By improving the wettability of ceramics/metals through 3D printing and current-assisted low-pressure infiltration, and combining it with vacuum high-temperature vibration and heat treatment, the problem of fabricating complex components of ceramic/metal composite materials has been solved, realizing the fabrication of complex components with high specific stiffness and high specific strength, meeting the requirements of lightweighting and high precision.

CN123149387APending Publication Date: 2026-11-24HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611330563.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies face challenges in preparing complex components from ceramic/metal bicontinuous composite materials, including poor wettability between ceramics and metals, low interfacial bonding strength, damage to porous ceramic skeletons caused by high-pressure infiltration, difficulty in handling internal pore structures by traditional machining, and metal loss from micron-level pores due to high-temperature melting methods. These challenges make it difficult to prepare complex components with high specific stiffness and high specific strength.

Method used

By 3D printing a porous ceramic skeleton and covering it with a silica layer, combined with an electric current-assisted low-pressure infiltration process, wettability is improved. The molten metal in the millimeter-scale pores is selectively removed by vacuum high-temperature vibration, and the internal mechanical support network is optimized by combining solution treatment and aging treatment.

Benefits of technology

The fabrication of complex ceramic/metal bicontinuous components with high specific stiffness and high specific strength has been achieved, meeting the performance requirements of lightweight and high-precision complex components, avoiding high-pressure damage and defects of traditional processing, and ensuring the structural integrity and mechanical properties of the components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149387A_ABST
    Figure CN123149387A_ABST
Patent Text Reader

Abstract

The application provides a ceramic / metal bicontinuous composite material and a preparation method of a complex component, and relates to the technical field of composite material preparation. The preparation method of the ceramic / metal bicontinuous complex component comprises the following steps: 3D printing a porous ceramic framework; pretreating the porous ceramic framework so that the surface of the porous ceramic framework is covered with a silicon dioxide layer; placing the porous ceramic framework covered with the silicon dioxide layer and metal into a mold; under vacuum conditions, performing pressure infiltration and introducing an electric current; maintaining the temperature above the melting point of the metal for more than 10 min, so that the metal liquid fully infiltrates into and fills the millimeter-level pores and micrometer-level pores of the porous ceramic framework, and is cooled and solidified; under vacuum conditions, maintaining the temperature above the melting point of the metal, and applying a shock force, so that the metal liquid in the millimeter-level pores of the porous ceramic framework is automatically discharged, and the metal liquid is retained in the micrometer-level pores; performing solid solution treatment and aging treatment, and obtaining the ceramic / metal bicontinuous complex component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite material preparation technology, and more specifically, to a method for preparing a ceramic / metal bicontinuous composite material and complex components. Background Technology

[0002] In the development of high-end equipment, lightweight structural design plays a decisive role in improving aircraft performance. Next-generation aircraft place dual demands on structural components, requiring materials to possess both high specific stiffness and high specific strength, and to be capable of precision forming of complex configurations such as topology optimization. Ceramic / metal bicontinuous composite materials, possessing both the high stiffness of the ceramic phase and the toughness of the metallic phase, have become an ideal material system to meet these requirements. However, existing technologies face multiple bottlenecks in the fabrication of such complex components: First, the poor natural wettability between ceramics and metals leads to low interfacial bonding strength. Conventional pressure infiltration processes require high pressures of over 5 MPa to achieve metal molten infiltration, but the porous ceramic skeletons prepared by 3D printing have insufficient structural strength after debinding and sintering. In particular, thin-walled or frame-type complex structures are prone to mechanical damage under high pressure. Second, traditional machining methods are difficult to process components with complex internal pore structures, which can easily cause internal material damage and are costly. Furthermore, to achieve lightweight topological structures, it is necessary to selectively remove the metal matrix in millimeter-level pores. However, existing high-temperature melting methods can lead to the simultaneous loss of metal in micrometer-level pores due to wettability issues, resulting in a decrease in material density and deterioration of mechanical properties. Summary of the Invention

[0003] This invention aims to address the significant bottlenecks in both material preparation and component processing in engineering applications, particularly in the fabrication of complex structural components (such as thin-walled structures and topological structures) using composite materials. It also highlights the difficulty in achieving the fabrication of complex ceramic / metal components with high specific stiffness and high specific strength.

[0004] To address the above problems, this invention provides a method for preparing ceramic / metal bicontinuous composite materials and complex components.

[0005] In a first aspect, the present invention provides a method for preparing a ceramic / metal dual-continuous complex component, comprising the following steps: S1: 3D printed porous ceramic skeleton; S2: Pre-treat the porous ceramic skeleton to cover the surface of the porous ceramic skeleton with a silicon dioxide layer; S3: Place the porous ceramic skeleton covered with a silica layer and the metal into a mold, perform pressure impregnation under vacuum and introduce current, keep it at a temperature above the metal melting point for more than 10 minutes, so that the molten metal can fully penetrate into and fill the millimeter-level and micrometer-level pores of the porous ceramic skeleton, cool and solidify, so that the silica layer and the metal can react in situ to improve wettability. S4: Under vacuum conditions, the metal is kept at a temperature above its melting point and subjected to vibration to allow the molten metal to drain autonomously from the millimeter-sized pores of the porous ceramic framework, while retaining the molten metal in the micrometer-sized pores. S5: Perform solution treatment at 450 ℃ to 500 ℃ and hold for more than 2 hours; perform aging treatment at 150 ℃ to 200 ℃ and hold for more than 7 hours to obtain a ceramic / metal bicontinuous complex component.

[0006] Optionally, in S3, pressure impregnation is performed using a micro-pressure of no more than 3 MPa.

[0007] Optionally, in S2, the pretreatment can be as follows: immersing the porous ceramic skeleton in an alkaline tetraethyl orthosilicate solution, drawing a vacuum, keeping it at 35 ℃ to 45 ℃ for more than 24 hours, cleaning and drying, so that the surface of the porous ceramic skeleton is covered with a silica layer.

[0008] Optionally, step 3 also includes the step of removing the binder from the porous ceramic skeleton introduced during the 3D printing process.

[0009] Optionally, in S2, the step of removing the binder from the porous ceramic skeleton includes: heating to 200 to 300 °C at a rate of 0.1 °C / min to 0.3 °C / min and holding for at least 4 hours; heating to 400 to 500 °C at a rate of 0.1 °C / min to 0.3 °C / min and holding for at least 4 hours; and heating to 550 to 650 °C at a rate of 0.1 °C / min to 0.3 °C / min and holding for at least 2 hours.

[0010] Optionally, in S3 and S4, the temperature above the metal melting point is 650 °C to 800 °C.

[0011] Optionally, in S4, the acceleration of the oscillating force is no greater than 10 G.

[0012] Optionally, in S1, the porous ceramic skeleton is heated to 1500 ℃ to 2000 ℃ to improve the skeleton strength of the porous ceramic skeleton.

[0013] Secondly, the present invention provides a method for preparing a ceramic / metal bicontinuous composite material. Includes the following steps: T1: 3D printed porous ceramic skeleton; T2: Pre-treat the porous ceramic skeleton to cover the surface of the porous ceramic skeleton with a silicon dioxide layer; T3: The porous ceramic skeleton covered with a silica layer and the metal are placed in a mold. Under vacuum conditions, pressure impregnation is performed and an electric current is introduced. The temperature is kept at a temperature above the melting point of the metal for more than 10 minutes, so that the molten metal can fully penetrate into and fill the millimeter-level and micrometer-level pores of the porous ceramic skeleton. After cooling and solidification, the silica layer and the metal react in situ to improve wettability. T4: Solution treatment is performed at 450 ℃ to 500 ℃ for more than 2 hours; aging treatment is performed at 150 ℃ to 200 ℃ for more than 7 hours to obtain a ceramic / metal bicontinuous composite material. Optionally, the flexural strength of the ceramic / metal bicontinuous composite material reaches more than 280 MPa and the specific strength reaches more than 93 N·m / kg.

[0014] The beneficial effects of the method for preparing ceramic / metal bicontinuous composite materials and complex components of the present invention are as follows: A porous ceramic skeleton with a complex configuration is prepared using 3D printing technology, and its surface is pretreated with a silica layer. Combined with an current-assisted low-pressure infiltration process, an in-situ reaction occurs between the silica layer and the metal, effectively improving the wettability between the ceramic and the metal, reducing the infiltration pressure, and avoiding damage to the ceramic skeleton under high pressure. Furthermore, the molten metal in millimeter-level pores is selectively removed by vacuum high-temperature vibration, while retaining the molten metal in micrometer-level pores, achieving lightweighting of the complex component and optimization of the internal mechanical support network. Finally, after solution treatment and aging, a ceramic / metal bicontinuous complex component with both high specific stiffness and high specific strength is obtained, meeting the performance requirements for lightweight load-bearing structures and high-precision complex components. Attached Figure Description

[0015] Figure 1 This is a schematic flowchart of a method for preparing a ceramic / metal dual-continuous complex component according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the 3D-printed porous silicon carbide skeleton of Example 1; Figure 3 This is a schematic diagram of the microstructure of the 3D-printed porous silicon carbide framework in Example 1. Figure 4 This is a schematic diagram of the silicon carbide / aluminum dual continuous complex component of Example 1; Figure 5 This is a schematic diagram of the microstructure of the silicon carbide / aluminum dual continuous complex component of Example 1; Figure 6 This is a schematic diagram of the silicon carbide / aluminum dual continuous complex component in Comparative Example 1. Figure 7 This is a schematic diagram of the pulverization of a silicon carbide / aluminum dual continuous complex component as shown in Comparative Example 1. Detailed Implementation

[0016] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Although some embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the accompanying drawings and embodiments of the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention.

[0017] Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this invention's description is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "comprising" and its variations as used herein are open-ended inclusion, meaning "including but not limited to"; the term "based on" means "at least partially based on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one additional embodiment"; the term "some embodiments" means "at least some embodiments"; and the term "optionally" means "optional embodiments". Definitions of other terms will be given in the description below.

[0018] In related technologies, traditional ceramic / metal composite materials face significant bottlenecks in both material preparation and component processing when fabricating complex structural components. Specifically, poor wettability between ceramics and metals leads to weak interfacial bonding and low material performance; the pressure infiltration method requires high infiltration pressure, which can easily cause the porous ceramic skeleton printed in 3D to crush during the infiltration process; at the same time, in order to achieve the topological structure processing of complex components, it is necessary to remove excess metal matrix from the composite material, but traditional machining is difficult and costly, and is prone to internal damage, while high-temperature melting methods can cause the internal molten metal to flow out, resulting in defects. Therefore, it is impossible to achieve the precise fabrication of complex ceramic / metal bicontinuous structures with high specific stiffness and high specific strength.

[0019] To address the problems existing in the aforementioned related technologies, embodiments of the present invention provide a ceramic / metal bicontinuous complex component and its preparation method.

[0020] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a ceramic / metal bicontinuous composite material and a complex component, comprising the following steps: S1: 3D printed porous ceramic skeleton; S2: Pre-treat the porous ceramic skeleton to cover the surface of the porous ceramic skeleton with a silicon dioxide layer; S3: Place the porous ceramic skeleton covered with a silica layer and the metal into a mold, perform pressure impregnation under vacuum and introduce current, keep it at a temperature above the metal melting point for more than 10 minutes, so that the molten metal can fully penetrate into and fill the millimeter-level and micrometer-level pores of the porous ceramic skeleton, cool and solidify, so that the silica layer and the metal can react in situ to improve wettability. S4: Under vacuum conditions, the metal is kept at a temperature above its melting point and subjected to vibration to allow the molten metal to drain autonomously from the millimeter-sized pores of the porous ceramic framework, while retaining the molten metal in the micrometer-sized pores. S5: Perform solution treatment at 450 ℃ to 500 ℃ and hold for more than 2 hours; perform aging treatment at 150 ℃ to 200 ℃ and hold for more than 7 hours to obtain a ceramic / metal bicontinuous complex component.

[0021] Specifically, the current is the directional current applied by the instrument. Applying the current can activate the sample, and the directional current can promote ion movement. Metal ions migrate directionally to the reaction interface and are introduced into the impregnation process. Its role is to assist in promoting the in-situ reaction between the silica layer and the molten metal, further optimize the interface wettability, and reduce the required impregnation pressure.

[0022] In-situ reaction refers to the chemical reaction that occurs directly between components under specific conditions during the material preparation process, forming new compounds or improving the interfacial bonding state, rather than through pre-synthesis and then mixing.

[0023] Solution treatment is a heat treatment process that involves heating an alloy to its solution temperature and holding it at that temperature to allow the alloying elements to fully dissolve in the matrix and form a homogeneous solid solution. The alloy is then rapidly cooled to maintain the solid solution state, laying the foundation for subsequent aging treatment.

[0024] Aging treatment is a heat treatment process following solution treatment. By holding the solution at a low temperature for a long time, supersaturated solute atoms in the solid solution precipitate out to form a finely dispersed precipitate phase, thereby improving the strength and hardness of the material.

[0025] In step S3, the mold is evacuated to remove gas from the pores, preventing gas retention from affecting the impregnation effect. Under vacuum, the metal is heated to melt, and an electric current is introduced to assist the impregnation process. At this time, a certain external pressure is applied, such as mechanical pressure, to force the molten metal to fully penetrate into the millimeter- and micrometer-sized pores within the porous ceramic framework. The temperature is maintained above the metal's melting point for at least 10 minutes to ensure that the molten metal fully fills all pores and allows the silica layer to react in situ with the molten metal, effectively improving the wettability between them. After impregnation, the mixture is cooled and solidified to form a ceramic / metal composite material.

[0026] In step S4, an vibrational force is applied to the composite material. This vibration can be generated by a mechanical vibration device or an ultrasonic generator, causing the molten metal to be autonomously discharged from the millimeter-scale pores of the porous ceramic framework under the vibrational action. Due to the capillary forces within the micrometer-scale pores and the improved interfacial wettability, the molten metal can be retained in these tiny pores, thereby achieving selective removal of metal from macropores.

[0027] In this embodiment, a porous ceramic framework with a complex configuration is fabricated using 3D printing technology. The surface of the framework is pretreated with a silica layer, and combined with an current-assisted low-pressure infiltration process, an in-situ reaction occurs between the silica layer and the metal, effectively improving the wettability between the ceramic and metal, reducing the infiltration pressure, and preventing damage to the framework. Furthermore, molten metal is selectively removed from millimeter-level pores by vacuum high-temperature vibration, while retaining molten metal in micrometer-level pores, achieving lightweighting of the complex component and optimization of the internal mechanical support network. Finally, after solution treatment and aging, a ceramic / metal bicontinuous complex component with both high specific stiffness and high specific strength is obtained, meeting the performance requirements for lightweight load-bearing structures and high-precision complex components.

[0028] Optionally, in S3, pressure impregnation is performed using a micro-pressure of no more than 3 MPa.

[0029] In this optional embodiment, limiting the pressure value during the pressure infiltration process to a micro-pressure range not exceeding 3 MPa significantly reduces the mechanical stress load on the 3D-printed porous ceramic skeleton. In traditional pressure infiltration methods, due to the poor wettability between ceramics and metals, high pressures (>10 MPa) are often required to ensure sufficient metal infiltration. However, for porous ceramic skeletons with thin walls or complex topologies prepared by 3D printing, excessively high infiltration pressure can easily lead to deformation, cracking, or even complete destruction of the skeleton, severely affecting the structural integrity and performance of the final component. This application significantly improves the wettability between ceramics and metals by covering the surface of the porous ceramic skeleton with a silica layer in step S2 and introducing current assistance in step S3 to promote an in-situ reaction between the silica layer and the metal. Furthermore, using a micro-pressure not exceeding 3 MPa for infiltration allows the molten metal to fully infiltrate and fill the millimeter- and micrometer-sized pores of the porous ceramic skeleton even under relatively low external pressure. This synergistic effect not only effectively avoids structural damage to the complex ceramic skeleton caused by high-pressure infiltration and ensures the precise forming of the component, but also ensures the full filling of the molten metal and the compactness of the material, thus successfully preparing a complex ceramic / metal bicontinuous component with high structural integrity and excellent mechanical properties.

[0030] Optionally, in S2, the pretreatment includes: immersing the porous ceramic skeleton in an alkaline tetraethyl orthosilicate solution, evacuating, keeping it at 35 ℃ to 45 ℃ for more than 24 hours, cleaning and drying, so that the surface of the porous ceramic skeleton is covered with a silica layer.

[0031] Specifically, the porous ceramic framework is impregnated in an alkaline tetraethyl orthosilicate solution to introduce a silica precursor onto the surface of the ceramic framework through a chemical reaction. The alkaline environment effectively catalyzes the hydrolysis and polycondensation reactions of tetraethyl orthosilicate, thereby forming a silica gel on the framework surface. Vacuum treatment is used to remove air from the pores inside the porous ceramic framework, ensuring that the impregnation solution can fully and uniformly penetrate into the deep pores of the framework, avoiding air bubbles hindering the wetting process. After the air inside the framework is expelled, the alkaline tetraethyl orthosilicate solution is introduced, allowing the solution to wet the framework under vacuum or low pressure. Holding at 35°C to 45°C for more than 24 hours allows for precise control of the hydrolysis and polycondensation reaction rates of tetraethyl orthosilicate, ensuring that the silica layer can be uniformly and densely deposited on the surface of the ceramic framework and form a good bond with it.

[0032] In this optional embodiment, a dense and well-bonded silica layer can be efficiently and uniformly formed on the surface of a complex porous ceramic framework, laying a solid foundation for the in-situ reaction between the silica layer and the metal in the subsequent step S3 to improve wettability. This not only significantly improves the wettability between the ceramic and the metal and reduces the pressure required for molten metal infiltration, but also ensures the uniformity and stability of the interfacial bonding, thereby effectively avoiding the problem of uneven improvement in interfacial wettability caused by improper pretreatment, and thus improving the overall performance of the finally prepared ceramic / metal bicontinuous complex component.

[0033] Optionally, step S3 may also include: removing the binder from the porous ceramic skeleton introduced during the 3D printing process.

[0034] Specifically, it involves thoroughly removing the organic binder introduced into the porous ceramic framework during the 3D printing process. Removing the binder is crucial for the smooth execution of subsequent processes and for improving the performance of the final component.

[0035] In this optional embodiment, the problem of residual binder decomposing or vaporizing during subsequent high-temperature infiltration, resulting in pores or defects within the ceramic skeleton and severely affecting the density and interfacial bonding quality of the composite material, is effectively solved. Specifically, thoroughly removing the binder ensures that the porous ceramic skeleton is in a pure state before entering the metal infiltration stage, preventing organic matter from generating gas under the action of high-temperature molten metal and forming pores or inclusions. This not only keeps the pore channels of the ceramic skeleton unobstructed, providing a good physical basis for the subsequent molten metal to smoothly fill millimeter- and micrometer-sized pores with current assistance, but also effectively improves the bonding strength between the ceramic and metal interfaces. Therefore, this step avoids internal defects caused by the decomposition of organic matter, thus ensuring that the ceramic / metal bicontinuous component can obtain a uniform and dense microstructure after subsequent solution treatment and aging, providing a key process guarantee for achieving the performance goals of high specific strength and high specific stiffness. Through this technical solution, the final prepared ceramic / metal bicontinuous complex component has a denser internal structure and a stronger interfacial bond, thereby significantly improving the overall mechanical properties and reliability of the component.

[0036] Optionally, in S2, the step of removing the binder from the porous ceramic skeleton includes: heating to 200 to 300 °C at a rate of 0.1 °C / min to 0.3 °C / min and holding for at least 4 hours; heating to 400 to 500 °C at a rate of 0.1 °C / min to 0.3 °C / min and holding for at least 4 hours; and heating to 550 to 650 °C at a rate of 0.1 °C / min to 0.3 °C / min and holding for at least 2 hours.

[0037] Specifically, the temperature is maintained between 200 °C and 300 °C for at least 4 hours. This stage primarily targets the initial decomposition of low molecular weight components and volatile organic compounds in the adhesive, ensuring these components have sufficient time to fully volatilize and exit the framework. Following this, the temperature is gradually increased to 400 °C to 500 °C at the same slow rate and maintained at this temperature for at least 4 hours. This stage aims to further decompose the main structure of the adhesive, ensuring that most polymer chains break down and that gaseous decomposition products can smoothly exit through the micron-sized pores of the framework, avoiding blockage or residue. Finally, the temperature is increased to 550 °C to 650 °C at a rate of 0.1 °C / min to 0.3 °C / min and maintained for at least 2 hours. This final high-temperature stage ensures that any residual carbonaceous materials or highly stable adhesive components are completely carbonized or volatilized, thus providing a clean, residue-free, and structurally intact ceramic framework channel for subsequent molten metal impregnation.

[0038] In this optional embodiment, slow heating effectively avoids excessive internal pressure in the skeleton caused by the rapid decomposition of the binder generating a large amount of gas, thereby preventing microcracks or deformation in the skeleton structure. The segmented temperature control strategy not only ensures the physical integrity of the porous ceramic skeleton, avoiding defects such as cracks and collapse caused by improper binder decomposition, but also ensures unobstructed flow of pores within the skeleton through thorough degreasing. This creates a favorable physicochemical environment for subsequent low-pressure infiltration of the molten metal, significantly improving the interfacial wettability between the ceramic and metal and promoting in-situ reactions. Ultimately, this helps to prepare dense, well-bonded, and mechanically superior ceramic / metal bicontinuous complex components, thereby effectively improving the overall performance and reliability of the composite material.

[0039] Optionally, in S3 and S4, the temperature above the metal melting point is 650 °C to 800 °C.

[0040] In this optional embodiment, the temperature during the infiltration process is precisely limited to the range of 650°C to 800°C, above the metal's melting point, providing a suitable thermodynamic environment for the interfacial reaction between ceramic and metal. Within this temperature range, the molten metal exhibits good fluidity, ensuring its smooth entry into the millimeter- and micrometer-sized pores of the porous ceramic framework. Simultaneously, the application of current within this temperature range effectively activates the in-situ reaction between the silica layer and the molten metal, thereby improving their wettability. By controlling the temperature within this specific range, it avoids both excessively low temperatures leading to excessively high molten metal viscosity that fails to fully fill the pores, and excessively high temperatures causing excessively low metal viscosity, mold sealing failure, and overly vigorous interfacial reactions resulting in excessive brittle phases. This lays a stable physicochemical foundation for subsequent process steps involving the removal of excess molten metal from the millimeter-sized pores through vibration and the retention of molten metal in the micrometer-sized pores, ensuring the structural integrity and mechanical properties of the final component.

[0041] Optionally, in S4, the acceleration of the oscillating force is no greater than 10 G.

[0042] In this optional embodiment, by precisely controlling the acceleration of the oscillation force to be no greater than 10 G, it can be ensured that the molten metal in millimeter-sized pores can be effectively discharged under vacuum and high-temperature conditions, while the molten metal in micrometer-sized pores can be retained. This is because in steps S2 and S3, the porous ceramic skeleton surface is coated with a silica layer through pretreatment, and the silica layer reacts in situ with the metal to improve wettability. Based on this, an appropriate oscillation force can overcome the surface tension and viscous resistance of the molten metal in the millimeter-sized pores, allowing it to flow out smoothly under gravity. At the same time, due to the relatively large capillary force in the micrometer-sized pores and the good wettability between the molten metal and the ceramic skeleton, the molten metal in the micrometer-sized pores can be stably retained in the skeleton under an acceleration of no more than 10 G, avoiding loss due to excessive oscillation. This precise limitation of the oscillation acceleration effectively solves the problem of damage to the ceramic skeleton structure or incomplete discharge of molten metal that may occur due to improper control of the oscillation force during vacuum and high-temperature oscillation. By controlling the acceleration to no more than 10 G, the excess molten metal in the millimeter-scale pores is fully drained while mechanical damage to the fragile 3D-printed porous ceramic framework is avoided, thus maintaining the structural integrity of the framework. Furthermore, it ensures the effective retention of molten metal in the micrometer-scale pores, guaranteeing the mechanical properties and structural density of the final ceramic / metal bicontinuous complex component. This precise control is a key process parameter for achieving high-performance, lightweight, and complex structural fabrication, resulting in components with excellent flexural strength and specific strength.

[0043] Optionally, in S1, the porous ceramic skeleton is heated to 1500 ℃ to 2000 ℃ to improve the skeleton strength of the porous ceramic skeleton.

[0044] In this optional embodiment, the 3D-printed porous ceramic skeleton undergoes high-temperature heat treatment, heating it to a temperature range of 1500 ℃ to 2000 ℃, thereby significantly improving the skeleton strength. This heating process promotes the growth and densification of sintering necks between ceramic particles, enhances the bonding force between particles, and enables the porous ceramic skeleton to maintain its porous structure while possessing higher mechanical load-bearing capacity. By pre-strengthening the skeleton strength, this technical solution effectively solves the structural damage problem that may occur in the porous ceramic skeleton during the subsequent pressure infiltration S3 and oscillation drainage S4 processes. In the pressure infiltration S3 step, the strengthened skeleton can effectively resist the extrusion force applied by the molten metal, avoiding deformation or breakage under low-pressure infiltration conditions. In the vacuum oscillation drainage S4 step, the strengthened skeleton can withstand the kinetic impact generated by high-frequency oscillation, ensuring that the molten metal in the millimeter-level pores can be smoothly drained, while the molten metal in the micrometer-level pores is retained, thereby ensuring the structural integrity of the final component and the expected bicontinuous structure. Therefore, by strengthening the porous ceramic framework with high temperature in S1, this application ensures the stability and reliability of the entire preparation process, providing a solid physical basis for finally obtaining a high-density, complex ceramic / metal bicontinuous complex component, and avoiding preparation failure or component performance degradation due to insufficient framework strength.

[0045] Another embodiment of the present invention provides a method for preparing a ceramic / metal bicontinuous composite material, comprising the following steps: T1: 3D printed porous ceramic skeleton; T2: Pre-treat the porous ceramic skeleton to cover the surface of the porous ceramic skeleton with a silicon dioxide layer; T3: The porous ceramic skeleton covered with a silica layer and the metal are placed in a mold. Under vacuum conditions, pressure impregnation is performed and an electric current is introduced. The temperature is kept at a temperature above the melting point of the metal for more than 10 minutes, so that the molten metal can fully penetrate into and fill the millimeter-level and micrometer-level pores of the porous ceramic skeleton. After cooling and solidification, the silica layer and the metal react in situ to improve wettability. T4: Solution treatment is performed at 450 ℃ to 500 ℃ for more than 2 hours; aging treatment is performed at 150 ℃ to 200 ℃ for more than 7 hours to obtain ceramic / metal bicontinuous composite material.

[0046] In this embodiment, a porous ceramic skeleton with a complex configuration is prepared using 3D printing technology, and its surface is pretreated with a silica layer. Combined with an current-assisted low-pressure infiltration process, an in-situ reaction occurs between the silica layer and the metal, effectively improving the wettability between the ceramic and the metal, reducing the infiltration pressure, and avoiding damage to the skeleton. After solution treatment and aging, a complex ceramic / metal bicontinuous component with both high specific stiffness and high specific strength is obtained, meeting the performance requirements for lightweight load-bearing structures and high-precision composite materials.

[0047] The ceramic and metallic phases interpenetrate in three-dimensional space, each forming a continuous network structure. Specifically, the porous ceramic framework prepared by 3D printing technology has millimeter- and micrometer-scale pore structures, with a uniform silica layer covering the surface. During the preparation process, an current-assisted low-pressure melting process is introduced, where the silica layer and molten metal react in situ under the action of current, significantly improving the wettability of the ceramic-metal interface. This allows the molten metal to fully penetrate into all pores at lower pressure, effectively avoiding damage to the ceramic framework caused by high pressure. Subsequently, a vacuum high-frequency oscillation method is used at temperatures above the metal's melting point to selectively remove excess molten metal from the millimeter-scale pores through oscillation force, while the molten metal in the micrometer-scale pores is retained due to capillary action. This achieves precise forming of complex topological shapes without damaging the internal structure. Finally, solution treatment and aging treatment further optimize the microstructure of the metal matrix, ensuring the high overall mechanical properties of the composite material.

[0048] Ceramic / metal bicontinuous composite materials not only possess excellent specific stiffness and specific strength, but also enable the precision fabrication of complex geometries. Due to the in-situ reaction between the silica layer and the molten metal, interfacial defects are effectively reduced, and interfacial bonding is significantly enhanced. This composite material is particularly suitable for core applications such as lightweight load-bearing structures in spacecraft and high-precision optical platforms. It can meet the comprehensive requirements of complex components such as mirrors in resisting gravitational deformation, maintaining high surface accuracy, and realizing topological structure design, providing an effective material solution for the high-performance of aerospace equipment.

[0049] Optionally, the flexural strength of the ceramic / metal bicontinuous composite material reaches 280 MPa or higher, and the specific strength reaches 93 N·m / kg or higher.

[0050] In this optional embodiment, the flexural strength of the ceramic / metal bicontinuous composite material reaches over 280 MPa. This indicates that the improved wettability achieved through the in-situ reaction between the silica layer and the metal in step T3, and the thorough penetration and filling of the micron-sized pores by the molten metal, results in a tight interfacial bond between the ceramic skeleton and the metal matrix. This effectively transfers stress under bending loads, preventing premature failure due to interfacial defects and ensuring the structural integrity and reliability of the composite material. The specific strength reaches over 93 N·m / kg, achieving significant weight reduction while maintaining structural load-bearing capacity. This quantitative definition of mechanical performance indicators not only verifies the effectiveness of the improved interfacial wettability and precise removal of excess molten metal in the aforementioned preparation process but also provides a clear performance benchmark for the engineering application of this type of composite material in demanding fields such as aerospace. It ensures that the composite material meets the design requirements of complex structures while possessing the reliability to withstand high-load environments, effectively solving the problems of difficulty in intuitively quantifying the final mechanical performance of components and the lack of clearly defined performance indicators.

[0051] The present invention will be further described below with reference to specific embodiments.

[0052] Example 1: Preparation of silicon carbide / aluminum dual continuous complex components.

[0053] 1. Prepare a silicon carbide ceramic slurry with 50% solid content, design the silicon carbide framework structure, and use 3D printing to fabricate the silicon carbide framework with the desired topology. After printing, remove the framework, dry it in an oven, and obtain a 3D printed porous silicon carbide framework, such as... Figure 2 As shown.

[0054] Microstructure of the prepared 3D printed porous silicon carbide framework Figure 3 As shown, there are continuous pores inside the skeleton.

[0055] 2. Immerse the 3D printed porous silicon carbide skeleton from step 1 into an alkaline tetraethyl orthosilicate solution, and evacuate the solution to fill the micron-sized pores with the reaction solution. Keep it at 40°C for 24 hours, then remove it, wash it with deionized water, and dry it in an oven. 3. Place the silicon carbide skeleton from step 2 into a muffle furnace and remove the binder from the silicon carbide skeleton using a segmented sintering process; heat to 200 ℃ at a rate of 0.1 ℃ / min and hold for more than 4 hours, heat to 400 ℃ at a rate of 0.1 ℃ / min and hold for more than 4 hours, and heat to 550 ℃ at a rate of 0.1 ℃ / min and hold for more than 2 hours.

[0056] 4. Place the silicon carbide skeleton obtained in step 3 into the graphite mold, place the 2024 aluminum block on the preform, seal it with flexible graphite paper to prevent the aluminum liquid from flowing out, place the preform in the groove of the graphite mold, and the graphite mold provides a certain support force to the aluminum block to prevent the silicon carbide skeleton from being compressed and damaged.

[0057] 5. Evacuate the sintering furnace to prevent oxidation during the preparation of composite materials.

[0058] 6. Apply directional current, heat to 700℃, apply vertical micro pressure of 1MPa, hold for 10 min, so that the aluminum liquid can fully penetrate into the micron-sized pores in the silicon carbide skeleton, and then cool and solidify with the furnace. 7. The composite material is placed in a vacuum sintering furnace, the device is heated to above 700°C, and high-frequency oscillation with an acceleration of 10 G is applied to remove the liquid aluminum in the millimeter-sized pores of the frame, resulting in a high-precision silicon carbide / aluminum-based composite frame. 8. The silicon carbide / aluminum-based composite frame obtained in step 7 is subjected to heat treatment. Solution treatment is performed at 496℃, followed by holding in a salt bath furnace for 2 hours, with a temperature error range of ±0.1℃. Aging treatment is then performed at 175℃, followed by holding in a constant temperature drying oven for 7 hours, with a temperature error range of ±1℃. This yields a lightweight, high-strength, high-precision, and highly dimensionally stable precision silicon carbide / aluminum dual-continuous complex component, such as… Figure 4 As shown in the attached figure, the microstructure of the precision silicon carbide / aluminum dual-continuous complex component is as follows. Figure 5 As shown.

[0059] A precision silicon carbide / aluminum dual continuous complex component was subjected to a three-point bending test, and the bending strength was found to be 280 MPa. The density of the precision silicon carbide / aluminum dual continuous complex component was determined by Archimedes' displacement method, and the specific strength was further calculated to be 93 N·m / kg.

[0060] Example 2: Preparation of silicon carbide / magnesium dual continuous complex components.

[0061] 1. Prepare a silicon carbide ceramic slurry with 50% solid content, design the silicon carbide skeleton structure, and use 3D printing to prepare the silicon carbide skeleton with the topological structure. After printing, remove the frame and put it in an oven to dry, and obtain a 3D printed porous silicon carbide skeleton.

[0062] 2. Place the silicon carbide skeleton from step 1 into a muffle furnace and remove the binder from the silicon carbide skeleton using a segmented sintering process; heat to 300 ℃ at a rate of 0.2 ℃ / min and hold for more than 4 hours, heat to 500 ℃ at a rate of 0.2 ℃ / min and hold for more than 4 hours, and heat to 650 ℃ at a rate of 0.2 ℃ / min and hold for more than 2 hours.

[0063] 3. Continue heating the silicon carbide skeleton from step 2 in a pressure furnace to 1700℃ to further improve the skeleton strength.

[0064] 4. Immerse the 3D printed porous silicon carbide skeleton from step 3 into an alkaline tetraethyl orthosilicate solution, and evacuate the vacuum to fill the micron-sized pores with the reaction solution. Keep it at 40°C for 24 hours, then remove it, wash it with deionized water, and dry it in an oven. 5. Place the silicon carbide skeleton obtained in step 4 into a graphite mold, place the magnesium block on the preform, and seal it with flexible graphite paper to prevent the magnesium liquid from flowing out. Place the preform in the groove of the graphite mold. The graphite mold provides a certain support force to the magnesium block to prevent it from being compressed and damaged.

[0065] 6. Evacuate the sintering furnace to prevent oxidation during the preparation of composite materials.

[0066] 7. Apply directional current, heat to 650℃, apply vertical micro pressure of 1MPa, hold for 10 min, so that the magnesium liquid can fully penetrate into the micron-sized pores in the silicon carbide skeleton, and then cool and solidify with the furnace. 8. The composite material is placed in a vacuum sintering furnace, the device is heated to above 650°C, and high-frequency oscillation with an acceleration of 10 G is applied to remove the magnesium liquid in the millimeter-scale large pores of the frame, so as to obtain a high-precision precision silicon carbide / magnesium-based composite frame. 9. The silicon carbide / magnesium-based composite frame obtained in step 8 is subjected to heat treatment. Solution treatment is performed at 496℃ and the frame is kept at a temperature in a salt bath furnace for 2 hours, with a temperature error range of ±0.1℃. Aging treatment is performed at 175℃ and the frame is kept at a temperature in a constant temperature drying oven for 7 hours, with a temperature error range of ±1℃. This yields a lightweight, high-strength, high-precision, and high-dimensional stability precision silicon carbide / magnesium dual continuous complex component.

[0067] Comparative Example 1: Preparation of silicon carbide / aluminum dual continuous complex components.

[0068] 1. Prepare a silicon carbide ceramic slurry with 50% solid content, design the silicon carbide framework structure, and use 3D printing to fabricate the silicon carbide framework with the desired topology. After printing, remove the framework, dry it in an oven, and obtain a 3D printed porous silicon carbide framework, such as... Figure 2 As shown.

[0069] Microstructure of the prepared 3D printed porous silicon carbide framework Figure 3 As shown, there are continuous pores inside the skeleton.

[0070] 2. Place the silicon carbide skeleton from step 1 into a muffle furnace and remove the binder from the silicon carbide skeleton using a segmented sintering process; heat to 200 ℃ at a rate of 0.1 ℃ / min and hold for more than 4 hours, heat to 400 ℃ at a rate of 0.1 ℃ / min and hold for more than 4 hours, and heat to 550 ℃ at a rate of 0.1 ℃ / min and hold for more than 2 hours.

[0071] 3. Place the silicon carbide skeleton obtained in step 2 into a graphite mold, place the 2024 aluminum block on the preform, and seal it with flexible graphite paper to prevent the aluminum liquid from flowing out. Place the preform in the groove of the graphite mold. The graphite mold provides a certain support force to the aluminum block to prevent it from being compressed and damaged.

[0072] 4. Evacuate the sintering furnace to prevent oxidation during the preparation of composite materials.

[0073] 5. Apply directional current, heat to 700℃, apply vertical micro pressure of 1MPa, hold for 10 min, so that the aluminum liquid can fully penetrate into the micron-sized pores in the silicon carbide skeleton, and then cool and solidify with the furnace. 6. The composite material is placed in a vacuum sintering furnace, the device is heated to above 700°C, and high-frequency oscillation with an acceleration of 10 G is applied to remove the liquid aluminum in the millimeter-sized pores of the frame, resulting in a high-precision silicon carbide / aluminum-based composite frame. 7. The silicon carbide / aluminum-based composite frame obtained in step 7 is subjected to heat treatment. Solution treatment is performed at 496℃, followed by holding in a salt bath furnace for 2 hours, with a temperature error range of ±0.1℃. Aging treatment is then performed at 175℃, followed by holding in a constant temperature drying oven for 7 hours, with a temperature error range of ±1℃. This yields a silicon carbide / aluminum dual-continuous complex component, such as... Figure 6 As shown.

[0074] Because Comparative Example 1 did not undergo pretreatment, the ceramic skeleton surface lacked a SiO2 layer. During the infiltration process, SiC and Al underwent an interfacial reaction to generate a large amount of Al4C3. The Al4C3 reacted with water in the air during storage and pulverized. After two months of storage... Figure 6 The sample shown was pulverized, and after pulverization, it resembled... Figure 7 As shown.

[0075] While the present invention has been disclosed above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and all such changes and modifications will fall within the scope of protection of the present invention.

Claims

1. A method for producing a ceramic / metal bicontinuous complex member, characterized by, Includes the following steps: S1: 3D printed porous ceramic skeleton; S2: Pre-treat the porous ceramic skeleton to cover the surface of the porous ceramic skeleton with a silicon dioxide layer; S3: The porous ceramic skeleton covered with the silica layer and the metal are placed in a mold. Under vacuum conditions, pressure impregnation is performed and an electric current is introduced. The temperature is kept above the melting point of the metal for more than 10 minutes to allow the molten metal to fully penetrate into and fill the millimeter-level and micrometer-level pores of the porous ceramic skeleton. The mixture is then cooled and solidified to allow the silica layer and the metal to react in situ to improve wettability. S4: Under vacuum conditions, the metal is kept at a temperature above its melting point and an vibration force is applied to allow the molten metal to be discharged autonomously from the millimeter-level pores of the porous ceramic skeleton, while the molten metal is retained in the micrometer-level pores. S5: Perform solution treatment at 450 ℃ to 500 ℃ and hold for more than 2 hours; perform aging treatment at 150 ℃ to 200 ℃ and hold for more than 7 hours to obtain a ceramic / metal bicontinuous complex component.

2. The method for producing a ceramic / metallic dual-continuous complex structure according to claim 1, characterized by, In step S3, pressure impregnation is performed using a micro-pressure of no more than 3 MPa.

3. The method of producing a ceramic / metallic dual-continuous complex structure according to claim 1, characterized by, In step S2, the pretreatment includes: immersing the porous ceramic skeleton in an alkaline tetraethyl orthosilicate solution, evacuating, keeping it at 35°C to 45°C for more than 24 hours, cleaning and drying, so that the surface of the porous ceramic skeleton is covered with the silicon dioxide layer.

4. The method for preparing a ceramic / metal bicontinuous complex component according to claim 1, characterized in that... The step preceding S3 includes: removing the adhesive introduced into the porous ceramic skeleton during the 3D printing process.

5. The method for preparing a ceramic / metal bicontinuous complex component according to claim 4, characterized in that, In step S2, the step of removing the adhesive from the porous ceramic skeleton includes: heating to 200°C to 300°C at a rate of 0.1°C / min to 0.3°C / min and holding for at least 4 hours; heating to 400°C to 500°C at a rate of 0.1°C / min to 0.3°C / min and holding for at least 4 hours; and heating to 550°C to 650°C at a rate of 0.1°C / min to 0.3°C / min and holding for at least 2 hours.

6. The method for preparing a ceramic / metal bicontinuous complex component according to claim 1, characterized in that, In S3 and S4, the temperature above the melting point of the metal is between 650 °C and 800 °C.

7. The method for preparing a ceramic / metal bicontinuous complex component according to claim 1, characterized in that, In S4, the acceleration of the oscillation force is no greater than 10 G.

8. The method for preparing a ceramic / metal bicontinuous complex component according to claim 1, characterized in that, In step S1, the porous ceramic skeleton is heated to 1500 ℃ to 2000 ℃ to improve the skeleton strength of the porous ceramic skeleton.

9. A method for preparing a ceramic / metal bicontinuous composite material, characterized in that, Includes the following steps: T1: 3D printed porous ceramic skeleton; T2: The porous ceramic skeleton is pretreated to cover the surface of the porous ceramic skeleton with a silicon dioxide layer. T3: The porous ceramic skeleton covered with the silica layer and the metal are placed in a mold. Under vacuum conditions, pressure impregnation is performed and an electric current is introduced. The temperature is kept above the melting point of the metal for more than 10 minutes to allow the molten metal to fully penetrate into and fill the millimeter-level and micrometer-level pores of the porous ceramic skeleton. The mixture is then cooled and solidified to allow the silica layer and the metal to react in situ to improve wettability. T4: Solution treatment is performed at 450 ℃ to 500 ℃ for more than 2 hours; aging treatment is performed at 150 ℃ to 200 ℃ for more than 7 hours to obtain a ceramic / metal bicontinuous composite material.

10. The method for preparing the ceramic / metal bicontinuous composite material according to claim 9, characterized in that, The flexural strength of the ceramic / metal bicontinuous composite material reaches over 280 MPa, and the specific strength reaches over 93 N·m / kg.