Apparatus and method for continuous production of silver nanoparticles

By combining microfluidic reactor design with a constant-temperature water bath ultrasonic system, the problems of particle agglomeration and clogging in the preparation of nano-silver were solved, achieving particle size uniformity and production stability, making it suitable for large-scale industrial production.

CN123149401APending Publication Date: 2026-11-24CHANGCHUN GOLD RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611663982.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing continuous nano-silver preparation devices suffer from severe particle agglomeration, uneven particle size distribution, and easy clogging due to excessive feed impact, making it difficult to meet the needs of large-scale industrial production.

Method used

The microfluidic reactor design incorporates a circular buffer chamber and an arc-shaped flow divider structure, combined with a constant-temperature water bath and an ultrasonic system, to achieve uniform premixing of the silver source and dispersant and mild reaction conditions, thereby reducing flow rate and impact force and preventing particle agglomeration and pipe blockage.

Benefits of technology

This method achieves uniform silver nanoparticle size, narrow distribution, and stable production, making it suitable for large-scale industrial production. It avoids particle agglomeration and pipeline blockage problems, and improves silver ion conversion rate and reaction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149401A_ABST
    Figure CN123149401A_ABST
Patent Text Reader

Abstract

This application provides an apparatus and method for the continuous preparation of nano-silver, belonging to the field of nanomaterials. The apparatus includes a microfluidic reactor, a constant-temperature water bath, and an ultrasonic system. The microfluidic reactor has three inlets: a first inlet, a second inlet, and a third inlet. A first circular buffer chamber is provided at the first inlet, and a second circular buffer chamber is provided at the second inlet. The outlets of the first and second circular buffer chambers are connected in a Y-shape to form a first confluence pipe. The outlet of the first confluence pipe is connected to a first distributor. The outlet of the third inlet is connected to a second distributor. The first and second distributors are connected to a main pipeline. This application achieves continuous and efficient production with mild and controllable reaction conditions, uniform and narrow-distribution nano-silver particles, and minimal pipeline clogging by using circular buffer chambers, an arc-shaped microfluidic pipe distribution structure, and a constant-temperature ultrasonic environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of nanomaterials technology, specifically to an apparatus and method for the continuous preparation of nanosilver. Background Technology

[0002] Silver powder possesses high electrical and thermal conductivity and is relatively inexpensive compared to other precious metals, making it widely used in electronics, automotive, medical, aerospace, and electromagnetic shielding fields. As electronic components evolve towards miniaturization, integration, and flexibility, the requirements for the quality and quantity of silver powder are gradually increasing. Currently, the main method for preparing nano-silver is chemical reduction, which produces silver powder with problems such as wide particle size distribution, poor dispersibility, and uneven particle size; production capacity is also limited by the volume control of the reactor in the production line.

[0003] To overcome the bottleneck of intermittent production, continuous preparation of nano-silver using microreactors or impinging flow reactors has emerged in recent years. However, existing devices have significant shortcomings: First, most microreactors employ a vertical impingement structure at the feed confluence, where two or more fluid streams collide directly at high velocities, creating strong local impacts and eddies. This leads to excessively high local supersaturation during the reaction, resulting in uncontrolled nucleation rates and severe agglomeration and uneven growth of silver particles. Second, existing devices generally lack precise control over the pre-reaction mixing process. The silver source and dispersant are difficult to fully and uniformly premix before contacting the reducing agent, preventing the dispersant from effectively encapsulating the silver source and further exacerbating agglomeration. Furthermore, during continuous operation, silver powder easily deposits on the inner walls of the microreactor pipes, causing blockages and affecting long-term stable operation.

[0004] In view of this, it is necessary to design an apparatus and method for the continuous preparation of nano-silver in order to solve the above problems. Summary of the Invention

[0005] In view of the technical problems existing in the background art, this application provides an apparatus and method for continuous preparation of nano-silver, which aims to solve the technical problems of severe particle agglomeration, uneven particle size distribution and easy clogging caused by excessive feed impact in existing continuous preparation devices for nano-silver.

[0006] In a first aspect, this application provides an apparatus for the continuous preparation of nano-silver, including a microfluidic reactor, a constant temperature water bath and an ultrasonic system, wherein the microfluidic reactor is provided with three feed inlets, namely a first feed inlet, a second feed inlet and a third feed inlet; The first feed inlet is provided with a first circular buffer chamber, and the second feed inlet is provided with a second circular buffer chamber. The outlet end of the first circular buffer chamber and the outlet end of the second circular buffer chamber are connected in a Y-shape to form a first confluence pipe. The outlet end of the first confluence pipe is connected to the first distributor; the outlet end of the third feed inlet is connected to the second distributor; the outlet ends of the first distributor and the second distributor are connected to the inlet end of the main pipeline. The feed pipes of the microfluidic reactors are all equipped with peristaltic pumps.

[0007] As a further improvement of this application, both the first and second splitters include three arc-shaped flow tubes.

[0008] As a further improvement of this application, the length of the first inlet pipe is 0.3-0.8m and the inner diameter of the pipe is 5-12cm; the length of the second inlet pipe is 0.3-0.8m and the inner diameter of the pipe is 3-8cm; and the length of the third inlet pipe is 0.3-0.8m and the inner diameter of the pipe is 3-8cm.

[0009] As a further improvement of this application, the pipeline length of the first feed inlet is 0.5m and the inner diameter of the pipe is 8cm; the pipeline length of the second feed inlet is 0.5m and the inner diameter of the pipe is 5cm; and the pipeline length of the third feed inlet is 0.5m and the inner diameter of the pipe is 5cm.

[0010] As a further improvement of this application, the microfluidic reactor is entirely disposed inside the constant temperature water bath and simultaneously placed in the ultrasonic field environment of the ultrasonic system.

[0011] As a further improvement of this application, the discharge end of the main pipeline is connected to a collection device.

[0012] Secondly, this application provides a method for the continuous preparation of silver nanoparticles, using the apparatus described in the first aspect, comprising the following steps: S1. Prepare a silver nitrate solution as a silver source and add it through the first inlet; S2. Prepare the dispersant solution and add it through the second feed inlet; S3. Prepare the reducing agent solution and add it through the third inlet; After the three solutions are mixed and reacted in a microfluidic reactor, the product is collected from the outlet of the main pipeline.

[0013] As a further improvement of this application, in step S2, the dispersant is one or two of polyvinylpyrrolidone, stearic acid, oleic acid, Tween, and gum arabic; in the nano silver solution system, the concentration ratio of the silver nitrate solution to the dispersant solution is 1:(1-5); in the nano silver powder system, the concentration ratio of the silver nitrate solution to the dispersant solution is (30-35):1.

[0014] As a further improvement of this application, in step S3, the reducing agent is ascorbic acid or sodium borohydride, and the concentration ratio of the reducing agent solution to the silver nitrate solution is 1:(1-3).

[0015] As a further improvement to this application, the reaction temperature is controlled at 20-40℃ using a constant temperature water bath.

[0016] The beneficial effects of this application are as follows: This application provides an apparatus and method for the continuous preparation of silver nanoparticles. The apparatus includes a microfluidic reactor, a constant-temperature water bath, and an ultrasonic system. The microfluidic reactor has three inlets: a first inlet, a second inlet, and a third inlet. A first circular buffer chamber is provided at the first inlet, and a second circular buffer chamber is provided at the second inlet. The outlets of the first and second circular buffer chambers are connected in a Y-shape to form a first confluence pipe. The outlet of the first confluence pipe is connected to a first distributor. The outlet of the third inlet is connected to the second distributor. The outlets of the first and second distributors are connected to the inlet of a main pipeline. A peristaltic pump is installed on each feed pipe of the microfluidic reactor. This application achieves continuous and efficient production with mild and controllable reaction conditions, uniform and narrowly distributed silver nanoparticle size, and minimal pipeline clogging by using circular buffer chambers, an arc-shaped thin-tube distribution structure, and a constant-temperature ultrasonic environment.

[0017] The apparatus and method for continuous preparation of silver nanoparticles provided in this application effectively reduce local eddies and fluid impacts by setting circular buffer chambers at the first and second inlets, ensuring thorough and uniform premixing of the silver source and dispersant before entering the reaction zone. Simultaneously, the structural design of the first confluence pipe branching into three arc-shaped fine streams and the third inlet branching into three arc-shaped fine streams significantly increases the reaction contact area and reduces the flow rate, minimizing the instantaneous impact force and avoiding particle agglomeration and uneven growth caused by a sharp increase in local supersaturation. This results in silver nanoparticles with a narrow particle size distribution and good dispersibility. The entire apparatus is placed in a constant-temperature water bath to ensure stable and controllable reaction system temperature. Placing it in an ultrasonic environment not only facilitates dispersion but also effectively prevents silver powder deposition and blockage in the pipes, ensuring reliable long-term continuous operation. Furthermore, the reaction time can be flexibly controlled by adjusting the main pipeline length, enabling controllable preparation of silver nanoparticles with different particle sizes. Compared to traditional reactor-based silver nanoparticle preparation apparatuses, this reactor has a larger specific surface area, resulting in a more complete reaction and a higher silver ion conversion rate. The device has a simple structure, is easy to operate, and operates under mild reaction conditions. It can continuously and efficiently produce nano-silver solutions or nano-silver powder. By adjusting the concentration, flow rate, and subsequent processing methods of each feed inlet, the production of the two products can be flexibly switched on the same device, making it suitable for large-scale industrial production.

[0018] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.

[0020] Figure 1 A schematic diagram of the apparatus for the continuous preparation of silver nanoparticles provided in an embodiment of this application; Figure 2 This is a particle size distribution diagram of the nano-silver solution prepared in Example 2 of this application; Figure 3 This is a SEM image of the silver nanopowder prepared in Example 3 of this application; Figure 4 This is a SEM image of the silver nanopowder prepared in Example 4 of this application; Figure 5 SEM image of the silver nanoparticles prepared in Comparative Example 1; Explanation of reference numerals in the attached drawings: 1. First feed inlet; 2. Second feed inlet; 3. Third feed inlet; 4. First circular buffer chamber; 5. Second circular buffer chamber; 6. First confluence pipe; 7. First distributor; 8. Second distributor; 9. Main pipeline; 10. Collection device. Detailed Implementation

[0021] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0023] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0024] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0025] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0026] In the description of the embodiments of this application, the technical terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0027] In the description of the embodiments of this application, unless otherwise expressly specified and limited, technical terms such as "installation," "connection," "joining," and "fixing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. For those skilled in the art, the specific meaning of the above terms in the embodiments of this application can be understood according to the specific circumstances.

[0028] Silver powder has excellent electrical and thermal conductivity and is widely used in electronics, automotive, medical, aerospace and other fields. However, as electronic components develop towards miniaturization and integration, the quality requirements for silver powder are increasing. Existing methods for preparing nano-silver are mainly based on chemical reduction, which is limited by the volume of the reactor and has insufficient production capacity. Although a technology for continuous preparation using impinging flow microreactors has emerged, existing devices mostly adopt a vertical impingement structure, which results in large feeding impact force, uneven mixing, and easy agglomeration of silver particles with a wide particle size distribution. Furthermore, the pipeline is prone to blockage during continuous operation, making it difficult to meet the needs of large-scale industrial production.

[0029] To address the technical problems of excessive feed impact leading to severe particle agglomeration, uneven particle size distribution, and easy clogging in existing continuous nano-silver preparation devices, this application provides a device and method for continuous preparation of nano-silver. The method involves setting up a circular buffer chamber at the feed inlet to reduce fluid impact and achieve uniform premixing. Then, a distributor diverts the combined material through multiple arc-shaped fine streams to increase the contact area, reduce the flow rate, and weaken the instantaneous impact force of the reaction. Simultaneously, combined with constant-temperature water bath control and ultrasonic-assisted dispersion and cleaning, the method achieves the technical effects of mild and controllable reaction conditions, uniform and narrowly distributed nano-silver particle size, less clogging of the pipes, and continuous and efficient production of products with different particle sizes.

[0030] Please refer to Figure 1 In the first aspect, embodiments of this application provide an apparatus for the continuous preparation of nano-silver, including a microfluidic reactor, a constant temperature water bath and an ultrasonic system. The microfluidic reactor is provided with three feed inlets, namely a first feed inlet 1, a second feed inlet 2 and a third feed inlet 3. The first feed inlet 1 is provided with a first circular buffer chamber 4, and the second feed inlet 2 is provided with a second circular buffer chamber 5. The outlet end of the first circular buffer chamber 4 and the outlet end of the second circular buffer chamber 5 are connected in a Y-shape to form a first confluence pipe 6. The outlet end of the first confluence pipe 6 is connected to the first distributor 7; the outlet end of the third feed inlet 3 is connected to the second distributor 8; the outlet ends of the first distributor 7 and the second distributor 8 are connected to the inlet end of the main pipeline 9. The feed pipes of the microfluidic reactors are all equipped with peristaltic pumps.

[0031] In the technical solution of this application embodiment, the device uses a circular buffer chamber to achieve mild premixing and uniform coating of silver source and dispersant, and then uses a splitter to divide the two materials to increase the contact area, reduce the flow rate, weaken the reaction impact, and avoid agglomeration; combined with constant temperature water bath temperature control and ultrasonic-assisted dispersion, it can achieve continuous preparation with controllable particle size, uniform dispersion and long-term stable operation.

[0032] Furthermore, in some embodiments, both the first splitter 7 and the second splitter 8 include three arc-shaped thin tubes.

[0033] In the technical solution of this application embodiment, the total contact area of ​​the reaction interface is increased by diverting the flow, which significantly improves the mixing efficiency and reaction uniformity. At the same time, the flow guiding effect of the arc-shaped pipe is used to further reduce the fluid linear velocity and suppress turbulent pulsation, so that the two materials can contact each other smoothly in laminar flow with minimal impact force. This effectively avoids local oversaturation and crystal nucleus proliferation caused by the instantaneous violent reaction between the silver source and the reducing agent, thereby controlling the uniform growth of particles at the source and ensuring the narrow particle size distribution of the product.

[0034] Furthermore, in some embodiments, the length of the pipe for the first inlet 1 is 0.3-0.8m and the inner diameter of the pipe is 5-12cm; the length of the pipe for the second inlet 2 is 0.3-0.8m and the inner diameter of the pipe is 3-8cm; and the length of the pipe for the third inlet 3 is 0.3-0.8m and the inner diameter of the pipe is 3-8cm.

[0035] In the technical solution of this application embodiment, a suitable pipeline length can provide sufficient flow development space for each solution before entering the reaction zone, making the fluid state tend to be stable and avoiding uneven flow velocity distribution due to excessively short pipelines, which would affect the mixing effect. At the same time, a suitable pipeline diameter can match the flow rate and velocity of the reactants, preventing pipeline deposition or insufficient mixing due to excessively low flow velocity. The three inlets synchronously coordinate and control the reaction process of the three fluids, further improving the overall stability and controllability of the reaction system. Preferably, the pipeline length of the first inlet 1 is 0.5m and the inner diameter is 8cm; the pipeline length of the second inlet 2 is 0.5m and the inner diameter is 5cm; and the pipeline length of the third inlet 3 is 0.5m and the inner diameter is 5cm.

[0036] Furthermore, in some embodiments, the microfluidic reactor is entirely housed in a constant-temperature water bath and simultaneously placed in the ultrasonic field environment of the ultrasonic system.

[0037] In the technical solution of this application embodiment, the entire microfluidic reactor is placed in a constant-temperature water bath, and the reaction system is precisely temperature-controlled using a constant-temperature circulating medium. This ensures that the reaction process is always within the optimal temperature window, avoiding the impact of temperature fluctuations on the uniformity of the nano-silver particle size and batch consistency. Simultaneously, the entire reactor is placed in the ultrasonic field environment of an ultrasonic system. The cavitation effect and microjets generated by ultrasonic oscillation promote the diffusion and mixing of reactant molecules at the microscale, making the reaction more complete and uniform. Furthermore, they provide continuous online cleaning of the pipe walls, effectively preventing the adsorption and deposition of silver particles on the pipe surface and avoiding pipe blockage caused by long-term continuous operation. The synergistic cooperation between the constant-temperature water bath and the ultrasonic system contributes to the stability and controllability of the reaction conditions, ensuring the reliability of long-term continuous operation of the equipment.

[0038] Furthermore, in some embodiments, the discharge end of the main pipeline 9 is connected to a collection device 10.

[0039] In the technical solution of this application embodiment, the nano-silver product solution after being fully reacted in the microfluidic reactor flows directly into the collection device 10 for centralized storage after the set reaction time is completed, realizing a continuous production process; with the flexible adjustment of the length of the main pipeline discharge pipe, the residence time of the reactants in the pipeline can be precisely controlled, thereby obtaining nano-silver products with different particle size specifications at the collection end.

[0040] Secondly, embodiments of this application provide a method for the continuous preparation of silver nanoparticles, using the above-mentioned apparatus for the reaction, including the following steps: S1. Prepare a silver nitrate solution as a silver source and add it through the first inlet 1; S2. Prepare a dispersant solution and add it through the second feed inlet 2; S3. Prepare the reducing agent solution and add it through the third feed inlet 3; After the three solutions are mixed and reacted in a microfluidic reactor, the product is collected from the outlet of main pipeline 9. Depending on whether the target product is a nano-silver solution or nano-silver powder, the appropriate concentration system, type of reducing agent, and post-treatment method are selected.

[0041] In the technical solution of this application embodiment, the silver source, dispersant solution and reducing agent solution are continuously pumped into the first feed port 1, the second feed port 2 and the third feed port 3 at a set flow rate. The silver source and dispersant are first gently premixed in a circular buffer chamber to make the dispersant uniformly coat the silver source. Then the mixture and reducing agent are split by a splitter and then merged in the form of multiple arc-shaped fine streams. The reduction reaction is carried out under mild conditions that increase the contact area, reduce the flow rate and weaken the reaction impact. Combined with the precise temperature control of the constant temperature water bath and the ultrasonic field-assisted dispersion and cleaning, the uniform nucleation and controllable growth of nano-silver are realized. Finally, the product is continuously collected from the outlet of the main pipeline 9. The entire process can stably produce nano-silver products with uniform particle size and good dispersibility by flexibly adjusting the concentration and flow rate of each feed port. It can also run continuously for a long time without clogging and is suitable for large-scale industrial production. Preferably, in the nano-silver solution system, the concentration of silver nitrate solution is 0.1-1 g / L, the concentration of dispersant solution is 0.1-4 g / L, and the concentration of reducing agent solution is 0.1-2 g / L; or, in the nano-silver powder system, the concentration of silver nitrate solution is 0.1-2 g / mL, the concentration of dispersant solution is 0.01-0.1 g / mL, and the concentration of reducing agent solution is 0.1-1 g / mL.

[0042] Furthermore, in some embodiments, in step S2, the dispersant is one or two of polyvinylpyrrolidone, stearic acid, oleic acid, Tween, and gum arabic; in the nano-silver solution system, the concentration ratio of silver nitrate solution to dispersant solution is 1:(1-5); in the nano-silver powder system, the concentration ratio of silver nitrate solution to dispersant solution is (30-35):1.

[0043] In the technical solution of this application embodiment, the polar groups in the dispersant molecule structure are used to selectively adsorb onto the surface of newly formed silver particles to form a steric hindrance or electrostatic repulsion layer, which effectively prevents the aggregation and coalescence of particles. Controlling the concentration ratio of dispersant to silver nitrate within a suitable range helps the dispersant in the system to form a complete and dense adsorption coating layer on the surface of silver particles, preventing particles from being exposed and agglomerated due to insufficient dispersant. At the same time, it avoids the formation of multilayer adsorption on the particle surface or the increase of system viscosity due to excessive dispersant, which would affect the reaction mass transfer efficiency and product purity.

[0044] Furthermore, in some embodiments, in step S3, the reducing agent is ascorbic acid or sodium borohydride, and the concentration ratio of the reducing agent solution to the silver nitrate solution is 1:(1-3).

[0045] In the technical solution of this application embodiment, the reducing agent utilizes its reducing power to achieve a controllable conversion of silver ions into silver atoms, avoiding particle agglomeration caused by excessively strong reducing power leading to excessively rapid nucleation rate, or incomplete reaction and low conversion rate caused by insufficient reducing power. Controlling the concentration ratio of reducing agent to silver nitrate within an appropriate range helps silver ions to be slowly and continuously reduced to silver atoms, keeping the concentration of silver atoms in the system at a low supersaturation level, which is conducive to the uniform formation and slow growth of crystal nuclei, effectively avoiding instantaneous explosive nucleation and subsequent Ostwald ripening caused by excessive reducing agent, thereby obtaining fine-sized and concentrated silver nanoparticles. In addition, the reduction reaction rate of the reducing agent and the coating rate of the dispersant reach a dynamic balance, further ensuring the monodispersity and batch stability of the product.

[0046] Furthermore, in some embodiments, the reaction temperature is controlled at 20-40°C using a constant temperature water bath.

[0047] In the technical solution of this application embodiment, within a suitable temperature range, the reaction system can obtain sufficient activation energy to drive the reduction reaction of silver ions at a suitable rate, avoiding the decomposition and failure of the reducing agent, the breakage of the dispersant molecular chain, or the agglomeration of particles due to intensified thermal motion caused by excessively high temperatures. Simultaneously, it prevents the problem of excessively slow reaction rates and low conversion rates when the temperature is too low. This temperature range is matched with the aforementioned feed inlet pipeline parameters, flow distribution structure, and flow rate settings, ensuring that the reactants remain in a constant thermodynamic state as they flow through each section of the pipeline. This ensures the consistency of the silver atom generation rate, the number of crystal nuclei formed, and the growth process, thereby guaranteeing a high degree of repeatability in the particle size distribution and morphology of each batch of product.

[0048] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0049] Example 1 This embodiment provides an apparatus for the continuous preparation of nano-silver, see [link to apparatus]. Figure 1 The system includes a microfluidic reactor, a constant temperature water bath, and an ultrasonic system. The microfluidic reactor has three inlets: inlet 1, inlet 2, and inlet 3. Inlet 1 has a pipe length of 0.5m and an inner diameter of 8cm; inlet 2 has a pipe length of 0.5m and an inner diameter of 5cm; and inlet 3 has a pipe length of 0.5m and an inner diameter of 5cm. Inlet 1 is used to add a silver source; inlet 2 is used to add a dispersant; and inlet 3 is used to add a reducing agent. A first circular buffer chamber 4 is provided at the first feed inlet 1, and a second circular buffer chamber 5 is provided at the second feed inlet 2. The outlet ends of the first circular buffer chamber 4 and the second circular buffer chamber 5 are connected in a Y-shape to form a first confluence pipe 6. The outlet end of the first confluence pipe 6 is connected to a first distributor 7. The outlet end of the third feed inlet 3 is connected to a second distributor 8. Both the first distributor 7 and the second distributor 8 include three arc-shaped thin tubes. The outlet ends of the first distributor 7 and the second distributor 8 are connected to the inlet end of the main pipeline 9. Peristaltic pumps are installed on the feed pipelines of the first feed inlet 1, the second feed inlet 2, and the third feed inlet 3. The entire microfluidic reactor is set in an ultrasonic field environment of a constant temperature water bath and an ultrasonic system.

[0050] Example 2 This embodiment provides a method for the continuous preparation of silver nanoparticles, using the apparatus provided in Example 1 to continuously prepare silver nanoparticle solutions, including the following steps: A silver nitrate solution with a concentration of 0.24 g / L was prepared as the silver source and introduced into the first feed inlet 1 at a flow rate of 1.6 L / min. A polyvinylpyrrolidone (PVP) solution with a concentration of 0.47 g / L was prepared as a dispersant and fed into the second inlet 2 at a flow rate of 100 mL / min. A sodium borohydride solution with a concentration of 0.23 g / L was prepared as a reducing agent and introduced into the third feed inlet 3 at a flow rate of 250 mL / min. The three solutions mentioned above enter the microfluidic reactor through their respective inlets. Before merging, the silver nitrate solution and PVP solution are buffered and slowed down by circular buffer chambers on their respective inlets to eliminate local eddies, and then gently merge in a Y-shape, so that the PVP can fully and uniformly coat the silver source before the reaction. Subsequently, the mixture of silver source and PVP is split into three arc-shaped fine streams by the three arc-shaped fine stream tubes of the first splitter 7, and the sodium borohydride solution is split into three arc-shaped fine streams by the second splitter 8. The fine streams merge in a Y-shape and are connected to the main pipeline 9, which is 5m long. The reduction reaction is carried out under mild conditions that increase the reaction contact area, reduce the flow rate, and weaken the reaction impact. The reaction temperature is controlled at 30°C by a constant temperature water bath, and the entire device is placed in a 40kHz ultrasonic environment. After the reaction is completed, the nano-silver product is collected from the outlet of the main pipeline 9.

[0051] The particle size of the nano-silver solution prepared in this embodiment was tested, and the results are shown in Table 1 and 2. Figure 2 As can be seen, the nano-silver solution prepared by this device has uniform particle size, and the device runs continuously for 48 hours without any clogging, and the particle size remains stable.

[0052] Table 1 Test Results of Example 2 Example 3 This embodiment provides a method for the continuous preparation of silver nanoparticles, using the apparatus provided in Example 1 to continuously prepare silver nanoparticle powder, including the following steps: A silver nitrate solution with a concentration of 0.375 g / mL was prepared as the silver source and introduced into the first feed inlet 1 at a flow rate of 60 mL / min. A polyvinylpyrrolidone (PVP) solution with a concentration of 0.012 g / mL was prepared as a dispersant and fed into the second inlet 2 at a flow rate of 24 mL / min. An ascorbic acid solution with a concentration of 0.224 g / mL was prepared and used as a reducing agent, and fed into the third feed inlet 3 at a flow rate of 60 mL / min. The three solutions mentioned above are fed into the microfluidic reactor through their respective inlets. The main pipeline is 5m long, the reaction temperature is 30℃, and the entire device is placed in an 80kHz ultrasonic environment. After the reaction is completed, the nano-silver powder product is collected from the outlet of the main pipeline 9. After sedimentation, washing, and drying, nano-silver powder is obtained with a yield of 99.7%. This is because the continuous flow device has a large reaction contact area, the reaction is more complete, the silver ion conversion rate is higher, and nano-silver powder can be continuously prepared, making it suitable for industrial production.

[0053] The particle size of the nano-silver powder prepared in this embodiment was tested, and the results are shown in Table 2 and 3. Figure 3 As can be seen, the silver powder parameters are stable, and the equipment operates without clogging for a long time, making it suitable for large-scale production.

[0054] Table 2 Test Results of Example 3 Example 4 This embodiment provides a method for the continuous preparation of nano-silver. Compared with Example 3, the only difference is that the length of the main pipeline 9 is increased to 10m, while the other reaction conditions are basically the same as in Example 3.

[0055] The particle size of the nano-silver powder prepared in this embodiment was tested, and the results are shown in Table 3 and 4. Figure 4 It can be seen that adjusting the length of the main pipeline to control the reaction time can produce nano-silver powder products with different particle sizes.

[0056] Table 3 Test Results of Example 4 Comparative Example 1 Comparative Example 1 provides an apparatus for the continuous preparation of nano-silver. Compared with Example 1, the only difference is that the first circular buffer chamber 4 and the second circular buffer chamber 5 are not provided, and the first feed port 1 and the second feed port 2 are directly connected in a Y-shape.

[0057] Using this apparatus to prepare nano-silver powder, with the same concentration and flow rate of raw materials as in Example 3, the prepared silver powder is as follows: Figure 5 As shown in Table 4, the particle size test results show that due to the lack of a buffer chamber, the silver source in the first feed port 1 and the dispersant in the second feed port 2 are not mixed evenly, and the dispersant is difficult to uniformly coat the silver source, resulting in obvious agglomeration of the prepared silver powder.

[0058] Table 4. Test results of Comparative Example 1 Comparative Example 2 Comparative Example 2 provides an apparatus for the continuous preparation of nano-silver. Compared with Example 1, the only difference is that the first splitter 7 and the second splitter 8 are not provided. After the first feed port 1 and the second feed port 2 merge, they are directly connected to the third feed port 3 in a Y-shape.

[0059] The device was used to prepare nano-silver solutions. The same concentration and flow rate of raw materials as in Example 3 were used. The particle size of the prepared silver powder is shown in Table 5. Due to the lack of a flow divider, the silver source and the reducing agent collided directly, resulting in a small instantaneous reaction contact area and a significantly wider particle size distribution of the prepared silver powder.

[0060] Table 5. Test results of Comparative Example 2 It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. An apparatus for the continuous preparation of nano-silver, characterized in that, It includes a microfluidic reactor, a constant temperature water bath, and an ultrasonic system. The microfluidic reactor is provided with three feed inlets, namely a first feed inlet, a second feed inlet, and a third feed inlet. The first feed inlet is provided with a first circular buffer chamber, and the second feed inlet is provided with a second circular buffer chamber. The outlet end of the first circular buffer chamber and the outlet end of the second circular buffer chamber are connected in a Y-shape to form a first confluence pipe. The outlet end of the first confluence pipe is connected to the first distributor; the outlet end of the third feed inlet is connected to the second distributor; the outlet ends of the first distributor and the second distributor are connected to the inlet end of the main pipeline. The feed pipes of the microfluidic reactors are all equipped with peristaltic pumps.

2. The apparatus for continuous preparation of nano-silver according to claim 1, characterized in that, Both the first and second splitters include three arc-shaped thin tubes.

3. The apparatus for continuous preparation of nano-silver according to claim 1, characterized in that, The first inlet has a pipe length of 0.3-0.8m and an inner diameter of 5-12cm; the second inlet has a pipe length of 0.3-0.8m and an inner diameter of 3-8cm; and the third inlet has a pipe length of 0.3-0.8m and an inner diameter of 3-8cm.

4. The apparatus for continuous preparation of nano-silver according to claim 1, characterized in that, The first inlet has a pipe length of 0.5m and an inner diameter of 8cm; the second inlet has a pipe length of 0.5m and an inner diameter of 5cm; and the third inlet has a pipe length of 0.5m and an inner diameter of 5cm.

5. The apparatus for continuous preparation of nano-silver according to claim 1, characterized in that, The microfluidic reactor is entirely housed within the constant temperature water bath and simultaneously placed within the ultrasonic field environment of the ultrasonic system.

6. The apparatus for continuous preparation of nano-silver according to claim 1, characterized in that, The discharge end of the main pipeline is connected to a collection device.

7. A method for continuously preparing nano-silver, comprising reacting using the apparatus described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Prepare a silver nitrate solution as a silver source and add it through the first inlet; S2. Prepare the dispersant solution and add it through the second feed inlet; S3. Prepare the reducing agent solution and add it through the third inlet; After the three solutions are mixed and reacted in a microfluidic reactor, the product is collected from the outlet of the main pipeline.

8. The method for continuous preparation of nano-silver according to claim 7, characterized in that, In step S2, the dispersant is one or two of polyvinylpyrrolidone, stearic acid, oleic acid, Tween, and gum arabic; in the nano silver solution system, the concentration ratio of the silver nitrate solution to the dispersant solution is 1:(1-5); in the nano silver powder system, the concentration ratio of the silver nitrate solution to the dispersant solution is (30-35):

1.

9. The method for continuous preparation of nano-silver according to claim 7, characterized in that, In step S3, the reducing agent is ascorbic acid or sodium borohydride, and the concentration ratio of the reducing agent solution to the silver nitrate solution is 1:(1-3).

10. The method for continuous preparation of silver nanoparticles according to claim 7, characterized in that, The reaction temperature is controlled at 20-40℃ using a constant temperature water bath.