A method for producing a bimetallic metallurgical composite billet

By combining liquid-liquid casting technology with host tilt control, argon protection, and multi-hole diversion, the problems of interface oxidation, flow field control, and demolding in the production of bimetallic billets have been solved, realizing the production of high-quality bimetallic metallurgical composite billets and improving production efficiency and yield.

CN123149389APending Publication Date: 2026-11-24NANJING JINZHI ENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611003687.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-07
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing liquid-liquid composite casting technology suffers from problems such as unstable interface oxidation and bonding quality, difficulty in flow field control, interface defects, and difficulty in demolding when producing bimetallic billets, resulting in low production efficiency and low yield.

Method used

The liquid-liquid casting method is adopted, which controls the composite interface by tilting the main unit, prevents interface oxidation by argon gas protection, assists in demolding by linking the upper mold and the push mold, and controls the casting scouring by multi-hole diversion. Combined with the temperature matching of stainless steel and carbon steel and the casting sequence, the uniform spread of molten metal and smooth demolding are ensured.

Benefits of technology

It significantly improves the metallurgical bonding quality of the composite interface, increases production efficiency and yield, reduces production costs, ensures the flatness and bonding quality of the composite interface, and avoids oxidation and demolding damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149389A_ABST
    Figure CN123149389A_ABST
Patent Text Reader

Abstract

This invention discloses a method for producing a stainless steel-carbon steel bimetallic composite billet. It employs a dual-gating-gate independent flow distribution design. First, stainless steel at 1520℃ is cast through the first gating gate under a protective gas atmosphere. Then, carbon steel at 1570℃ is cast through the second gating gate. The superheat of the molten carbon steel causes micro-melting at the interface, achieving liquid-liquid casting metallurgical composite. By controlling the casting temperature, sequence, interface gas protection, and dynamic switching of the mold posture, this invention effectively avoids interface oxidation, significantly improving the interfacial bonding quality and mechanical properties of the stainless steel-carbon steel bimetallic composite billet. The resulting composite billet has a clean interface, high shear strength, and no obvious defects, meeting the requirements of subsequent direct rolling or forging processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for producing billets, specifically a method for producing bimetallic metallurgical composite billets, belonging to the field of metal casting technology. Background Technology

[0002] Bimetallic composite billets combine the superior properties of different metal components (such as the corrosion resistance of stainless steel and the high strength of carbon steel), and have wide applications in petrochemical, marine engineering, and pressure vessel industries. Currently, the mainstream processes for preparing such composite materials include solid-state composite methods (such as explosive welding and hot rolling) and liquid-state composite methods. While solid-state composite methods are technically mature, they have limitations such as high equipment investment, interface bonding strength limited by deformation, and difficulty in preparing products with complex cross-sections.

[0003] In contrast, liquid-liquid composite casting technology, as a near-net-shape forming process, utilizes the superheat of molten metal to achieve interfacial metallurgical bonding, offering significant advantages such as shorter process and lower cost. However, existing liquid-liquid composite casting technologies still face the following key technical bottlenecks in producing high-quality bimetallic billets: 1. Unstable interfacial oxidation and bonding quality: During the step casting process, the solidified surface of the first cast metal layer is highly susceptible to forming an oxide film upon contact with air. If the subsequent molten metal cannot effectively break down or dissolve this oxide layer, it will lead to inclusions or incomplete fusion defects at the interface, severely weakening the shear strength.

[0004] 2. Difficulty in flow field control leads to interface defects: In the traditional vertical casting method, the impact of the later-cast molten metal on the first-cast solidified shell is greater, which easily causes interface turbulence and air entrapment; and due to gravity, the molten metal spreads unevenly, making it difficult to ensure the flatness and consistency of the composite interface.

[0005] 3. Difficult demolding affects yield: Due to the difference in shrinkage rates between the two metals, bimetallic billets generate significant thermal stress and adhesion to the mold wall after solidification. Traditional demolding methods are cumbersome and easily cause surface damage or even cracking of the billet, thus hindering production efficiency.

[0006] Therefore, there is an urgent need to develop a bimetallic metallurgical composite billet production method that can effectively isolate interface oxidation, optimize melt flow behavior, and facilitate demolding, in order to solve the above-mentioned technical problems. Summary of the Invention

[0007] In order to solve the above-mentioned technical problems and overcome the shortcomings of the prior art, this invention provides a production method for stainless steel and carbon steel bimetallic composite billets. The method adopts liquid-liquid casting, and effectively improves the metallurgical bonding quality of the composite interface by controlling the composite interface by tilting the main machine, protecting the interface from oxidation by argon gas, linking the upper mold and the push-side mold to assist demolding, and controlling the casting and scouring by multi-hole diversion.

[0008] The technical solution adopted in this invention is: a method for producing bimetallic metallurgical composite billets, comprising the following steps: Step 1: Apply stainless steel anti-adhesion coating to the mold body, install two central injection pipes, and inject high-purity argon gas into the mold cavity to seal and prepare for casting. Step 2: Smelt stainless steel and carbon steel separately. The tapping temperature of stainless steel is 1580℃, and the tapping temperature of carbon steel is 1650℃. Step 3: After completing the preparation in Step 2, stop the argon gas to purge the air from the cavity. Operate the tilting cylinder to tilt the main unit to 15° and cool the molten stainless steel from Step 1 to 1520°C for casting. 20 seconds after casting, operate the main unit to a horizontal position, lift the mold, and begin injecting argon gas. Simultaneously, cool the carbon steel to 1570°C for casting. After 10 seconds, stop the argon gas and slowly lower the main unit to a horizontal position. When the central injection tube is full, lower the rear end of the main unit to its lowest position and push the side mold until casting is complete. Step 4: 20 minutes after casting is completed, begin the mold opening and billet removal operation. First, lift away the two intermediate injection pipes and pull the base of the intermediate injection pipe to the designated position. Then, pull the return water-cooling base and the side mold back to the endpoint and open the water-cooling head. Next, use the billet removal lifting tool to clamp the billet, lift the upper machine body and the billet. After the billet removal carriage enters the lower mold body, release the lifting tool and lift it away. Finally, pull the billet removal carriage and the billet back outside the casting machine. Use a crane to transfer the billet to the storage area or insulation pit for subsequent storage processing.

[0009] In step one, the stainless steel ladle has a capacity of 3 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke; the carbon steel ladle has a capacity of 7 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke.

[0010] In step one, the argon purity is ≥99.999%, the O2 content is ≤1ppm, the N2 content is ≤3ppm, and the pressure is 0.6MPa.

[0011] The stainless steel used is 304 stainless steel, and the carbon steel is Q235 material, ensuring that the content of harmful impurity elements in the molten steel meets national standards.

[0012] In step two, the casting machine has a casting cross-section of 250×1500×2500 mm and a flow rate of 150-200 m³ / h. 3 / h, inlet water pressure 0.2-0.3MPa.

[0013] In step three, when casting molten metal, a multi-hole diversion steel flow channel is used to ensure that the molten metal flows evenly into the cavity. The diameter of the pores in the steel flow brick is 60mm.

[0014] The beneficial effects of this invention are: Compared with the prior art, the present invention has the following advantages: (1) Significantly improved composite interface quality: When casting stainless steel, the present invention guides the molten metal to spread smoothly into layers by precisely controlling the tilt angle of the host machine. When casting carbon steel, the host machine posture is continuously adjusted so that the high-temperature carbon steel is evenly spread on the semi-solidified interface of stainless steel, avoiding defects such as interface turbulence and air entrapment caused by concentrated molten metal flushing, and ensuring the flatness and bonding quality of the composite interface.

[0015] (2) Effective prevention of interface oxidation: The present invention introduces high-purity argon gas as a protective gas immediately during the lifting and moving of the upper mold, which effectively prevents the stainless steel surface from contacting the air and forming an oxide film, ensuring the cleanliness of the composite interface, thereby achieving a high-strength, defect-free metallurgical bond.

[0016] (3) Matching the temperature and timing of bimetallic materials to ensure the quality of the bonding surface: By casting carbon steel first and then stainless steel, the two metals reach the optimal casting temperature at the same time. By casting stainless steel first and then carbon steel, the carbon steel liquid can cover the stainless steel in time when the semi-solidified micro-melting interface is formed, so as to achieve perfect bonding of the bimetallic liquids and avoid incomplete fusion or interface defects caused by temperature mismatch.

[0017] (4) Improved demolding efficiency and product integrity: By applying stainless steel anti-adhesion coating to the inner cavity of the mold and coordinating the lifting of the upper mold and the pushing of the edge mold, the present invention effectively solves the problem of adhesion between the bimetallic composite blank and the inner cavity of the mold, improves demolding efficiency, and ensures the surface quality of the blank and the integrity of the product.

[0018] (5) Effective control of casting erosion: The present invention adopts a multi-hole diversion steel flow channel during casting, so that the stainless steel and carbon steel molten metal are evenly diverted into the mold cavity, which effectively controls the erosion of the composite interface during the casting process and is conducive to obtaining a uniform metallurgical bonding interface.

[0019] (6) Significantly reduced production costs: The present invention adopts liquid-liquid composite casting method for one-time forming. Compared with the traditional composite billet making technology, it can save subsequent heating, rolling and other processes, greatly reduce production costs, and has strong market competitiveness. Attached Figure Description

[0020] Figure 1 This is a process flow diagram of the present invention; Figure 2 This is a graph showing the C element scanning analysis results of the bonding surface of the composite blank of the present invention; Figure 3 This is a graph showing the O element scanning analysis results of the bonding surface of the composite blank of the present invention; Figure 4 This is a graph showing the Cr element scanning analysis results of the bonding surface of the composite blank of the present invention; Figure 5 This is a graph showing the Si element scanning analysis results of the bonding surface of the composite blank of the present invention. Detailed Implementation

[0021] A method for producing bimetallic metallurgical composite billets, using an existing casting machine for auxiliary production, is shown in the flowchart in Figure 1, and includes the following steps: Step 1: Apply stainless steel anti-adhesion coating to the mold body, install two central injection pipes, and inject high-purity argon gas into the mold cavity to seal and prepare for casting. Step 2: Smelt stainless steel and carbon steel separately. The tapping temperature of stainless steel is 1580℃, and the tapping temperature of carbon steel is 1650℃. Step 3: After completing the preparation in Step 2, stop the argon gas to purge the air from the cavity. Operate the tilting cylinder to tilt the main unit to 15° and cool the molten stainless steel from Step 1 to 1520°C for casting. 20 seconds after casting, operate the main unit to a horizontal position, lift the mold, and begin injecting argon gas. Simultaneously, cool the carbon steel to 1570°C for casting. After 10 seconds, stop the argon gas and slowly lower the main unit to a horizontal position. When the central injection tube is full, lower the rear end of the main unit to its lowest position and push the side mold until casting is complete. Step 4: 20 minutes after casting is completed, begin the mold opening and billet removal operation. First, lift away the two intermediate injection pipes and pull the base of the intermediate injection pipe to the designated position. Then, pull the return water-cooling base and the side mold back to the endpoint and open the water-cooling head. Next, use the billet removal lifting tool to clamp the billet, lift the upper machine body and the billet. After the billet removal carriage enters the lower mold body, release the lifting tool and lift it away. Finally, pull the billet removal carriage and the billet back outside the casting machine. Use a crane to transfer the billet to the storage area or insulation pit for subsequent storage processing.

[0022] In step one, the stainless steel ladle has a capacity of 3 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke; the carbon steel ladle has a capacity of 7 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke.

[0023] In step one, the argon purity is ≥99.999%, the O2 content is ≤1ppm, the N2 content is ≤3ppm, and the pressure is 0.6MPa.

[0024] The stainless steel used is 304 stainless steel, and the carbon steel is Q235 material, ensuring that the content of harmful impurity elements in the molten steel meets national standards.

[0025] In step two, the casting machine has a casting cross-section of 250×1500×2500 mm and a flow rate of 150-200 m³ / h. 3 / h, inlet water pressure 0.2-0.3MPa.

[0026] In step three, when casting molten metal, a multi-hole diversion steel flow channel is used to ensure that the molten metal flows evenly into the cavity. The diameter of the pores in the steel flow brick is 60mm. Example 1

[0027] A method for producing bimetallic metallurgical composite billets, using an existing casting machine for auxiliary production, is shown in the flowchart in Figure 1, and includes the following steps: Step 1: Apply stainless steel anti-adhesion coating to the mold body, install two injection tubes, and inject high-purity argon gas into the mold cavity. The purity is ≥99.999%, the O2 content is ≤1ppm, the N2 content is ≤3ppm, and the pressure is 0.6MPa. Step 2: Smelt stainless steel and carbon steel separately. Use 304 stainless steel and tap the steel at 1580℃. Use Q235 carbon steel and tap the steel at 1650℃. The stainless steel ladle has a capacity of 3 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke; the carbon steel ladle has a capacity of 7 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke. The casting machine has a casting cross-section of 250×1500×2500, a flow rate of 150-200 m3 / h, and an inlet water pressure of 0.2-0.3 MPa. Step 3: Stop the argon gas, operate the tilting cylinder to tilt the main body of the casting machine to 15°, cool the stainless steel liquid to 1520℃ for casting, and 20 seconds after the casting is completed, operate the main body to a horizontal position, lift the mold, inject argon gas, and at the same time cool the carbon steel to 1570℃ for casting. Stop the argon gas at 10 seconds and operate the main body to slowly level it. When the middle injection tube is filled, operate the rear end of the main body to the lowest position, push the side mold until the casting is completed. During the casting process, the bimetal uses a multi-hole diversion steel flow channel, and the diameter of the steel flow brick is 60mm. Step 4: 20 minutes after casting is completed, begin the mold opening and billet removal operation. First, lift away the two intermediate injection pipes and pull the base of the intermediate injection pipe to the designated position. Then, pull the return water-cooling base and the side mold back to the endpoint and open the water-cooling head. Next, use the billet removal lifting tool to clamp the billet, lift the upper machine body and the billet. After the billet removal carriage enters the lower mold body, release the lifting tool and lift it away. Finally, pull the billet removal carriage and the billet back outside the casting machine. Use a crane to transfer the billet to the storage area or insulation pit for subsequent storage processing.

[0028] The scanning analysis results of C, O, Cr, and Si elements on the interface of the composite steel billet produced in this embodiment are shown in the figure below. Figure 2-5 As shown, the method of the present invention achieves high metallurgical bonding quality of the composite interface, and argon gas protection prevents interface oxidation.

[0029] In addition to the embodiments described above, the present invention may have other implementations. All technical solutions formed by equivalent substitution or equivalent transformation fall within the protection scope claimed by the present invention.

Claims

1. A method for producing a bimetallic metallurgical composite billet, characterized in that, Specifically, the following steps are included: Step 1: Apply stainless steel anti-adhesion coating to the mold body, install two central injection pipes, and inject high-purity argon gas into the mold cavity to seal and prepare for casting. Step 2: Smelt stainless steel and carbon steel separately. The tapping temperature of stainless steel is 1580℃, and the tapping temperature of carbon steel is 1650℃. Step 3: After completing the preparation in Step 2, stop the argon gas to purge the air from the cavity. Operate the tilting cylinder to tilt the main body of the casting machine to 15°, and cool the stainless steel smelted in Step 1 to 1520°C for casting. 20 seconds after casting is completed, operate the main body to a horizontal position, lift the mold, and start injecting argon gas. At the same time, cool the carbon steel to 1570°C for casting. After 10 seconds, stop the argon gas and slowly lower the main body to a horizontal position. When the middle injection tube is full, lower the rear end of the main body to the lowest position and push the side mold until casting is complete. Step 4: 20 minutes after casting is completed, begin the mold opening and billet removal operation. First, lift away the two intermediate injection pipes and pull the base of the intermediate injection pipe to the designated position. Then, pull the return water-cooling base and the side mold back to the endpoint and open the water-cooling head. Next, use the billet removal lifting tool to clamp the billet, lift the upper machine body and the billet. After the billet removal carriage enters the lower mold body, release the lifting tool and lift it away. Finally, pull the billet removal carriage and the billet back outside the casting machine. Use a crane to transfer the billet to the storage area or insulation pit for subsequent storage processing.

2. The method for producing bimetallic metallurgical composite billet as described in claim 1, characterized in that: In step one, the stainless steel ladle has a capacity of 3 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke; the carbon steel ladle has a capacity of 7 tons, a 50mm sizing nozzle, a 65mm stopper, and a 100mm stopper rod stroke.

3. The method for producing bimetallic metallurgical composite billet as described in claim 1, characterized in that: In step one, the argon purity is ≥99.999%, the O2 content is ≤1ppm, the N2 content is ≤3ppm, and the pressure is 0.6MPa.

4. The method for producing bimetallic metallurgical composite billet as described in claim 1, characterized in that: The stainless steel used is 304 stainless steel, and the carbon steel is Q235 material, ensuring that the content of harmful impurity elements in the molten steel meets national standards.

5. The method for producing bimetallic metallurgical composite billet as described in claim 1, characterized in that: In step two, the casting machine has a casting cross-section of 250×1500×2500 mm and a flow rate of 150-200 m³ / h. 3 / h, inlet water pressure 0.2-0.3MPa.

6. The method for producing bimetallic metallurgical composite billet as described in claim 1, characterized in that: In step three, when casting molten metal, a multi-hole diversion steel flow channel is used to ensure that the molten metal flows evenly into the cavity. The diameter of the pores in the steel flow brick is 60mm.