surfactant, and water to make up to 100 parts; the back layer coating, by weight, includes: 55-65 parts quartz powder, 3-5 parts white latex, 4-6 parts water glass, 2-4 parts sepiolite, 3-5 parts graphite powder, and water to make up to 100 parts. The zircon powder has a particle size of 320 mesh, and the quartz powder has a particle size of 100-150 mesh. The coating is applied in three coats, with each coat air-dried or oven-dried for at least 5 hours after application. The final total coating thickness is 0.8-1.2 mm, and the coating's air permeability is 2-5 cm. 3 / (cm 2 (·min·kPa); Further, in step S2, the mass ratio of the new quartz sand to the recycled quartz sand is 3:(6~8), and the sand particle size is 50~70 mesh; the sand temperature is controlled at 25~35℃ during sand mixing, and the sand box is preheated to 30~40℃.

[0010] Furthermore, in step S3, the thickness of each layer of sand is 150~200mm when filling in layers; the vibration compaction adopts a vibration frequency of 25~30Hz and a vibration duration of 15~20s, and the vacuum degree is maintained at -0.07~-0.09MPa during the compaction process.

[0011] Further, in step S4, the ingredients, by mass percentage, are: 45% pig iron, 20% scrap steel, and 35% recycled material; smelting is carried out using a medium-frequency induction furnace, with the temperature raised to 1500~1540℃ and held for 8~12 minutes; during refining, a composite inoculant, accounting for 0.3%~0.5% of the total mass of the molten iron, is added. The composite inoculant is a silicon-barium-calcium composite inoculant, comprising by mass percentage: 65~72% silicon, 2~4% barium, 1~2% calcium, 1~2% aluminum, with the balance being iron; after addition, the mixture is electromagnetically stirred for 3~5 minutes, and after removing the slag, the molten iron is allowed to stand for 5 minutes.

[0012] Furthermore, in step S5, the pouring temperature is 1420~1460℃, the pouring speed is 4~6kg / s, and the pressure is maintained at -0.07~-0.09MPa throughout the process; after pouring, the pressure is maintained at negative pressure for 30 minutes for shrinkage compensation.

[0013] Further, in step S6, the segmented cooling is specifically as follows: First cooling, the sand box is naturally cooled for 90~120 minutes to reduce the casting temperature to 750~800℃; Second cooling, the air cooling system is turned on with a wind speed of 3~4m / s to cool to below 300℃; The negative pressure system is turned off when the casting temperature drops to below 200℃.

[0014] Furthermore, in step S7, the shot blasting is performed using a tracked shot blasting machine with a steel shot particle size of 1.0 mm and a processing time of 8-12 minutes; the low-temperature aging treatment is performed at a temperature of 520-560℃, and the temperature is maintained for 3.5-4.5 hours before being cooled in the furnace to eliminate casting internal stress.

[0015] Compared with the prior art, the beneficial effects of the present invention are: This invention controls the moisture content of the foam pattern to ≤0.2% through gradient drying and applies a double-layer composite refractory coating consisting of a surface layer of fine-grained zircon powder and a back layer of coarse-grained quartz powder. Combined with full-process negative pressure pouring, this ensures that the gas generated by the vaporization and decomposition of the foam pattern is promptly and fully discharged from the sand mold, significantly reducing the porosity of the casting to ≤1% from the source. The use of a high proportion of recycled sand significantly reduces raw material costs while maintaining the performance of the molding sand, achieving sand recycling. Layered sand filling and negative pressure synergistic compaction ensure dense filling of the molding sand and uniform negative pressure within the sand box, preventing casting collapse and deformation while ensuring unobstructed ventilation channels in the molding sand. A silicon-barium-calcium composite inoculant, combined with electromagnetic stirring refining, refines graphite, promotes uniform graphite distribution, increases pearlite content, and enhances the tensile strength and hardness of the casting. Bottom-pouring uniform speed pouring combined with full-process negative pressure ensures stable metal filling and orderly vaporization of the foam pattern, avoiding turbulent flow and gas inclusions, and completely resolving slag inclusions and porosity defects. Segmented gradient cooling prevents internal stress and cracks in the casting. The above-mentioned technical features work together synergistically to produce castings with a porosity of ≤1%, excellent graphite morphology, superior mechanical properties, and dense structure. This provides an excellent base material for subsequent welding processing, which helps to reduce welding porosity, improve the quality of welded joints, and meet the needs of intelligent integrated welding and casting production. Attached Figure Description

[0016] Figure 1 The graphite morphology diagram of the casting obtained in Example 1 of the present invention is shown on the left. The left side is a metallographic micrograph of the casting sample, and the right side is a schematic diagram of the standard type A graphite. The magnification of both is 100x. Figure 2 The image shows a metallographic micrograph of the matrix structure of the low-porosity casting prepared in Example 1 of this invention. Detailed Implementation

[0017] To better understand the technical content of this invention, specific embodiments are provided below to further illustrate the invention.

[0018] Unless otherwise specified, the experimental methods used in the embodiments of this invention are all conventional methods.

[0019] Unless otherwise specified, all materials and reagents used in the embodiments of this invention are commercially available.

[0020] Example 1 This embodiment provides a low-porosity lost foam casting process for gray cast iron parts. The specific steps are as follows: S1. Foam pattern preparation and pretreatment (1) Raw materials: EPS foam beads with a particle size of 0.4 mm and a pre-expansion density controlled at 20 kg / m³. 3 .

[0021] (2) Molding: The pre-foamed beads are filled into the mold and steam foaming is used for molding. The steam pressure is 0.13MPa and the molding heat preservation time is 40s to obtain the foam pattern.

[0022] (3) Drying: The pattern is dried in a gradient. First, it is preheated at 35℃ for 2.5h, and then heated to 50℃ and kept for 14h to reduce the moisture content of the pattern to 0.15%.

[0023] (4) Dipping and Coating: A composite refractory coating is applied to the surface of the pattern using a two-layer composite coating. The top layer coating, by weight, includes 75 parts zircon powder (320 mesh), 10 parts silica sol, 2 parts bentonite, 0.08 parts surfactant, and water to make up to 100 parts. The back layer coating, by weight, includes 60 parts quartz powder (120 mesh), 4 parts white latex, 5 parts water glass, 3 parts sepiolite, 4 parts graphite powder, and water to make up to 100 parts. The coating is applied in three coats, each coat air-dried for 6 hours. The final total coating thickness is 1.0 mm, and the air permeability of the coating, measured using an air permeability tester, is 3.5 cm. 3 / (cm 2 (·min·kPa).

[0024] S2. Molding Sand Preparation and Sand Box Pretreatment (1) Sand: The mass ratio of new quartz sand to recycled quartz sand is 3:7, and the sand particle size is 60 mesh.

[0025] (2) Sand mixing: Dry sand without binder is mixed, and the sand temperature is controlled at 30℃.

[0026] (3) Sand box: Clean the sand box, spray the inner wall with an anti-stick coating, and preheat to 35℃.

[0027] S3, the pattern box and sand filling are compacted. (1) Assembly: Fix the dried pattern in the sand box according to the layout, and reserve a special exhaust channel.

[0028] (2) Sand filling: Sand is filled in layers, with each layer being 180mm thick.

[0029] (3) Compacting: The vibration table is used for compaction. The vibration frequency is 28Hz and the vibration duration is 18s. The pressure is maintained at -0.08MPa during the compaction process.

[0030] S4. Melting and Refining of Molten Metal (1) Ingredients: 45% pig iron, 20% scrap steel, 35% recycled material, supplemented with ferrosilicon and ferromanganese alloys to finely adjust the composition.

[0031] (2) Melting: Melt in a medium frequency induction furnace, heat to 1520℃ and hold for 10 minutes.

[0032] (3) Refining: Add 0.4% of silicon-barium-calcium composite inoculant, which by mass percentage includes 68% silicon, 3% barium, 1.5% calcium, 1.5% aluminum, and the balance is iron; stir electromagnetically for 4 minutes, remove slag, and let the molten iron stand for 5 minutes.

[0033] S5, Negative Pressure Casting (1) Temperature measurement: The temperature is remeasured after the furnace is removed, and the pouring temperature is controlled at 1440℃.

[0034] (2) Pouring: Bottom pouring uniform speed is adopted, with a pouring speed of 5kg / s and a pressure of -0.08MPa throughout the process.

[0035] (3) Feeding: Continuous feeding is carried out using the insulation riser, and the pressure is maintained at negative pressure for 30 minutes after the casting is completed.

[0036] S6, Segmented cooling and solidification (1) First cooling: After the casting is completed, the sand box is naturally cooled for 100 minutes, and the casting temperature drops to 780℃.

[0037] (2) Secondary cooling: Turn on the air cooling system, with a wind speed of 3.5m / s, and cool to 280℃.

[0038] (3) Release the negative pressure: When the temperature drops to 180℃, turn off the negative pressure system.

[0039] S7. Sand Removal and Post-treatment Vibration is used to remove the sand, with a vibration duration of 22 seconds, separating the casting from the molding sand. Intact castings are sorted, and waste sand is sent to a sand recycling system for processing and reuse. The casting is then fed into a crawler-type shot blasting machine with 1.0mm steel shot for 10 minutes to remove surface oxide scale and adhering sand. Subsequently, a low-temperature aging treatment is performed at 540℃ for 4 hours, followed by furnace cooling to eliminate casting internal stress and obtain the finished casting.

[0040] The products undergo visual inspection, dimensional accuracy testing, magnetic particle testing, and mechanical property testing in sequence. Once all indicators meet the standards, they are put into storage.

[0041] Example 2 The difference between this embodiment and Embodiment 1 is that: In step S1, the EPS foam beads have a particle size of 0.3 mm and a pre-expansion density of 18 kg / m³. 3 Steam foaming molding was performed at a steam pressure of 0.12 MPa for 45 seconds. Drying involved preheating at 30°C for 3 hours, followed by heating to 55°C and holding for 12 hours. The topcoat consisted of 70 parts zircon powder and 12 parts silica sol, with the rest being the same. The backcoat consisted of 55 parts quartz powder, 6 parts water glass, and 2 parts sepiolite, with the rest being the same. The final coating thickness was 0.8 mm, and the measured air permeability was 2.0 cm. 3 / (cm 2 (·min·kPa).

[0042] In step S3, each layer of sand is 150mm thick, the vibration frequency is 25Hz, the vibration duration is 20s, and the pressure is -0.09MPa.

[0043] In step S5, the pouring temperature is 1420℃, the pouring speed is 4kg / s, and the pressure is -0.09MPa.

[0044] In step S6, the first cooling process takes 120 minutes to reach 750°C, the second cooling process takes 3 m / s to reach 250°C, and the negative pressure is turned off at 200°C.

[0045] The remaining steps are the same as in Example 1.

[0046] Example 3 The difference between this embodiment and Embodiment 1 is that: In step S1, the EPS foam beads have a particle size of 0.6 mm and a pre-expansion density of 22 kg / m³. 3 Steam foaming molding: steam pressure 0.15 MPa, holding time 30 s; drying: preheating at 40℃ for 2 hours, then raising the temperature to 45℃ and holding for 16 hours; the topcoat contains 80 parts zircon powder and 8 parts silica sol, the rest are the same; the backcoat contains 65 parts quartz powder, 4 parts water glass, and 4 parts sepiolite, the rest are the same; the final coating thickness is 1.2 mm, and the air permeability is 5.0 cm. 3 / (cm 2 (·min·kPa).

[0047] In step S3, each layer of sand is 200mm thick, the vibration frequency is 30Hz, the vibration duration is 15s, and the pressure is -0.07MPa.

[0048] In step S5, the pouring temperature is 1460℃, the pouring speed is 6kg / s, and the pressure is -0.07MPa.

[0049] In step S6, the first cooling process takes 90 minutes to reach 800°C, and the second cooling process takes 4 m / s to reach 300°C.

[0050] The remaining steps are the same as in Example 1.

[0051] Comparative Example 1 The difference between this comparative example and Example 1 is that it employs the industry-standard lost foam casting process: the foam pattern is dried at a constant temperature (50℃ for 14 hours), resulting in a pattern moisture content of 0.52%; a single-component quartz powder refractory coating is applied, with a coating thickness of 1.0 mm; all molding sand is new quartz sand, filled in once and then compacted by vibration; ordinary 75% ferrosilicon is used for inoculation, without electromagnetic stirring; and the entire process is naturally cooled after casting, without low-temperature aging treatment. The measured air permeability of the coating is only 0.4 cm. 3 / (cm 2 (·min·kPa).

[0052] Comparative Example 2 The difference between this comparative example and Example 1 is that a conventional single-layer refractory coating with quartz powder as aggregate was used, applied in three coats with a total thickness of 1.0 mm; the remaining procedures and parameters were the same as in Example 1. The measured air permeability of the coating was only 0.5 cm. 3 / (cm 2 (·min·kPa).

[0053] Comparative Example 3 The difference between this comparative example and Example 1 is that the gradient drying process is omitted, and the foam pattern is directly placed in a 50°C constant temperature drying room for 14 hours. After drying, the moisture content of the pattern is 0.46%. The remaining processes and parameters are the same as in Example 1.

[0054] Comparative Example 4 The difference between this comparative example and Example 1 is that no negative pressure was applied during casting; atmospheric pressure casting was used, while the other conditions remained the same.

[0055] Comparative Example 5 The difference between this comparative example and Example 1 is that the segmented cooling process is eliminated, the negative pressure is maintained for 30 minutes after casting, and then the negative pressure is released by natural cooling to below 200°C. No secondary forced air cooling is performed, and the other conditions are the same.

[0056] Comparative Example 6 The difference between this comparative example and Example 1 is that the silicon-barium-calcium composite inoculant and electromagnetic stirring refining are omitted. Only 0.4% of ordinary 75 ferrosilicon inoculant by mass of molten iron is added, and the mixture is manually stirred and then allowed to stand after slag removal. The remaining processes and parameters are the same as in Example 1.

[0057] Effect verification 1. Preparation of test samples HT300 gray cast iron box castings of the same specifications as in Example 1 were selected as test objects. They were mass-produced using the processes of Examples 1-3 and Comparative Examples 1-6, with 50 castings prepared in each group. The structural dimensions, raw material batches, and production equipment of all castings were kept consistent. Samples were taken from the same position on the casting body for performance testing to ensure that the test variables were unique and the results were comparable.

[0058] 2. Testing Methods All samples were taken from castings of the same batch and specifications, and performance tests were conducted in accordance with the corresponding national standards. (1) Porosity: The density method was used to determine the porosity, calculated as porosity = (theoretical density - measured density) / theoretical density × 100%; (2) Coating air permeability: The air permeability of the coating sample under a specified pressure difference was measured using an air permeability tester, and the unit is cm. 3 / (cm2 (·min·kPa); (3) Graphite morphology: Metallographic specimens were prepared according to GB / T 7216, and the graphite morphology grade was observed and evaluated using an optical microscope; (4) Pearlite content: The percentage of pearlite area was determined by image analysis according to GB / T 7216; (5) Mechanical strength: The single-cast test bar was cast in accordance with GB / T 9439-2023 and the test bar was heat-treated in the same furnace as the casting; the single-cast test bar was machined into standard tensile test specimens and the room temperature tensile strength was determined in accordance with GB / T 228.1-2021; the Brinell hardness was tested in accordance with GB / T 231.1-2018. (6) Internal defects: Magnetic particle testing is used to detect microcracks inside the casting.

[0059] 3. Performance Comparison Results

[0060] The castings in Examples 1-3 were free of porosity and cracks and were of qualified quality. The castings in Comparative Examples 1-4 had more porosity and decreased mechanical properties. The castings in Comparative Example 5 had high internal residual stress and microcracks were detected. The castings in Comparative Example 6 had coarse graphite and low mechanical properties.

[0061] 4. Results Analysis The performance comparison results show that the porosity of the embodiments of the present invention is ≤1%, the graphite morphology is excellent, the pearlite content and tensile strength are significantly improved, and the residual stress is greatly reduced. This confirms that the present invention achieves synergistic optimization throughout the entire process, effectively solving the problems of high porosity, poor microstructure, and high internal stress in lost foam castings. Among them, the porosity of the castings obtained by Examples 1 to 3 is 0.65% to 0.89%, all less than 1%; while the porosity of Comparative Example 1, which uses industry-standard processes, is as high as 2.45%, Comparative Example 4 has a porosity of 2.18%, Comparative Example 2 has a porosity of 1.82%, and Comparative Example 3 has a porosity of 1.65%, all significantly higher than the examples. This indicates that full-process negative pressure casting, double-layer composite coating, and gradient drying are the key features for reducing porosity. In Examples 1-3, the graphite morphology was all type A, with a uniform distribution and a pearlite content of 92%-95%. In contrast, the graphite morphology in Comparative Examples 1 and 6 was a mixture of type A and type B, with an uneven distribution and a pearlite content reduced to 82% and 84%, respectively. This indicates that the silicon-barium-calcium composite inoculant combined with electromagnetic stirring refining can effectively refine graphite, promote uniform graphite distribution, and increase pearlite content.

[0062] Examples 1-3 exhibit tensile strengths of 305-322 MPa and Brinell hardness of 202-215 HBW, significantly higher than Comparative Examples 1, 4, and 6. Comparative Example 6, due to the elimination of composite inoculation and electromagnetic stirring, saw a reduction in pearlite content to 84%, resulting in a significant decrease in tensile strength and hardness, further validating the crucial role of composite inoculation and electromagnetic stirring in improving mechanical properties. Comparative Example 5, after eliminating segmented cooling, maintained porosity and mechanical properties comparable to the examples; however, segmented gradient cooling effectively prevented internal stress and cracks in the casting, playing a vital role in ensuring the overall quality of the casting.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A lost foam casting process with low porosity, characterized in that, Includes the following steps: S1. Preparation of foam pattern: Select EPS foam beads and pre-foam, steam foaming to form foam pattern. Dry the pattern to a moisture content of ≤0.2%. Then, apply composite refractory coating to the surface of the pattern in multiple coats to form a coating. S2. Molding sand preparation and sand box pretreatment: Mix new quartz sand with recycled quartz sand to obtain binder-free dry sand, clean the sand box and spray an anti-stick coating on its inner wall and then preheat it. S3. Pattern assembly and sand compaction: Fix the dried pattern in the sand box and reserve an exhaust channel. Fill the sand box with the dry sand in layers, vibrate and apply negative pressure while filling the sand to make the molding sand compact. S4. Metal molten metal smelting and refining: Smelt according to the batch and refine with the addition of a composite inoculant to obtain molten iron; S5. Negative pressure casting: Under the condition of maintaining negative pressure throughout the process, the molten iron is poured at a uniform speed using a bottom pouring method, and the heat-insulating riser is used to continuously feed the iron. S6. Segmented cooling and solidification: After casting is completed, natural cooling is carried out first, followed by forced air cooling. The negative pressure is released after the casting drops to the specified temperature. S7. Shaking and post-treatment: Vibration shake-off separates the casting from the molding sand. After shot blasting, the casting is subjected to low-temperature aging treatment to obtain castings with low porosity.

2. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S1, the EPS foam beads have a particle size of 0.3~0.6mm and a pre-expansion density controlled at 18~22kg / m³. 3 The steam pressure for steam foaming molding is 0.12~0.15MPa, and the molding heat preservation time is 30~45s.

3. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S1, the drying adopts a gradient drying method: the sample is placed in a constant temperature drying room, and preheated slowly at 30~40℃ for 2~3 hours, and then heated to 45~55℃ and kept at that temperature for 12~16 hours, so that the moisture content of the sample is ≤0.2%.

4. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S1, the composite refractory coating is a two-layer composite coating, including a top layer coating and a back layer coating; The topcoat, by weight, comprises: 70-80 parts zircon powder, 8-12 parts silica sol, 1-3 parts bentonite, 0.05-0.1 parts surfactant, and water to make up to 100 parts; the backcoat, by weight, comprises: 55-65 parts quartz powder, 3-5 parts white latex, 4-6 parts water glass, 2-4 parts sepiolite, 3-5 parts graphite powder, and water to make up to 100 parts; the zircon powder has a particle size of 320 mesh, and the quartz powder has a particle size of 100-150 mesh; the coating is applied in 3 coats, and each coat is allowed to air dry or baked for at least 5 hours after application, resulting in a final total coating thickness of 0.8-1.2 mm.

5. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S2, the mass ratio of new quartz sand to recycled quartz sand is 3:(6~8), and the sand particle size is 50~70 mesh; the sand temperature is controlled at 25~35℃ during sand mixing, and the sand box is preheated to 30~40℃.

6. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S3, the thickness of each layer of sand is 150~200mm when filling in layers; the vibration compaction adopts a vibration frequency of 25~30Hz and a vibration duration of 15~20s, and the pressure is maintained at -0.07~-0.09MPa during the compaction process.

7. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S4, the ingredients, by mass percentage, are: 45% pig iron, 20% scrap steel, and 35% recycled material; smelting is carried out using a medium-frequency induction furnace, with the temperature raised to 1500~1540℃ and held for 8~12 minutes; during refining, a composite inoculant, accounting for 0.3%~0.5% of the total mass of the molten iron, is added. The composite inoculant is a silicon-barium-calcium composite inoculant, comprising by mass percentage: 65~72% silicon, 2~4% barium, 1~2% calcium, 1~2% aluminum, with the balance being iron; after addition, the mixture is electromagnetically stirred for 3~5 minutes, and after removing the slag, the molten iron is allowed to stand for 5 minutes.

8. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S5, the pouring temperature is 1420~1460℃, the pouring speed is 4~6kg / s, and the pressure is maintained at -0.07~-0.09MPa throughout the process; after pouring, the pressure is maintained at negative pressure for 30 minutes for shrinkage compensation.

9. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S6, the segmented cooling is as follows: First cooling, the sand box is allowed to cool naturally for 90~120 minutes to reduce the casting temperature to 750~800℃; Second cooling, the air cooling system is turned on with a wind speed of 3~4m / s to cool to below 300℃; The negative pressure system is turned off when the casting temperature drops to below 200℃.

10. The low-porosity lost foam casting process as described in claim 1, characterized in that, In step S7, the shot blasting is performed using a tracked shot blasting machine with a steel shot particle size of 1.0 mm and a processing time of 8-12 minutes; the low-temperature aging treatment is performed at a temperature of 520-560℃, and the temperature is maintained for 3.5-4.5 hours before being cooled in the furnace.