Low-pressure casting process for aluminum-magnesium alloy motor end cover

By combining ultrasonic vibrating rods with inert gas blowing pipes for degassing, spiral guide grooves with annular inert gas chamber protection, multiple temperature control channels, and local extrusion mechanisms, the problems of insufficient degassing of molten metal, secondary oxidation during mold filling, and shrinkage porosity in thick parts in low-pressure casting have been solved, thus improving the casting quality and yield of aluminum-magnesium alloy motor end caps.

CN123149385APending Publication Date: 2026-11-24江西铭喆铝镁新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611412671.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing low-pressure casting technology has problems in the production of aluminum-magnesium alloy motor end caps, such as insufficient degassing of the melt, secondary oxidation during the filling process, difficulty in eliminating shrinkage porosity in thick and large parts, and open-loop control of process parameters. These problems result in high porosity, poor mechanical properties, and unstable yield of the castings.

Method used

The system employs a combination of ultrasonic vibrating rods and inert gas jets for degassing, spiral guide channels and annular inert gas chambers for protection within the riser pipe, multiple independent temperature control channels, and local extrusion mechanisms. Combined with a pulsed pneumatic system and closed-loop control, it achieves molten metal purification, mold filling with anti-oxidation, and precise shrinkage of thick and large sections.

Benefits of technology

It effectively reduces the gas content of the molten metal, prevents secondary oxidation, ensures the internal density of the casting, improves the mechanical properties and yield of the casting, and achieves the stability and consistency of the casting quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149385A_ABST
    Figure CN123149385A_ABST
Patent Text Reader

Abstract

This invention provides a low-pressure casting process for aluminum-magnesium alloy motor end caps, relating to the field of non-ferrous metal casting technology. The low-pressure casting apparatus for aluminum-magnesium alloy motor end caps includes a holding furnace, a liquid-lifting assembly, a mold assembly, a pulsed pneumatic system, and a local extrusion mechanism. The holding furnace is equipped with an ultrasonic vibrator and an inert gas injection pipe, and the upper gas chamber of the holding furnace is connected to the pulsed pneumatic system. The liquid-lifting assembly includes a liquid-lifting pipe, a protective sleeve, an annular inert gas chamber, a spiral guide groove, and an air inlet connector. The inner wall of the liquid-lifting pipe is machined with a spiral guide groove, and the protective sleeve is coaxially fitted around the outside of the liquid-lifting pipe to form an annular inert gas chamber. The pulsed pneumatic system achieves stable pulsating filling of the mold with molten metal, combined with inert gas protection in the liquid-lifting pipe, independent temperature control of the mold zones, and temperature-triggered local extrusion, achieving a comprehensive effect of improved internal density and enhanced mechanical properties of the casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metal casting technology, specifically to a low-pressure casting process for aluminum-magnesium alloy motor end caps. Background Technology

[0002] Aluminum-magnesium alloy motor end caps are key structural components in high-end equipment such as drive motors for new energy vehicles, industrial servo motors, and wind turbines. They serve multiple functions, including supporting bearings, providing sealing protection, and dissipating heat. Their internal quality and mechanical properties directly determine the operational reliability and service life of the entire motor. As motors develop towards higher power density, higher speed, and lighter weight, the wall thickness of end cap castings is continuously decreasing, and their structures are becoming increasingly complex, placing higher demands on casting processes. Low-pressure casting, with its advantages of stable filling, good feeding effect, and high yield, has become the mainstream forming process for aluminum-magnesium alloy motor end caps. However, existing low-pressure casting technology still faces several problems that urgently need to be solved in actual production.

[0003] Existing low-pressure casting equipment generally employs a single inert gas rotary degassing method in the molten metal treatment stage. This method has limited degassing efficiency. Magnesium in molten aluminum-magnesium alloys is highly chemically reactive and readily combines with hydrogen at high temperatures to form pinhole defects. A single degassing method is insufficient to reduce the gas content of the molten metal to below 0.2 mL / 100g, resulting in a porosity in finished castings generally exceeding 1.5%, severely weakening the fatigue strength and pressure resistance of the castings. Furthermore, the riser pipes in existing equipment are mostly smooth, straight-through structures. As the molten metal rises under gas pressure, turbulence and vortices are easily generated. The low-pressure zone at the center of the vortex entrains air above the liquid surface into the molten metal, creating secondary air entrapment and further increasing the risk of porosity defects in the castings.

[0004] Current low-pressure casting filling control generally adopts a constant air pressure drive method. Under constant pressure, the molten liquid surface at the front end has a large contact area with air, which easily generates splashing, resulting in prominent problems of air entrapment and oxidation during the filling process. The magnesium content in molten aluminum-magnesium alloys is as high as 4.5%. At high temperatures of 720–760℃, it can instantly generate magnesium oxide and spinel-like oxide inclusions upon contact with air. These hard particles, once they enter the casting, become fatigue crack initiation sites, significantly reducing the mechanical properties and service life of the casting. Existing equipment lacks effective inert gas protection measures at the riser pipe outlet. When the molten liquid flows out of the riser pipe and into the gating sleeve, it comes into direct contact with air, making secondary oxidation difficult to avoid.

[0005] Existing low-pressure casting mold temperature control systems generally use an integrated cooling channel, where the temperature of each part cannot be independently adjusted, making it difficult to create an ideal sequential solidification temperature gradient within the mold cavity. The wall thickness of the motor end cover bearing chamber is typically 2 to 3 times that of other parts. This thicker section has a longer solidification time, and under overall temperature control, it is prone to forming isolated liquid phase zones, resulting in shrinkage porosity and defects. Existing devices lack precise feeding methods for thicker sections; relying solely on riser pipe pressure feeding is insufficient to completely eliminate shrinkage porosity in these areas, leading to insufficient internal density in the casting and making it prone to leakage and cracking during subsequent processing and use.

[0006] Current low-pressure casting processes generally employ open-loop sequential control, where parameters such as filling pressure, holding time, and cooling rate are executed according to a preset sequence, lacking a closed-loop adjustment mechanism based on real-time temperature and pressure feedback from the casting. Fluctuations in melt temperature, composition, and mold thermal state between different batches mean that open-loop control cannot dynamically adjust process parameters based on actual conditions, resulting in poor casting quality consistency and large fluctuations in yield. Furthermore, existing equipment lacks an intelligent local extrusion trigger mechanism at critical solidification moments in thick sections; the timing of extrusion relies entirely on operator experience. Extrusion too early leads to melt backflow, while extrusion too late results in insufficient deformation, making it difficult to consistently achieve the desired local extrusion feeding effect.

[0007] The existing low-pressure casting of aluminum-magnesium alloy motor end caps has four drawbacks: insufficient degassing of the melt leading to high porosity; lack of protection during liquid filling leading to secondary oxidation and inclusions; uneven mold temperature control leading to shrinkage and porosity in thick parts; and open-loop process control leading to poor quality consistency. These drawbacks restrict the improvement of the mechanical properties and yield of the end cap castings. Summary of the Invention

[0008] To address the shortcomings of existing technologies, this invention provides a low-pressure casting process for aluminum-magnesium alloy motor end caps, which solves the problems of insufficient degassing of the melt, secondary oxidation during the filling process, difficulty in eliminating shrinkage porosity in thick parts, and open-loop control of process parameters in existing low-pressure casting.

[0009] To achieve the above objectives, the present invention provides the following technical solution: a low-pressure casting processing device for aluminum-magnesium alloy motor end caps, comprising a heat-holding melting furnace, a liquid lifting assembly, a mold assembly, a pulse air pressure system, and a local extrusion mechanism. The heat-insulating smelting furnace is equipped with an ultrasonic vibrating rod and an inert gas injection pipe, and the upper air chamber of the heat-insulating smelting furnace is connected to a pulsed gas pressure system. The liquid lifting assembly includes a liquid lifting pipe, a protective sleeve, an annular inert gas chamber, a spiral guide groove, and an air inlet connector. The inner wall of the liquid lifting pipe is machined with a spiral guide groove. The protective sleeve is coaxially sleeved on the outside of the liquid lifting pipe to form an annular inert gas chamber. The air inlet connector is connected to the annular inert gas chamber. The mold assembly includes an upper mold, a lower mold, a side mold, a temperature control channel, and a sprue sleeve. The upper mold, lower mold, and side mold together form a cavity. The sprue sleeve is installed at the center of the lower mold and connected to the riser pipe. The temperature control channel is independently set inside the upper mold, lower mold, and side mold. The pulsed pneumatic system includes a gas storage tank, a proportional regulating valve, and a pulse solenoid valve. The gas outlet of the gas storage tank is connected to the proportional regulating valve and the pulse solenoid valve in sequence and then connected to the gas chamber of the heat-insulating melting furnace. The local extrusion mechanism is equipped with an extrusion push rod, a drive cylinder, a pressure sensor, and a displacement sensor. The drive cylinder drives the extrusion push rod to penetrate the thick part of the upper mold cavity, and the pressure sensor and displacement sensor detect the extrusion force and displacement, respectively.

[0010] Preferably, the ultrasonic vibrating rod and the inert gas injection pipe are arranged at 90° intervals around the circumference of the furnace cover. The vibrating head of the ultrasonic vibrating rod is immersed 120-180 mm below the surface of the molten liquid, and its axis is parallel to the axis of the heat-preserving smelting furnace with a spacing of 60-80 mm. The lower end of the inert gas injection pipe extends to 20-30 mm above the bottom of the crucible, and the gas outlet is equipped with porous graphite balls with uniformly distributed injection holes of 0.3-0.8 mm in diameter on the surface of the balls.

[0011] Preferably, the riser tube is a straight circular tube made of silicon nitride ceramic material, with its lower end inserted 80-120mm below the molten liquid surface and its upper end connected to the sprue sleeve. The spiral guide groove has a lead of 1.5-3 times the inner diameter of the riser tube and a groove depth of 2-5mm. The width of the annular inert gas chamber is 15-25mm. The gas inlet connector is connected to an argon gas source via a flexible hose.

[0012] Preferably, the internal temperature control channel of the lower mold is a double-ring structure, with the inner ring 10-20mm from the outer wall of the sprue sleeve and the outer ring 20-30mm from the inner ring. The internal temperature control channel of the side mold is a serpentine structure arranged at equal intervals from top to bottom. The internal temperature control channel of the upper mold is an Archimedean spiral structure. Each group of temperature control channels is connected to an independent mold temperature controller.

[0013] Preferably, the proportional regulating valve has an adjustment range of 0 to 0.1 MPa, and the pulse solenoid valve opens and closes rapidly at a frequency of 0.5 to 3 Hz to superimpose the reference pressure to form a periodic pulse pressure. The pulse pneumatic system also includes a controller and a pressure transmitter. The detection end of the pressure transmitter extends into the gas chamber of the heat-insulating melting furnace, and the signal output end is connected to the controller. The output end of the controller is connected to the proportional regulating valve and the pulse solenoid valve respectively to form a pressure closed loop.

[0014] Preferably, the driving cylinder is a pneumatic-hydraulic booster cylinder, the pressure sensor is a spoke-type tension / compression sensor connected in series between the piston rod of the driving cylinder and the extrusion push rod, the displacement sensor is a pull rod-type linear displacement sensor, the end of the pull rod is connected to the side wall of the extrusion push rod, the lower end of the extrusion push rod is provided with a contoured pressure head, the surface of the pressure head is coated with a 0.1-0.3mm thick titanium nitride coating, the mold assembly is also provided with a temperature sensor, the temperature measuring end is in close contact with the inner wall of the thick part of the cavity, and the signal output end is connected to the controller.

[0015] A low-pressure casting process for an aluminum-magnesium alloy motor end cap includes the following steps: S1. Melt preparation: Add aluminum-magnesium alloy raw materials to a heat-insulating melting furnace and heat to 720-760℃. Start the ultrasonic vibrating rod and inert gas blowing pipe to degas for 8-15 minutes. S2. Mold preheating: Heating medium is introduced into the temperature control channels of the upper mold, lower mold and side mold through an independent mold temperature controller. The upper mold is preheated to 320-360℃, the lower mold is preheated to 280-320℃, and the side mold is preheated to 300-340℃. S3, Pulse Liquefaction Filling: The pulse air pressure system applies a pulse pressure of 25-35 kPa to the gas chamber of the heat-insulating melting furnace, with a pulse frequency of 0.5-3 Hz. The molten liquid fills the mold cavity through the riser pipe at a speed of 80-120 mm / s, and the filling time is 8-15 s. S4. Pressure Crystallization: After filling, the pressure in the gas chamber is increased to 60-90 kPa and held for 12-20 seconds. The casting is fed through the molten liquid column in the riser pipe. S5. Local extrusion and compensation: When the temperature sensor detects that the temperature of the molten metal in the thick part drops to 15-30°C above the solidus line, the controller triggers the drive cylinder to push the extrusion push rod downward at 15-30 mm / s, applying an extrusion force of 20-40 kN, holding the pressure for 3-6 seconds, and then retracting. S6. Pressure relief and cooling: Release the pressure in the air chamber, allow the unsolidified molten liquid in the riser pipe to flow back, switch the cooling medium in the temperature control channel, and cool the casting to 180-220°C at a rate of 3-6°C / s. S7. Mold opening and part removal: The upper mold rises to open the mold, the side mold pulls the core horizontally, and the ejection mechanism ejects the casting from the lower mold. S8. Heat treatment: Solution treatment of castings at 530-550℃ for 4-6 hours, quenching transfer time ≤15s, water quenching at 60-80℃, aging treatment at 160-180℃ for 6-8 hours.

[0016] Preferably, in step S1, the aluminum-magnesium alloy composition by mass percentage is Mg 4.5%–5.5%, Mn 0.3%–0.6%, Si 0.2%–0.4%, Ti 0.1%–0.2%, Be 0.005%–0.01%, with the balance being Al. An Al-Ti-B modifier is added during the melt preparation process, with the amount added being 0.8%–1.2% of the alloy mass. After degassing, the gas content of the melt is ≤0.15mL / 100g.

[0017] Preferably, in step S3, the pulse pressure waveform is a trapezoidal wave with a pulse frequency of 1-2 Hz, a duty cycle of 30%-70%, and a pressure amplitude fluctuation of ±15% of the reference pressure. In step S6, the surface temperature of the casting is monitored by an infrared temperature measuring device, and when the surface temperature of the casting exceeds 420°C, the controller automatically increases the flow rate of the cooling medium.

[0018] Preferably, in step S5, the extrusion stroke of the extrusion pusher is 5-20mm, the extrusion pressure is fed back in real time by a pressure sensor, and the extrusion depth is fed back in real time by a displacement sensor. When the extrusion pressure reaches the set value or the displacement reaches the set stroke, the controller automatically stops the extrusion and holds the pressure. In step S8, the solution treatment heating rate is 80-120℃ / h, and the final casting has a tensile strength ≥280MPa, a yield strength ≥160MPa, an elongation ≥8%, a porosity ≤0.5%, and a dimensional accuracy of CT6 grade.

[0019] Working Principle: During the low-pressure casting of aluminum-magnesium alloy motor end caps, the system first completes initial configuration after power-on. The controller reads the pre-stored process parameter formula, including pressure setpoints for each stage, pulse frequency, preheating temperatures of various parts of the mold, extrusion trigger temperature thresholds, and heat treatment curves. Each mold temperature controller starts and circulates heating oil into the temperature control channels of the upper mold, lower mold, and side mold according to the set temperatures. Once the temperature of each part of the mold stabilizes within the set range, the system enters the production standby state.

[0020] During the melt preparation stage, the aluminum-magnesium alloy raw material is melted by resistance heating elements in a holding furnace and heated to 720–760°C. After reaching the set temperature, the ultrasonic vibrator is activated, generating a high-intensity ultrasonic field at a frequency of 20 kHz inside the melt. The periodic alternation of positive and negative sound pressure causes a large number of tiny cavitation nuclei to be generated in the melt. The cavitation nuclei grow rapidly in the negative pressure phase and collapse violently in the positive pressure phase. The local high temperature and pressure generated at the moment of collapse, along with the micro-jet, break the hydrogen film adsorbed on the surface of oxide inclusions in the melt, allowing the hydrogen to be released. At the same time, the porous graphite ball at the bottom of the inert gas jet pipe disperses the argon gas into microbubbles with a diameter of 0.3–0.8 mm and diffuses them into the bottom of the melt. The microbubbles rise slowly under the action of buoyancy. Since the partial pressure of hydrogen inside the bubbles is zero, hydrogen atoms in the melt diffuse into the interior of the bubbles under the drive of the concentration gradient and are carried to the surface by the bubbles and escape. The rising microbubbles also adsorb suspended oxide inclusion particles to form scum. After 8–15 minutes of synergistic action of ultrasonic cavitation and inert gas microbubbles, the gas content of the melt decreased to below 0.15 mL / 100 g.

[0021] Before filling, argon gas is continuously injected into the annular inert gas chamber through the inlet connector. After the air in the chamber is completely replaced, a slightly positive pressure argon atmosphere of 5-15 kPa is formed. The argon gas slowly overflows from the outlet of the riser pipe, forming an inert gas protective layer in the gating sleeve and the bottom area of ​​the cavity, completely displacing the air in that area. After the pre-protection lasts for 3-5 seconds, the pulse pressure system is activated. The compressed air in the gas tank is adjusted to a reference pressure of 25-35 kPa by the proportional regulating valve, and then the pulse solenoid valve is rapidly opened and closed at a frequency of 0.5-3 Hz, so that the driving pressure acting on the surface of the molten liquid presents a composite waveform of the reference pressure superimposed with pulse fluctuations. Driven by the pressure difference, the molten liquid flows upward along the riser pipe. The spiral guide groove on the inner wall of the riser pipe applies a circumferential velocity component to the molten liquid, causing the molten liquid to form a spiral upward flow state rotating around the axis. The centrifugal effect of the spiral flow causes residual bubbles to gather towards the center and accelerate upward, while suppressing the generation of transverse secondary flow and local vortices, significantly reducing the risk of air entrapment. The molten liquid flows through the riser pipe at an average speed of 80-120 mm / s, and is injected from the bottom of the cavity through the sprue sleeve. It fills the cavity smoothly from bottom to top and from the center to the edge, with the filling time controlled at 8-15 seconds.

[0022] After the mold cavity is filled, the proportional control valve increases the output pressure to 60-90 kPa, entering the pressurized crystallization stage. The holding pressure is transmitted to the casting through the molten liquid column in the riser pipe, continuously compensating for volume shrinkage during solidification. Simultaneously, four independent temperature control channels operate continuously at preset temperatures. The upper mold has the lowest temperature, allowing thin-walled sections to solidify first; the upper part of the side mold has a lower temperature than the lower part, causing the solidification front to advance from top to bottom; the lower mold has a higher temperature, and the area around the gate is even hotter, ensuring the gate area solidifies last, thus creating a sequential solidification path from the far end of the mold cavity to the gate. A pressure transmitter at the gas cavity of the holding furnace detects the gas cavity pressure in real time at a sampling frequency of 100 Hz and feeds the signal back to the controller. The controller dynamically adjusts the opening of the proportional control valve using a PID algorithm, keeping the deviation between the actual pressure and the set curve within ±1 kPa.

[0023] During solidification, a temperature sensor monitors the cavity wall temperature in real time for the thicker section of the bearing chamber in the upper mold. When the molten metal temperature in this section drops to 15–30°C above the solidus line, the molten metal is in a semi-solid state, having formed a continuous grain skeleton but still containing liquid phase between the grains, making it compressible. The controller immediately triggers the drive cylinder. The drive cylinder pushes the extrusion push rod downwards at a speed of 15–30 mm / s, applying an extrusion force of 20–40 kN to the thicker section, compressing the intergranular liquid phase in the semi-solid structure and compacting the grain skeleton. A pressure sensor detects the extrusion force in real time, and a displacement sensor detects the extrusion depth in real time. Both signals are fed back to the controller to form a double closed loop of force and displacement. When the extrusion force reaches the set value or the displacement reaches the set stroke of 5–20 mm, the system automatically stops and holds the pressure for 3–6 seconds, after which the push rod retracts.

[0024] After the pressure holding and local extrusion are completed, the pressure in the air chamber is rapidly released, and the unsolidified molten liquid in the riser pipe flows smoothly back along the spiral channel under gravity, avoiding vacuum suction caused by liquid column breakage. The temperature control channel switches to cooling medium, accelerating the cooling of the casting at a rate of 3-6℃ / s. An infrared thermometer monitors the surface temperature of the casting, automatically increasing the cooling flow rate when it exceeds 420℃. After the casting cools to 180-220℃, the mold is opened. The upper mold rises with the moving template, and the side mold horizontally pulls out the heat dissipation fins and mounting bosses, etc., and the ejection mechanism ejects the casting from the lower mold. The casting then enters the heat treatment process, being heated to 530-550℃ at a heating rate of 80-120℃ / h and held for 4-6 hours for solution treatment. The quenching transfer time is controlled within 15 seconds. After quenching in water at 60-80℃, it undergoes aging treatment at 160-180℃ for 6-8 hours, finally obtaining a high-performance aluminum-magnesium alloy motor end cover casting.

[0025] This invention provides a low-pressure casting process for aluminum-magnesium alloy motor end caps. It offers the following advantages: This invention achieves efficient degassing and purification by using an ultrasonic vibrating rod and an inert gas jet pipe working synergistically within a heat-insulating melting furnace, and by employing a phase difference arrangement to avoid mutual interference between vibration and airflow.

[0026] This invention uses a spiral guide groove on the inner wall of the riser tube to make the molten liquid form an orderly spiral upward flow, and with the positive pressure argon protection of the annular inert gas cavity between the protective sleeve and the riser tube, it achieves a dual protection effect of preventing gas entrapment and secondary oxidation during the filling process.

[0027] This invention achieves precise temperature control by using multiple independent temperature control systems, including an upper mold spiral channel, a lower mold double annular channel, and a side mold serpentine channel, along with a temperature gradient setting from the far end to the gate, to achieve sequential solidification of the entire casting and delayed solidification of thick parts.

[0028] This invention uses a temperature sensor to detect the temperature of thick sections in real time and triggers the action of a local extrusion mechanism. Combined with the dual closed-loop feedback of a pressure sensor and a displacement sensor, it achieves precise extrusion and shrinkage compensation and shrinkage elimination effects in the semi-solid region of thick sections. Attached Figure Description

[0029] Figure 1 This is a perspective view of the present invention; Figure 2 This is a half-sectional view of the heat-insulating smelting furnace of the present invention; Figure 3 This is a half-sectional view of the mold assembly of the present invention; Figure 4 This is a schematic diagram of the ultrasonic vibrating rod structure of the present invention; Figure 5 This is a half-sectional view of the liquid lifting assembly of the present invention; Figure 6 This is a half-sectional view of the mold assembly of the present invention; Figure 7 This is a schematic diagram of the pulse pneumatic system structure of the present invention; Figure 8 This is a flowchart of the steps of the present invention; Figure 9 This is a pulse filling pressure curve diagram of the present invention.

[0030] The components include: 1. Insulating melting furnace; 11. Ultrasonic vibrator; 12. Inert gas injection pipe; 2. Liquid lifting assembly; 21. Liquid lifting pipe; 22. Protective sleeve; 23. Annular inert gas chamber; 24. Spiral guide groove; 25. Air inlet connector; 3. Mold assembly; 31. Upper mold; 32. Lower mold; 33. Side mold; 34. Temperature control channel; 35. Sprue sleeve; 4. Pulse air pressure system; 41. Gas storage tank; 42. Proportional regulating valve; 43. Pulse solenoid valve. Detailed Implementation

[0031] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example

[0032] like Figure 1-9 As shown, this embodiment of the invention provides a low-pressure casting processing device for aluminum-magnesium alloy motor end caps, including a heat-holding melting furnace 1, a liquid lifting assembly 2, a mold assembly 3, a pulsed pneumatic system 4, and a local extrusion mechanism. The heat-holding melting furnace 1 is equipped with an ultrasonic vibrating rod 11 and an inert gas jet pipe 12. The upper gas chamber of the heat-holding melting furnace 1 is connected to the pulsed pneumatic system 4. The ultrasonic vibrating rod 11 and the inert gas jet pipe 12 are arranged at 90° intervals in the circumferential direction of the furnace cover. The vibrating head of the ultrasonic vibrating rod 11 is immersed 120-180 mm below the surface of the molten liquid, and its axis is parallel to the axis of the heat-holding melting furnace 1 with a spacing of 60-80 mm. The lower end of the inert gas jet pipe 12 extends to 20-30 mm above the bottom of the crucible, and the gas outlet is equipped with a porous graphite ball with uniformly distributed jet holes of 0.3-0.8 mm in diameter on the surface of the ball. The liquid riser assembly 2 includes a liquid riser tube 21, a protective sleeve 22, an annular inert gas chamber 23, a spiral guide groove 24, and an inlet connector 25. The inner wall of the liquid riser tube 21 is machined with a spiral guide groove 24. The protective sleeve 22 is coaxially sleeved on the outside of the liquid riser tube 21 to form an annular inert gas chamber 23. The inlet connector 25 is connected to the annular inert gas chamber 23. The liquid riser tube 21 is a straight circular tube made of silicon nitride ceramic material. The lower end is inserted 80-120mm below the surface of the molten liquid, and the upper end is connected to the gate sleeve 35. The lead of the spiral guide groove 24 is 1.5-3 times the inner diameter of the liquid riser tube 21, and the groove depth is 2-5mm. The width of the annular inert gas chamber 23 is 15-25mm. The inlet connector 25 is connected to an argon gas source through a flexible hose. The mold assembly 3 includes an upper mold 31, a lower mold 32, a side mold 33, a temperature control channel 34, and a sprue sleeve 35. The upper mold 31, lower mold 32, and side mold 33 together form a cavity. The sprue sleeve 35 is installed at the center of the lower mold 32 and is connected to the riser pipe 21. The temperature control channels 34 are independently set inside the upper mold 31, lower mold 32, and side mold 33. The temperature control channel 34 inside the lower mold 32 has a double ring structure, with the inner ring 10-20mm away from the outer wall of the sprue sleeve 35 and the outer ring 20-30mm away from the inner ring. The temperature control channels 34 inside the side mold 33 have four sets of serpentine structures arranged at equal intervals from top to bottom. The temperature control channels 34 inside the upper mold 31 have an Archimedean spiral structure. Each set of temperature control channels 34 is connected to an independent mold temperature controller. The pulse pressure system 4 includes a gas storage tank 41, a proportional regulating valve 42, and a pulse solenoid valve 43. The outlet of the gas storage tank 41 is connected to the proportional regulating valve 42 and the pulse solenoid valve 43 in sequence and then connected to the gas chamber of the heat-insulating smelting furnace 1. The proportional regulating valve 42 has an adjustment range of 0 to 0.1 MPa. The pulse solenoid valve 43 opens and closes rapidly at a frequency of 0.5 to 3 Hz to superimpose the reference pressure to form a periodic pulse pressure. The pulse pressure system 4 also includes a controller and a pressure transmitter. The detection end of the pressure transmitter extends into the gas chamber of the heat-insulating smelting furnace 1, and the signal output end is connected to the controller. The output end of the controller is connected to the proportional regulating valve 42 and the pulse solenoid valve 43 respectively to form a pressure closed loop. The local extrusion mechanism includes an extrusion push rod, a drive cylinder, a pressure sensor, and a displacement sensor. The drive cylinder drives the extrusion push rod to penetrate the thick part of the upper mold 31 cavity. The pressure sensor and displacement sensor detect the extrusion force and displacement, respectively. The drive cylinder is a pneumatic-hydraulic booster cylinder. The pressure sensor is a spoke-type tension / compression sensor connected in series between the piston rod of the drive cylinder and the extrusion push rod. The displacement sensor is a pull rod-type linear displacement sensor. The end of the pull rod is connected to the side wall of the extrusion push rod. The lower end of the extrusion push rod is equipped with a contoured pressure head. The surface of the pressure head is coated with a 0.1-0.3mm thick titanium nitride coating. The mold assembly 3 is also equipped with a temperature sensor. The temperature measuring end is in close contact with the inner wall of the thick part of the cavity, and the signal output end is connected to the controller.

[0033] A low-pressure casting process for an aluminum-magnesium alloy motor end cap includes the following steps: S1. Melt preparation: The aluminum-magnesium alloy raw material is added to the heat-holding melting furnace 1 and heated to 720-760℃. The ultrasonic vibrating rod 11 and the inert gas blowing pipe 12 are started to degas together for 8-15 minutes. The aluminum-magnesium alloy composition by mass percentage is Mg 4.5%-5.5%, Mn 0.3%-0.6%, Si 0.2%-0.4%, Ti 0.1%-0.2%, Be 0.005%-0.01%, and the balance is Al. During the melt preparation process, Al-Ti-B modifier is added at a rate of 0.8%-1.2% of the alloy mass. After degassing, the gas content of the melt is ≤0.15mL / 100g. S2. Mold preheating: Heating medium is introduced into the temperature control channels 34 of the upper mold 31, lower mold 32 and side mold 33 by independent mold temperature controllers. The upper mold 31 is preheated to 320-360℃, the lower mold 32 is preheated to 280-320℃ and the side mold 33 is preheated to 300-340℃. S3, Pulse-driven liquid filling: The pulse air pressure system 4 applies a pulse pressure of 25-35 kPa to the gas chamber of the heat-insulating melting furnace 1, with a pulse frequency of 0.5-3 Hz. The molten liquid fills the mold cavity through the liquid riser pipe 21 at a speed of 80-120 mm / s, with a filling time of 8-15 s. The pulse air pressure waveform is a trapezoidal wave with a pulse frequency of 1-2 Hz, a duty cycle of 30%-70%, and a pressure amplitude fluctuation of ±15% of the reference pressure. In step S6, the surface temperature of the casting is monitored by an infrared temperature measuring device. When the surface temperature of the casting exceeds 420°C, the controller automatically increases the flow rate of the cooling medium. S4. Pressure Crystallization: After filling, the pressure in the gas chamber is increased to 60-90 kPa and held for 12-20 seconds. The molten liquid column in the riser pipe 21 is used to feed the casting. S5. Local extrusion and feeding: When the temperature sensor detects that the molten temperature in the thick part drops to 15-30℃ above the solidus line, the controller triggers the drive cylinder to push the extrusion pusher downward at 15-30mm / s, applying an extrusion force of 20-40kN. After holding the pressure for 3-6s, the pusher retracts. The extrusion stroke of the extrusion pusher is 5-20mm. The extrusion force is fed back in real time by the pressure sensor, and the extrusion depth is fed back in real time by the displacement sensor. When the extrusion force reaches the set value or the displacement reaches the set stroke, the controller automatically stops the extrusion and holds the pressure. The solution treatment heating rate in step S8 is 80-120℃ / h. The final casting has a tensile strength ≥280MPa, a yield strength ≥160MPa, an elongation ≥8%, a porosity ≤0.5%, and a dimensional accuracy of CT6 grade. S6, Pressure relief and cooling: Release the pressure in the air chamber, the unsolidified molten liquid in the riser pipe 21 flows back, the temperature control channel 34 switches the cooling medium, and cools the casting to 180-220°C at a rate of 3-6°C / s. S7. Mold opening and part removal: The upper mold 31 rises to open the mold, the side mold 33 pulls the core horizontally, and the ejection mechanism ejects the casting from the lower mold 32. S8. Heat treatment: Solution treatment of castings at 530-550℃ for 4-6 hours, quenching transfer time ≤15s, water quenching at 60-80℃, aging treatment at 160-180℃ for 6-8 hours. Example

[0034] This embodiment describes the molten metal treatment and filling operation of the low-pressure casting processing device. The holding furnace 1 is a resistance-heated crucible furnace with a nominal capacity of 300 kg. The furnace lining is made of corundum refractory material, and the resistance heating element is iron-chromium-aluminum wire. The maximum operating temperature is 850℃, and the temperature control accuracy is ±3℃. The ultrasonic vibrator 11 is made of titanium alloy, with a vibration frequency of 20 kHz and a rated power of 2 kW. The vibrating head is conical to enhance the cavitation effect, and the vibrating head is immersed 150 mm below the molten metal surface. The inert gas blowing pipe 12 is made of 310S stainless steel, with a pipe diameter of 12 mm. The bottom has a porous graphite ball with a diameter of 25 mm, and 60 small blowing holes with a diameter of 0.5 mm are distributed on the sphere. The lower end of the blowing pipe extends 25 mm above the bottom of the crucible. The ultrasonic vibrating rod 11 and the inert gas injection pipe 12 are arranged at 90° intervals around the circumference of the furnace cover, located slightly to the left and slightly to the right of the center, respectively, with a axial distance of 70 mm between them, to avoid interference between the ultrasonic vibration field and the rising argon gas flow field. The upper gas chamber of the holding melting furnace 1 has a volume of approximately 0.05 m³. A gas pipe interface is provided on the side of the furnace cover to connect to the pulse gas pressure system 4. A diffused silicon pressure transmitter is installed on the top of the gas chamber, with a measurement range of 0–0.2 MPa and an accuracy of 0.2 class. It samples at a frequency of 100 Hz and transmits the signal to the controller via a 4–20 mA shielded cable.

[0035] The riser tube 21 is made of reaction-sintered silicon nitride ceramic, with an outer diameter of 60 mm, an inner diameter of 40 mm, a total length of 600 mm, a bending strength ≥500 MPa, and a coefficient of thermal expansion of 3.2 × 10⁻⁻⁻⁶. 6 The temperature is / ℃, exhibiting excellent thermal shock resistance and non-stick properties to aluminum. The inner wall of the riser tube 21 is machined with a continuous spiral guide groove 24, with a lead of 80mm (twice the inner diameter), a groove depth of 3mm, and a groove width of 5mm. It spirals upwards from the lower opening to the upper outlet. The lower end of the riser tube 21 is immersed 100mm below the molten metal surface, and the upper end is connected to the bottom gating sleeve 35 of the lower mold 32 via a flange, with a 2mm thick aluminum silicate refractory fiber sealing gasket between the end faces. The protective sleeve 22 is made of 304 stainless steel, with an inner diameter of 90mm and a wall thickness of 5mm. It is coaxially sleeved on the outside of the riser tube 21, forming a 20mm wide annular inert gas cavity 23 between them. The upper and lower ends of the protective sleeve 22 are sealed and fixed to the bottom surface of the lower mold 32 and the furnace cover respectively via flanges, with high-temperature resistant graphite sealing rings used between the flanges. The air inlet connector 25 is a ZG 1 / 2-inch external thread connector, which is welded to the upper side wall of the protective sleeve 22, 50mm away from the upper flange. It is connected to the argon gas source through a Φ8mm stainless steel metal hose. The argon gas flow rate is controlled at 3-5L / min by a rotor flow meter to maintain a slight positive pressure of 8-12kPa in the annular cavity. Example

[0036] This embodiment describes the mold temperature control and local extrusion operation of the device. Mold assembly 3 is machined from H13 hot-work mold steel. The cavity surface is CNC milled and polished to Ra0.8μm, then nitrided with a nitriding layer depth of 0.3–0.5 mm and a surface hardness of HV800 or higher. The lower mold 32 has external dimensions of 450 mm × 450 mm × 80 mm, with a central stepped hole diameter of 50 mm. The sprue sleeve 35 is made of beryllium copper alloy CuBe2, with a hardness of HRC35–40 and a thermal conductivity of 180 W / (m·K). It is press-fitted into the central hole of the lower mold 32 with an H7 / k6 interference fit. The inner diameter of the sprue sleeve 35 is 40 mm, consistent with the inner diameter of the riser pipe 21. The lower mold 32 has a double-ring temperature control channel 34 machined inside. The inner ring channel has a diameter of 8mm and is distributed in a 35mm radius ring around the sprue sleeve 35, 15mm from the outer wall of the sprue. The outer ring channel has a diameter of 8mm and is distributed in a 70mm radius ring, 25mm from the inner ring. The two ring channels are independent and are connected to independent mold temperature controllers through G1 / 4 inch pipe fittings. The two side molds 33 have external dimensions of 200mm×400mm×120mm and are driven by hydraulic cylinders with a diameter of 80mm for horizontal core pulling. The core pulling stroke is 120mm and the mold closing force is 100kN on each side. The mold closing surface of the side mold 33 and the side positioning surface of the lower mold 32 adopt an H7 / h6 clearance fit. The parting surface is located at the maximum contour of the casting. Each side mold 33 has four sets of serpentine temperature control channels 34 machined vertically inside, with a channel diameter of 8mm. Each channel folds back 6 times, and the four sets of channels are arranged at equal intervals of 25mm from top to bottom. Each channel is connected to an independent mold temperature controller to achieve gradient temperature control along the height of the side mold. The upper mold 31 has external dimensions of 450mm×450mm×70mm and has Archimedes spiral temperature control channels 34 machined inside, with a channel diameter of 8mm. The channels start from a center radius of 20mm and expand outward to a radius of 180mm, spiraling for a total of 3 turns. They are connected to an independent mold temperature controller through side pipe joints. The upper mold 31 has a vertical through hole with a diameter of 25mm machined at the thick part of the bearing chamber. An H13 steel guide sleeve is press-fitted into the hole. The guide sleeve has an inner hole of 20mm and a length of 50mm, and it has an H7 / f7 clearance fit with the extrusion push rod. The temperature sensor uses a K-type nickel-chromium / nickel-silicon armored thermocouple with an outer diameter of 3mm. It is inserted through the mounting hole on the top surface of the upper mold 31, with the measuring end close to the inner wall of the thick part of the cavity. The insertion depth is 15mm. The signal is transmitted to the controller through a high-temperature shielded cable. The temperature measurement range is 0~800℃, and the accuracy is ±1.5℃.

[0037] The gas storage tank 41 of the pulse pneumatic system 4 is a vertical carbon steel pressure vessel with a volume of 50L and a design pressure of 0.8MPa. The top outlet is connected to a proportional regulating valve 42 and a pulse solenoid valve 43 via a Φ12mm stainless steel pipe, and then into the gas chamber of the heat-insulating melting furnace 1. The proportional regulating valve 42 is an electro-proportional valve with an input signal of 4~20mA, an adjustment range of 0~0.1MPa, a linear accuracy of ±0.5%, and a response time ≤50ms. The pulse solenoid valve 43 is a high-frequency direct-acting solenoid valve with a diameter of 8mm, a response time ≤10ms, and a maximum operating frequency of 5Hz, rapidly opening and closing at a frequency of 0.5~3Hz to generate pulsed airflow. The controller uses a Siemens S7-1200 series PLC, mounted on the electrical mounting plate in front of the gas storage tank 41. It has a built-in analog input module to receive signals from the pressure transmitter and temperature sensor, a digital output module to control the pulse solenoid valve 43, and an analog output module to control the proportional regulating valve 42. The PID control cycle is 10ms. The air inlet of the air tank 41 connects to an external 0.7MPa compressed air pipeline. The pipeline is equipped with a DN15 shut-off valve and a pressure reducing valve, with the pressure reducing valve's outlet pressure set to 0.3MPa. The drive cylinder for the local extrusion mechanism is a pneumatic-hydraulic booster cylinder with a 100mm diameter, a pressure ratio of 5:1, a maximum output force of 50kN, and a working stroke of 100mm. The pressure sensor is a spoke-type tension / compression sensor with a range of 100kN and an accuracy of 0.5. The extrusion push rod is made of 3Cr2W8V hot-work die steel, with a diameter of 20mm and a total length of 350mm. The lower end contoured pressure head has a diameter of 22mm and a height of 8mm. The surface is coated with a 0.2mm thick titanium nitride coating using physical vapor deposition, with a coating hardness of HV2000 or higher and a friction coefficient ≤0.3. The displacement sensor is a rod-type linear displacement sensor with a range of 100mm and a linear accuracy of 0.1%. The fixed crossbeam is a box-shaped structure welded from No. 45 steel with a cross-section of 200mm×150mm. The top of the two columns of the formwork is horizontally erected. The columns are made of 100mm×100mm square steel and the column spacing is 600mm. Example

[0038] This embodiment describes the complete process for producing aluminum-magnesium alloy motor end caps using this device and process. An Al-Mg5 series aluminum-magnesium alloy is used, specifically composed of Mg 5.0%, Mn 0.45%, Si 0.3%, Ti 0.15%, Be 0.008%, with the balance being Al. The raw materials are pure aluminum ingots, pure magnesium ingots, Al-Mn20 master alloy, Al-Si20 master alloy, Al-Ti5 master alloy, and Al-Be3 master alloy, proportioned together. Melting process: First, pure aluminum ingots are added to a holding furnace 1 and heated to 740℃ for melting. Then, Al-Mn, Al-Si, and Al-Ti master alloys are added sequentially, stirred evenly, and then pure magnesium ingots are added. The magnesium ingots are pressed into the bottom of the molten metal using a bell jar to prevent combustion. Finally, the Al-Be master alloy is added. After the composition is adjusted, an Al-Ti-B modifier, Ti5%B1%, is added at 1.0% of the alloy mass. The modifier is pressed into the lower part of the molten metal using a bell jar for slow melting.

[0039] The melt preparation temperature was controlled at 740℃. After reaching the temperature, the ultrasonic vibrator 11 (1.5kW power) and the inert gas jet pipe 12 (argon flow rate 8L / min) were activated for combined degassing for 12 minutes. During the degassing process, the ultrasonic vibration caused the melt to produce a strong acoustic flow and cavitation effect. Argon microbubbles rose from the bottom and adsorbed hydrogen and oxide inclusions. After degassing, the gas content of the melt was measured to be 0.12mL / 100g by the reduced pressure solidification method. The slag on the surface of the melt was cleaned with a slag remover. Mold preheating parameters: the upper mold 31 temperature controller was set to 340℃, and the actual cavity surface temperature was 335℃; the lower mold 32 temperature controller was set to 300℃, and the actual cavity surface temperature was 295℃; the upper two sets of channels of the side mold 33 were set to 310℃, and the lower two sets were set to 335℃. The actual temperature gradient from top to bottom on the side mold cavity surface was 305℃~330℃. The mold preheating time is 35 minutes. After the temperature of each part stabilizes, the mold is closed. The mold closing force is 630kN, and the side mold closing force is 100kN per side.

[0040] Pulse filling parameters: reference pressure 30 kPa, pulse frequency 1.5 Hz, duty cycle 50%, trapezoidal waveform, pressure amplitude fluctuation ±15%. Filling time 12 s, average molten metal rising speed 100 mm / s. During filling, the pressure transmitter provides real-time feedback, and the PID-controlled proportional valve 42 maintains the pressure deviation within ±0.8 kPa. After filling, the pressure increases to 75 kPa and is held for 16 s. Local extrusion trigger: a temperature sensor detects the temperature of the thickest part of the bearing chamber. The solidus temperature of this alloy is approximately 580℃. Extrusion is triggered when the temperature drops to 605℃, 25℃ above the solidus temperature. The extrusion pusher descends at a speed of 22 mm / s, with an extrusion force of 30 kN, an extrusion depth of 12 mm, and retraction after 5 s holding. The pressure sensor reports an actual extrusion force of 29.5–30.8 kN, and the displacement sensor reports an actual extrusion depth of 11.8 mm. The control accuracy meets the requirements. Cooling parameters: After depressurization, the molten liquid reflux time in riser pipe 21 is approximately 3 seconds. Temperature control channel 34 switches to 25℃ cooling water at a cooling rate of 4.5℃ / s. The casting cools to 200℃ in approximately 90 seconds. During the cooling process, infrared thermography monitors the surface temperature of the casting, with the highest temperature of 405℃ not exceeding the 420℃ threshold. After mold opening, the casting surface is smooth, without cold shuts or incomplete filling defects. Heat treatment parameters: The casting is placed in a bogie-type heat treatment furnace and heated to 540℃ at a heating rate of 100℃ / h, held for 5 hours for solution treatment. After being removed from the furnace, it is quickly transferred to 70℃ water for quenching, with a transfer time of 12 seconds. After quenching, it is immediately transferred to an aging furnace, heated to 170℃ and held for 7 hours for artificial aging, and then air-cooled after removal from the furnace. Final casting performance testing: tensile strength 295MPa (sampling location: bearing housing mounting boss), yield strength 175MPa, elongation 9.5%, Brinell hardness 95HBW, porosity 0.35%, X-ray flaw detection according to GB / T11346, dimensional accuracy CT6 grade according to GB / T6414, yield 96%.

[0041] Comparative Example 1: This comparative example uses a traditional constant-pressure low-pressure casting process. The apparatus does not include an ultrasonic vibrator 11, an inert gas injection pipe 12, or a smooth, straight-through riser pipe 21 without a protective sleeve 22. The mold uses an integral cooling channel and lacks a local extrusion mechanism. Process parameters: constant filling pressure 30 kPa, filling time 12 s, holding pressure 75 kPa for 16 s, overall mold preheating 320°C, and other alloy composition and heat treatment parameters are the same as in Example 3. Final test results: Three shrinkage defects with a maximum diameter of 1.2 mm were found in the thickest part of the bearing chamber of the casting. The porosity was 1.8%, tensile strength was 235 MPa, yield strength was 145 MPa, elongation was 5.2%, and the yield was 78%. The comparison shows that without the five core measures of combined degassing, pulse filling, inert gas protection, zoned temperature control, and local extrusion, the internal quality and mechanical properties of the casting significantly decreased.

[0042] Comparative Example 2: This comparative example uses pulse filling but omits a local extrusion mechanism. The device includes ultrasonic degassing, inert gas protection, a riser pipe 21, a spiral guide groove 24, and zoned temperature control of the mold. The filling uses pulsed gas pressure parameters similar to Example 3, but local extrusion is not performed on the thicker parts. Final test results: Microscopic shrinkage porosity was observed in the thicker parts of the bearing chamber of the casting, with diffuse small black spots visible on X-ray inspection. The porosity was 0.9%, tensile strength was 260 MPa, yield strength was 158 MPa, elongation was 7.0%, and yield was 88%. The comparison shows that pulse filling and zoned temperature control can significantly improve filling quality and overall solidification, but shrinkage porosity in thicker parts still requires local extrusion to completely eliminate.

[0043] Comparative Example 3: This comparative example uses partial extrusion but the mold filling is constant pressure without inert gas protection. The device includes a partial extrusion mechanism, ultrasonic degassing, and mold zone temperature control, but the riser pipe 21 is a smooth straight pipe without a protective sleeve 22, and the mold filling uses a constant pressure of 30 kPa. Final test results: Pinhole defects exist on the surface and inside the casting, mainly distributed near the gate and on the upper surface; porosity is 1.2%; tensile strength is 255 MPa; yield strength is 155 MPa; elongation is 6.5%; and yield is 85%. The comparison shows that partial extrusion can improve the density of thick sections, but the constant pressure filling and lack of inert gas protection still cannot avoid air entrapment and oxidation defects.

[0044] The results of the three sets of comparative examples prove that the five technical features of the present invention—combined degassing, pulse filling, inert gas protection, zoned temperature control, and local extrusion—are indispensable. Only the synergistic effect of these five features can achieve the comprehensive technical effect of porosity ≤0.5%, tensile strength ≥280MPa, and yield ≥95%.

[0045] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

[0046] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A low-pressure casting processing device for an aluminum-magnesium alloy motor end cap, comprising a heat-holding melting furnace (1), a liquid lifting assembly (2), a mold assembly (3), a pulse air pressure system (4), and a local extrusion mechanism, characterized in that: The heat-insulating smelting furnace (1) is equipped with an ultrasonic vibrating rod (11) and an inert gas blowing pipe (12). The upper air chamber of the heat-insulating smelting furnace (1) is connected to the pulse air pressure system (4). The liquid lifting assembly (2) includes a liquid lifting pipe (21), a protective sleeve (22), an annular inert gas chamber (23), a spiral guide groove (24), and an air inlet connector (25). The inner wall of the liquid lifting pipe (21) is machined with a spiral guide groove (24). The protective sleeve (22) is coaxially sleeved on the outside of the liquid lifting pipe (21) to form an annular inert gas chamber (23). The air inlet connector (25) is connected to the annular inert gas chamber (23). The mold assembly (3) includes an upper mold (31), a lower mold (32), a side mold (33), a temperature control channel (34), and a sprue sleeve (35). The upper mold (31), the lower mold (32), and the side mold (33) together form a cavity. The sprue sleeve (35) is installed at the center of the lower mold (32) and connected to the riser pipe (21). The temperature control channel (34) is independently set inside the upper mold (31), the lower mold (32), and the side mold (33). The pulse air pressure system (4) includes an air storage tank (41), a proportional regulating valve (42) and a pulse solenoid valve (43). The air outlet of the air storage tank (41) is connected to the proportional regulating valve (42) and the pulse solenoid valve (43) in sequence and then connected to the air chamber of the heat preservation melting furnace (1). The local extrusion mechanism is equipped with an extrusion push rod, a drive cylinder, a pressure sensor and a displacement sensor. The drive cylinder drives the extrusion push rod to penetrate the thick part of the upper mold (31) cavity. The pressure sensor and the displacement sensor detect the extrusion force and displacement respectively.

2. The low-pressure casting processing device for aluminum-magnesium alloy motor end caps according to claim 1, characterized in that: The ultrasonic vibrating rod (11) and the inert gas blowing pipe (12) are arranged at 90° intervals in the circumferential direction of the furnace cover. The vibrating head of the ultrasonic vibrating rod (11) is immersed 120-180 mm below the surface of the molten liquid. The axis is parallel to the axis of the heat-preserving smelting furnace (1) and the distance between them is 60-80 mm. The lower end of the inert gas blowing pipe (12) extends to 20-30 mm above the bottom of the crucible. The gas outlet end is equipped with porous graphite balls with evenly distributed blowing holes of 0.3-0.8 mm in diameter on the surface of the balls.

3. The low-pressure casting processing device for aluminum-magnesium alloy motor end caps according to claim 1, characterized in that: The riser tube (21) is a straight circular tube made of silicon nitride ceramic material. Its lower end is inserted 80-120mm below the surface of the molten liquid, and its upper end is connected to the gating sleeve (35). The lead of the spiral guide groove (24) is 1.5-3 times the inner diameter of the riser tube (21), and the groove depth is 2-5mm. The width of the annular inert gas chamber (23) is 15-25mm. The gas inlet connector (25) is connected to the argon gas source through a flexible hose.

4. The low-pressure casting processing device for an aluminum-magnesium alloy motor end cover according to claim 1, characterized in that: The internal temperature control channel (34) of the lower mold (32) is a double ring structure. The inner ring is 10-20 mm away from the outer wall of the sprue sleeve (35), and the outer ring is 20-30 mm away from the inner ring. The internal temperature control channel (34) of the side mold (33) is a serpentine structure arranged at equal intervals from top to bottom. The internal temperature control channel (34) of the upper mold (31) is an Archimedean spiral structure. Each group of temperature control channels (34) is connected to an independent mold temperature controller.

5. The low-pressure casting processing device for an aluminum-magnesium alloy motor end cover according to claim 1, characterized in that: The proportional regulating valve (42) has an adjustment range of 0 to 0.1 MPa. The pulse solenoid valve (43) opens and closes rapidly at a frequency of 0.5 to 3 Hz to superimpose the reference pressure to form a periodic pulse pressure. The pulse air pressure system (4) also includes a controller and a pressure transmitter. The detection end of the pressure transmitter extends into the gas chamber of the heat preservation melting furnace (1), and the signal output end is connected to the controller. The output end of the controller is connected to the proportional regulating valve (42) and the pulse solenoid valve (43) respectively to form a pressure closed loop.

6. The low-pressure casting process for an aluminum-magnesium alloy motor end cover according to claim 1, characterized in that: The driving cylinder is a gas-liquid booster cylinder. The pressure sensor is a spoke-type tension and pressure sensor connected in series between the piston rod of the driving cylinder and the extrusion push rod. The displacement sensor is a pull rod type linear displacement sensor. The end of the pull rod is connected to the side wall of the extrusion push rod. The lower end of the extrusion push rod is provided with a contoured pressure head. The surface of the pressure head is coated with a 0.1-0.3mm thick titanium nitride coating. The mold assembly (3) is also provided with a temperature sensor. The temperature measuring end is close to the inner wall of the thick part of the cavity, and the signal output end is connected to the controller.

7. A low-pressure casting process for an aluminum-magnesium alloy motor end cap, using the low-pressure casting apparatus for an aluminum-magnesium alloy motor end cap as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Melt preparation: Add aluminum-magnesium alloy raw materials to the heat-insulating melting furnace (1) and heat to melt. Raise the temperature to 720-760℃ and start the ultrasonic vibrating rod (11) and the inert gas blowing pipe (12) to degas for 8-15 minutes. S2, Mold preheating: Heating medium is introduced into the temperature control channels (34) of the upper mold (31), lower mold (32) and side mold (33) respectively by independent mold temperature controller. The upper mold (31) is preheated to 320-360℃, the lower mold (32) is preheated to 280-320℃, and the side mold (33) is preheated to 300-340℃. S3, Pulse liquid filling: The pulse gas pressure system (4) applies a pulse pressure of 25-35 kPa to the gas chamber of the heat-insulating melting furnace (1), with a pulse frequency of 0.5-3 Hz. The molten liquid fills the mold cavity through the liquid riser pipe (21) at a speed of 80-120 mm / s, and the filling time is 8-15 s. S4, Pressure-increasing crystallization: After filling the mold, the pressure in the gas chamber is increased to 60-90 kPa and held for 12-20 seconds. The molten liquid in the riser pipe (21) is used to replenish the casting. S5. Local extrusion and compensation: When the temperature sensor detects that the temperature of the molten metal in the thick part drops to 15-30°C above the solidus line, the controller triggers the drive cylinder to push the extrusion push rod downward at 15-30 mm / s, applying an extrusion force of 20-40 kN, holding the pressure for 3-6 seconds, and then retracting. S6, Depressurization and Cooling: Release the pressure in the air chamber, the unsolidified molten liquid in the riser pipe (21) flows back, the temperature control channel (34) switches the cooling medium, and cools the casting to 180-220°C at a rate of 3-6°C / s; S7. Mold opening and part removal: The upper mold (31) rises to open the mold, the side mold (33) pulls the core horizontally, and the ejection mechanism ejects the casting from the lower mold (32); S8. Heat treatment: Solution treatment of castings at 530-550℃ for 4-6 hours, quenching transfer time ≤15s, water quenching at 60-80℃, aging treatment at 160-180℃ for 6-8 hours.

8. The low-pressure casting process for an aluminum-magnesium alloy motor end cover according to claim 7, characterized in that: In step S1, the aluminum-magnesium alloy composition by mass percentage is Mg 4.5%–5.5%, Mn 0.3%–0.6%, Si 0.2%–0.4%, Ti 0.1%–0.2%, Be 0.005%–0.01%, with the balance being Al. An Al-Ti-B modifier is added during the melt preparation process, with an addition amount of 0.8%–1.2% of the alloy mass. After degassing, the gas content of the melt is ≤0.15mL / 100g.

9. The low-pressure casting process for an aluminum-magnesium alloy motor end cover according to claim 7, characterized in that: In step S3, the pulsed air pressure waveform is a trapezoidal wave with a pulse frequency of 1-2 Hz, a duty cycle of 30%-70%, and a pressure amplitude fluctuation of ±15% of the reference pressure. In step S6, the surface temperature of the casting is monitored by an infrared temperature measuring device. When the surface temperature of the casting exceeds 420°C, the controller automatically increases the flow rate of the cooling medium.

10. The low-pressure casting process for an aluminum-magnesium alloy motor end cover according to claim 7, characterized in that: In step S5, the extrusion stroke of the extrusion pusher is 5-20mm, the extrusion pressure is fed back in real time by a pressure sensor, and the extrusion depth is fed back in real time by a displacement sensor. When the extrusion pressure reaches the set value or the displacement reaches the set stroke, the controller automatically stops the extrusion and holds the pressure. In step S8, the solution treatment heating rate is 80-120℃ / h. The final casting has a tensile strength ≥280MPa, a yield strength ≥160MPa, an elongation ≥8%, a porosity ≤0.5%, and a dimensional accuracy of CT6 grade.