A ladle shroud structured packing and method of use thereof

By designing a three-layer structured packing, the problem of insufficient melting of the Fe-C alloy sealing layer in electromagnetic tapping technology was solved, achieving efficient molten steel flow, improving the self-opening rate and reducing heating energy consumption.

CN123149397APending Publication Date: 2026-11-24BAOSHAN IRON & STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510658664.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing electromagnetic tapping technology, the Fe-C alloy sealing layer is not fully melted and becomes denser through sintering, which prevents the molten steel from breaking through the sealing layer under static pressure, thus affecting the self-opening rate.

Method used

The three-layer structured filler includes a melting layer, a heat insulation layer, and a support layer. The melting layer melts and transfers heat after contacting the molten steel. The heat insulation layer and the support layer are locally sintered under the action of the induction heating coil. The support layer provides support before the slide plate opens, ensuring that the molten steel flows out under static pressure.

Benefits of technology

This improves the melting effect of the electromagnetic induction heating system, significantly increases the self-opening rate, reduces the induction heating power requirement, and avoids damage to the slide plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149397A_ABST
    Figure CN123149397A_ABST
Patent Text Reader

Abstract

This invention discloses a structured packing for the ladle inlet, comprising, from top to bottom, a molten layer with molten particles, a heat-insulating layer with heat-insulating particles, and a supporting layer with supporting particles. The molten layer completely melts into a liquid phase upon contact with molten steel and permeates into the heat-insulating layer. The melting point of the molten layer is lower than that of the heat-insulating particles. Accordingly, this invention also discloses a method for using the structured packing for the ladle inlet. This invention can effectively improve the melting effect of the electromagnetic induction heating system while keeping the required induction coil heating position unchanged, enabling the molten steel to break through the sealing layer under static pressure and significantly increasing the self-opening rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a component for steel smelting, and more particularly to a packing material. Background Technology

[0002] The smelting and production of high-quality and long-life clean steel is crucial for the development of steel smelting and low-carbonization. Given that existing clean steel smelting technologies are gradually reaching their limits, electromagnetic tapping technology, which uses Fe-C alloys to replace traditional guide sand, is essential for improving the final quality of steel and reducing carbon emissions during the use and service of steel materials. Because electromagnetic tapping technology avoids the use of guide sand, compared to the sliding gate tapping process currently used by most steel mills, the total oxygen content and the number of inclusions in the cast billet can be effectively reduced, resulting in a significant improvement in steel cleanliness, overall steel quality, and service life.

[0003] For example, Chinese patent document CN1810417A, entitled "A steel ladle with a heating and tapping device and a method for tapping steel therefrom", discloses filling the space between the bottom of the ladle and the upper slide plate with carbon powder and iron particles or a mixture of both, wherein the volume ratio of iron particles to carbon powder is 1:1 to 3.

[0004] In addition, Chinese patent document CN108356258A, entitled "A combined sprue seat brick based on an electromagnetic steel tapping system", discloses that an induction coil is encapsulated inside the lower seat brick and the size of the molten steel channel is optimized to ensure that the sintered layer is cylindrical, but the thickness of the sintered layer is difficult to limit.

[0005] Currently, patents related to electromagnetic tapping technology provide relevant designs in terms of principle and structure. However, in actual industrial applications, there are still difficulties in successfully starting the casting process. There are two main reasons for this. First, the solid-liquid interface and thickness of the single Fe-C alloy filler are affected by factors such as refining time and hot conveying process, resulting in the fact that they are not completely consistent with the Fe-C alloy area heated and melted by the induction heating coil. This leads to insufficient melting of the Fe-C alloy sealing layer. Second, the Fe-C alloy inside the sealing layer will sinter and become dense. The electromagnetic induction heating system cannot fully heat the sealing layer within the safe output power range, making it impossible for the molten steel to break through the sealing layer under static pressure and thus preventing the start of casting. Summary of the Invention

[0006] One of the objectives of this invention is to provide a structured packing for the ladle nozzle, which can effectively improve the melting effect of the electromagnetic induction heating system while keeping the required induction coil heating position unchanged, so that the molten steel can break through the sealing layer under static pressure and significantly increase the self-opening rate.

[0007] To achieve the above objectives, the present invention proposes a structured packing for the top nozzle of a steel ladle, which comprises, from top to bottom, a melting layer with melting layer particles, a heat insulation layer with heat insulation layer particles, and a support layer with support layer particles; wherein the melting layer melts completely into a liquid phase after contacting molten steel and permeates into the heat insulation layer; the melting point of the melting layer particles is lower than that of the heat insulation layer particles.

[0008] According to this configuration, the structured filler material for the ladle nozzle of the present invention includes at least three layers of filler material with different compositions. The melting layer melts completely after contacting the molten steel and transfers heat to the next insulating layer. The insulating layer is in contact with the upper melting layer. The support layer provides support before the slide plate is opened.

[0009] Furthermore, in the structured filler for the ladle nozzle described in this invention, the melting point of the molten layer particles is 1100℃~1400℃.

[0010] Furthermore, in the structured packing material for the ladle nozzle described in this invention, the material of the molten layer particles is a low-melting-point Fe-C alloy, and the C element content in the low-melting-point Fe-C alloy is 1.8 to 4.3 wt%.

[0011] Furthermore, in the structured filler for the ladle nozzle described in this invention, the melting point of the insulation layer particles is 1500℃~1600℃.

[0012] Furthermore, in the structured packing material for the ladle inlet of the present invention, the heat insulation layer particles are made of iron-based material, and the Fe element content in the iron-based material is ≥99.5wt%.

[0013] Furthermore, in the structured packing material for the ladle inlet of the present invention, the material of the supporting layer particles is an Fe-C alloy.

[0014] It should be noted that the present invention does not particularly limit the Fe-C alloy of the support layer; it can be a low-melting-point Fe-C alloy or an ordinary Fe-C alloy.

[0015] Furthermore, in the structured filler for the ladle nozzle described in this invention, the filling height h1 of the molten layer is 100-450 mm, and / or the filling height h2 of the insulation layer is 50-200 mm; and / or the filling height h3 of the support layer is 250-550 mm.

[0016] The top of the molten layer is not lower than the bottom of the ladle, and the bottom of the support layer is level with the upper surface of the slide plate.

[0017] Considering that the maximum power area of ​​the induction heating coil is within the range of 1 / 4 downward from the upper surface of the coil to 1 / 4 upward from the lower surface, further, in the structured filler of the ladle nozzle described in this invention, the interface between the melting layer and the heat insulation layer is located at 1 / 4 to 1 / 3 of the height of the induction heating coil downward from the upper surface of the induction heating coil.

[0018] Furthermore, in the structured filler for the ladle water inlet of the present invention, the particle size of the heat insulation layer particles is 0.15 to 1.5 mm.

[0019] This is because the molten steel melts the particles in the molten layer and then penetrates further into the insulation layer. Using particles with a diameter of 0.15 to 1.5 mm can reduce the penetration depth and prevent the particles from penetrating into the support layer due to excessive size.

[0020] Furthermore, in the structured filler for the ladle inlet of the present invention, among the insulation layer particles, particles with a diameter <0.4 mm account for 10% to 40% of the total volume of the insulation layer particles, particles with a diameter of 0.4 to 0.7 mm account for 30% to 70% of the total volume of the insulation layer particles, and particles with a diameter >0.7 mm account for 10% to 20% of the total volume of the insulation layer particles.

[0021] Furthermore, in the structured packing material for the ladle inlet of the present invention, the particle size of the supporting layer particles is 0.8 to 3 mm.

[0022] This is because the support layer particles with a particle size of 0.8 to 3 mm require relatively little filling material, and can fall quickly after the slide plate under the ladle is opened, thus speeding up the pouring time.

[0023] Furthermore, in the structured packing for the ladle inlet of the present invention, among the supporting layer particles, particles with a diameter <1.5 mm account for 30% to 50% of the total volume of all supporting layer particles, particles with a diameter of 1.5 to 2.5 mm account for 20% to 60% of the total volume of all supporting layer particles, and particles with a diameter >2.5 mm account for 10% to 20% of the total volume of all supporting layer particles.

[0024] Another objective of this invention is to provide a method for using the structured packing material at the ladle inlet as described above. When used in conjunction with the heating of the induction heating coil, it can effectively improve the melting effect of the electromagnetic induction heating system, enabling the molten steel to break through the sealing layer under static pressure and significantly increase the self-opening rate.

[0025] Based on the above-mentioned objectives, the present invention also provides a method for using the structured packing material at the ladle inlet as described above, comprising the following steps:

[0026] The ladle top nozzle is filled with the structured filler material described above.

[0027] The ladle receives molten steel, which is then refined.

[0028] After refining is completed and tapping begins, current is passed through the induction coil: if the refining time is ≤40min, the output power of the induction coil is controlled to be 100~300KW; if the refining time is >40min, the output power of the induction coil is controlled to be 300~500KW.

[0029] The structured packing for the ladle nozzle described in this invention utilizes the characteristic of the uppermost molten layer absorbing heat from the molten steel and completely melting it. The molten alloy penetrates downwards to the lower insulation layer and undergoes localized sintering within the gaps between the insulation layer particles, thereby defining the specific area that the induction coil needs to heat. Because the molten alloy forms a sintered structure within the gaps between the insulation layer particles, the induction coil does not need to heat the entire insulation layer to a molten state; the molten steel will automatically flow out under static pressure, significantly reducing the power required for induction heating and simultaneously improving the ladle's self-opening rate.

[0030] Furthermore, the bottommost support layer of the structured packing material at the ladle top nozzle described in this invention supports the upper molten layer and heat insulation layer before the ladle taps out steel. After the lower slide plate is opened, the support layer can fall freely, effectively preventing the molten alloy from contacting the upper slide plate and avoiding damage to the upper slide plate. Attached Figure Description

[0031] Figure 1 The diagram shows the structure and usage status of the structured packing material for the ladle inlet of the present invention in one embodiment. Detailed Implementation

[0032] The structured packing material for the ladle inlet and its application method described in this invention will be further explained and illustrated below with reference to the accompanying drawings and specific embodiments. However, this explanation and illustration do not constitute an undue limitation on the technical solution of this invention.

[0033] Figure 1 The structure of the structured packing for the ladle inlet of the present invention is shown in one embodiment.

[0034] like Figure 1 As shown, in some embodiments, the ladle includes an outer shell 3 and a refractory layer 2 disposed within the outer shell 3, thereby forming an inner cavity 1 for containing molten steel within the ladle. A seat brick 7 is provided below the inner cavity 1 to form a ladle top nozzle 8. Structured packing material for the ladle top nozzle is disposed within the top nozzle 8.

[0035] In some implementations, such as Figure 1As shown, the structured packing material at the ladle nozzle includes, from top to bottom, a melting layer 4 with melting layer particles, a heat insulation layer 5 with heat insulation layer particles, and a support layer 6 with support layer particles; wherein the melting layer melts completely into a liquid phase after contacting the molten steel and penetrates into the heat insulation layer 5; the melting point of the melting layer particles is lower than that of the heat insulation layer particles.

[0036] According to this configuration, the structured filler material for the ladle nozzle of the present invention includes at least three layers of filler material with different compositions. The melting layer 4 melts completely after contacting the molten steel and transfers heat to the next insulation layer. The insulation layer 5 is in contact with the upper melting layer. The support layer 6 provides support before the lower slide plate 11 opens relative to the upper slide plate 10.

[0037] In some more specific embodiments, the molten layer is made of a low-melting-point Fe-C alloy, wherein the C content of the low-melting-point Fe-C alloy is 1.8 to 4.3 wt%. The melting point of the low-melting-point Fe-C alloy is 1100°C to 1400°C.

[0038] In some more specific embodiments, the insulation layer particles are made of iron-based materials, and the Fe content in the iron-based materials is ≥99.5wt%.

[0039] In some more specific embodiments, the melting point of the insulation particles is 1500°C to 1600°C.

[0040] In some more specific embodiments, the material of the support layer particles can be a common Fe-C alloy with a higher melting point than the low-melting-point Fe-C alloy.

[0041] In some more specific embodiments, the particle size of the insulation layer particles can be 0.15 to 1.5 mm.

[0042] In some more specific embodiments, in the insulation layer particles, particles with a diameter <0.4 mm account for 10% to 40% of the total volume of all insulation layer particles, particles with a diameter of 0.4 to 0.7 mm account for 30% to 70% of the total volume of all insulation layer particles, and particles with a diameter >0.7 mm account for 10% to 20% of the total volume of all insulation layer particles.

[0043] In some more specific embodiments, the particle size of the support layer particles is 0.8–3 mm.

[0044] In some more specific embodiments, in the support layer particles, particles with a diameter <1.5 mm account for 30% to 50% of the total volume of all support layer particles, particles with a diameter of 1.5 to 2.5 mm account for 20% to 60% of the total volume of all support layer particles, and particles with a diameter >2.5 mm account for 10% to 20% of the total volume of all support layer particles.

[0045] like Figure 1 As shown, in some specific embodiments, the top of the molten layer 4 is not lower than the bottom of the ladle, the filling height h1 of the molten layer 4 is 100-450mm, and / or the filling height h2 of the heat insulation layer 5 is 50-200mm; and / or the filling height h3 of the support layer 6 is 250-550mm, and the bottom end of the support layer 6 is flush with the upper surface of the lower slide plate 11.

[0046] In some specific implementation methods, such as Figure 1 As shown, the interface between the melting layer 4 and the heat insulation layer 5 is located at 1 / 4 to 1 / 3 of the height of the induction heating coil downwards from the upper surface of the induction heating coil 9.

[0047] In this configuration, the uppermost molten layer absorbs the heat from the molten steel and melts completely. The molten alloy penetrates downwards to the lower insulation layer and undergoes localized sintering within the gaps between the insulation layer particles, thus defining the specific area that the induction coil needs to heat. Because the molten alloy forms a sintered structure within the gaps between the insulation layer particles, the induction coil does not need to heat the entire insulation layer to a molten state. The molten steel automatically flows out under static pressure, significantly reducing the power required for induction heating and simultaneously increasing the ladle's self-opening rate.

[0048] Furthermore, the bottom support layer supports the upper molten layer and insulation layer before the ladle taps out the steel. After the lower slide plate 11 is opened, it can fall freely, effectively preventing the molten alloy from contacting the upper slide plate 10 and avoiding damage to the upper slide plate.

[0049] In some embodiments, the present invention also provides a method for using the above-mentioned structured filler material for the ladle nozzle.

[0050] Figure 1 The diagram also shows the usage status of the structured packing material for the ladle inlet of the present invention in one embodiment.

[0051] In some embodiments, the ladle inlet 8 and outlet 12 can be cleaned before filling the ladle with structured filler to remove residual steel and impurities, and then the ladle can be baked.

[0052] Then, as Figure 1 As shown, a support layer 6, a heat insulation layer 5, and a melting layer 4 are sequentially added into the ladle top nozzle to fill the ladle top nozzle with structured filler.

[0053] Then, the ladle receives the molten steel, which is then refined.

[0054] After refining is completed and tapping begins, current is passed through the induction heating coil 9: if the steel refining time in the previous step is ≤40min, the output power of the induction heating coil is controlled to be 100~300KW; if the steel refining time in the previous step is >40min, the output power of the induction heating coil is controlled to be 300~500KW.

[0055] After current is applied to the induction heating coil for 30 to 60 seconds, the lower slide plate 11 is moved to connect the upper water inlet 8 with the lower water inlet 12, and the molten steel flows out from the lower water inlet 12.

[0056] In an example of producing automotive sheet steel using a 110t ladle, after the ladle undergoes baking and nozzle cleaning processes, the ladle's upper nozzle is first filled with structured filler. The support layer is made of ordinary Fe-C alloy, with particle sizes ranging from 0.8 to 2 mm. Particles <1.5 mm account for 50% of the total volume of the support layer particles, and particles with a diameter between 1.5 and 2 mm account for the remaining 50%. The filling height of the support layer is h3 = 300 mm. Subsequently, an insulation layer is filled. The insulation layer particles are made of pure Fe with a particle size of 0.15–1 mm. Particles with a diameter <0.4 mm account for 30% of the total volume of the insulation layer particles, particles with a diameter of 0.4–0.7 mm account for 60% of the total volume of the insulation layer particles, and particles with a diameter >0.7 mm account for 10% of the total volume of the insulation layer particles. The filling height h2 = 200 mm. Finally, a molten layer is filled, which is made of a low-melting-point Fe-C alloy with a content of 2% ≤ C ≤ 3%, and the filling height h1 = 200 mm.

[0057] After filling, the molten steel is poured into a ladle for ladle refining for 30 minutes. During refining, the upper molten layer melts rapidly upon contact with the high-temperature molten steel, forming a liquid phase that penetrates downwards into the insulation layer. Because the temperature of the molten alloy is below its melting point, this layer remains solid, with some solid-state sintering occurring. The molten alloy dissipates heat outwards through thermal conduction, lowering its temperature. Liquid sintering occurs between the particles of the insulation layer. The portion in contact with the lower support layer has a temperature below the solidus temperature of the support layer, preventing further penetration of the alloy. After refining, the ladle is transferred to the continuous casting station for pouring. Current is passed through the induction heating coil, controlling its output power to 200-250 kW. The Joule heat generated by induction heating remelts the sintered portion of the insulation layer. Subsequently, the sliding plate moves, connecting the upper and lower inlet, allowing the support layer to flow out from the lower inlet. Under gravity, the molten steel breaks through the incompletely melted sintered area from the induction heating, achieving automatic pouring.

[0058] It should be noted that the prior art portion within the scope of protection of this invention is not limited to the embodiments given in this invention. All prior art that does not contradict the solution of this invention, including but not limited to prior patent documents, prior publications, prior public uses, etc., can be included within the scope of protection of this invention.

[0059] Furthermore, the combination of the technical features in this case is not limited to the combination methods described in the claims of this case or the combination methods described in the specific embodiments. All technical features described in this case can be freely combined or combined in any way, unless they contradict each other.

[0060] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made thereto are those that can be directly derived or easily conceived by those skilled in the art from the content disclosed in the present invention, and should all fall within the protection scope of the present invention.

Claims

1. A structured packing for the inlet nozzle of a steel ladle, characterized in that, From top to bottom, it includes a melting layer with melting layer particles, a heat insulation layer with heat insulation layer particles, and a support layer with support layer particles; wherein the melting layer melts completely into a liquid phase after contacting the molten steel and penetrates into the heat insulation layer. The melting point of the molten layer particles is lower than that of the insulation layer particles.

2. The structured packing for the ladle inlet as described in claim 1, characterized in that, The melting point of the molten layer particles is 1100℃~1400℃.

3. The structured packing for the ladle inlet as described in claim 1, characterized in that, The material of the molten layer particles is a low-melting-point Fe-C alloy, and the C element content in the low-melting-point Fe-C alloy is 1.8 to 4.3 wt%.

4. The structured packing for the ladle inlet as described in claim 1, characterized in that, The melting point of the insulation layer particles is 1500℃~1600℃.

5. The structured packing for the ladle inlet as described in claim 1, characterized in that, The insulation layer particles are made of iron-based material, and the Fe element content in the iron-based material is ≥99.5wt%.

6. The structured packing for the ladle inlet as described in claim 1, characterized in that, The material of the support layer particles is Fe-C alloy.

7. The structured packing for the ladle inlet as described in claim 1, characterized in that, The filling height h1 of the molten layer is 100-450 mm, and / or the filling height h2 of the heat insulation layer is 50-200 mm; and / or the filling height h3 of the support layer is 250-550 mm.

8. The structured packing for the ladle inlet as described in claim 1, characterized in that, The interface between the melting layer and the heat insulation layer is located at 1 / 4 to 1 / 3 of the height of the induction heating coil, below the upper surface of the induction heating coil.

9. The structured packing for the ladle inlet as described in claim 1, characterized in that, The particle size of the insulation layer particles is 0.15 to 1.5 mm.

10. The structured packing for the ladle inlet as described in claim 1, characterized in that, In the heat insulation layer particles, particles with a diameter <0.4 mm account for 10% to 40% of the total volume of all heat insulation layer particles, particles with a diameter of 0.4 to 0.7 mm account for 30% to 70% of the total volume of all heat insulation layer particles, and particles with a diameter >0.7 mm account for 10% to 20% of the total volume of all heat insulation layer particles.

11. The structured packing for the ladle inlet as described in claim 1, characterized in that, The particle size of the support layer particles is 0.8 to 3 mm.

12. The structured packing for the ladle inlet as described in claim 1, characterized in that, In the support layer particles, particles with a diameter <1.5 mm account for 30% to 50% of the total volume of all support layer particles, particles with a diameter of 1.5 to 2.5 mm account for 20% to 60% of the total volume of all support layer particles, and particles with a diameter >2.5 mm account for 10% to 20% of the total volume of all support layer particles.

13. The method of using the structured packing material for the ladle inlet as described in any one of claims 1-12, characterized in that, Including the following steps: The ladle top nozzle is filled with the structured filler material described above. The ladle receives molten steel, which is then refined. After refining is completed and tapping begins, current is passed through the induction coil: if the refining time is ≤40min, the output power of the induction coil is controlled to be 100~300KW; if the refining time is >40min, the output power of the induction coil is controlled to be 300~500KW.

Citation Information

Patent Citations

  • Combined type pocket block based on electromagnetic induction heating tapping technology

    CN108356258A

  • Ladle with steel heating and tapping set and its tapping method

    CN1810417A