High-temperature-resistant nano-copper material and preparation method thereof

By combining nano-copper powder with high-temperature resistant additives, grain boundary stabilizers, dispersants, and antioxidants, the problem of insufficient performance of copper materials in high-temperature environments has been solved, achieving high-temperature stability and performance consistency of the materials, and improving electrical and thermal conductivity as well as mechanical properties.

CN123149402APending Publication Date: 2026-11-24JIANGSU HANQIAO NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611474951.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing copper materials have insufficient high-temperature resistance in high-temperature environments. The addition of alloying elements may reduce electrical and thermal conductivity, and the limited interfacial bonding strength of ceramic particles leads to a decline in material performance.

Method used

By employing a combination of nano-copper powder, high-temperature resistant additives, grain boundary stabilizers, dispersants, and antioxidants, and through high-energy ball milling, ultrasonic dispersion, centrifugal separation, and sintering, a uniform microstructure is formed, thereby improving the high-temperature stability and performance consistency of the material.

Benefits of technology

It significantly improves the material's high-temperature resistance, electrical conductivity, and thermal conductivity, extends its service life, and enhances its mechanical properties and oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149402A_ABST
    Figure CN123149402A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of new material preparation technology, and discloses a high-temperature resistant nano-copper material and its preparation method. The high-temperature resistant nano-copper material includes the following components: nano-copper powder, high-temperature resistant additives, grain boundary stabilizers, dispersants, and antioxidants. The preparation method of the high-temperature resistant nano-copper material includes the following steps: S1, raw material pretreatment; S2, premixing and dispersing; S3, suspension preparation; S4, mixed powder preparation; S5, green body pressing; S6, green body sintering treatment. The high-temperature resistant nano-copper material of this invention has excellent high-temperature resistance, good microstructure uniformity, good mechanical properties, and good antioxidant capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of new material preparation technology, specifically to a high-temperature resistant nano-copper material and its preparation method. Background Technology

[0002] High-temperature resistant nano-copper materials hold a crucial position and have a wide range of applications in numerous high-tech fields and industrial applications. In the aerospace field, during high-speed flight, engine components and thermal protection systems of aircraft are subjected to extremely high temperatures. High-temperature resistant nano-copper materials, with their excellent high-temperature resistance and good electrical and thermal conductivity, can be used to manufacture high-temperature engine components, such as turbine blades and combustion chamber liners, effectively improving engine efficiency and reliability and extending its service life. In the electronics industry, as electronic devices develop towards miniaturization and high power density, chips generate a large amount of heat during operation. High-temperature resistant nano-copper materials can be used to manufacture high thermal conductivity heat dissipation substrates and thermal interface materials, rapidly transferring the heat generated by the chips and ensuring the stable operation of electronic devices. In the automotive industry, especially in high-performance and new energy vehicles, components such as engines and battery packs also generate high temperatures during operation. High-temperature resistant nano-copper materials can be used to manufacture heat dissipation components and conductive connectors for these parts, improving vehicle performance and safety.

[0003] Currently, there is considerable research on optimizing the performance of copper-based materials in specific industrial scenarios. Regarding copper material modification, some studies focus on adding alloying elements to improve the overall properties of copper. For example, adding elements such as chromium and zirconium to copper forms copper alloys. These alloying elements form dispersed precipitates in the copper matrix, hindering grain boundary movement and dislocation motion, thereby enhancing the strength and deformation resistance of the copper alloys. Other studies employ powder metallurgy to prepare copper-based composite materials, mixing copper powder with ceramic particles (such as alumina and silicon carbide), and then processing them through pressing and sintering to create composite materials. The aim is to leverage the properties of ceramic particles to enhance the specific properties of the composite materials.

[0004] However, existing copper material technologies still have some shortcomings. While adding alloying elements to copper alloys improves properties such as strength to some extent, their high-temperature resistance still falls short of the requirements of some extreme applications. Furthermore, the addition of alloying elements may reduce the electrical and thermal conductivity of copper, which is detrimental to applications requiring high electrical and thermal conductivity (such as heat dissipation components in the electronics industry). Copper-based composite materials prepared using powder metallurgy methods are prone to interfacial separation at high temperatures due to the limited interfacial bonding strength between ceramic particles and the copper matrix. This leads to a decline in the overall performance of the material, making it difficult to withstand prolonged high-temperature exposure and resulting in poor high-temperature resistance. Summary of the Invention

[0005] To address the above problems, this invention provides a high-temperature resistant nano-copper material and its preparation method, which is achieved through the following technical solutions.

[0006] A high-temperature resistant nano-copper material, by weight percentage, comprises the following components: 85%–95% nano-copper powder, 3%–7% high-temperature resistant additives, 1%–3% grain boundary stabilizer, 1%–2% dispersant, and 1%–2% antioxidant.

[0007] As a further embodiment of the present invention, the particle size of the nano-copper powder is in the range of 10nm-100nm, and the purity is not less than 99.5%; the high-temperature resistant additive is one of yttrium oxide, zirconium oxide, and aluminum oxide; the grain boundary stabilizer is one of yttrium, lanthanum, and cerium; the dispersant is one of polyvinylpyrrolidone and sodium dodecylbenzenesulfonate; and the antioxidant is vitamin E or tea polyphenols.

[0008] As a further embodiment of the present invention, the following components are included by weight percentage: 90% nano copper powder, 5% high-temperature resistant additive, 2% grain boundary stabilizer, 1.5% dispersant and 1.5% antioxidant.

[0009] A method for preparing high-temperature resistant copper nanomaterials includes the following steps: S1, raw material pretreatment, the nano copper powder, high temperature resistant additives, grain boundary stabilizers, dispersants and antioxidants are placed in a vacuum drying oven for drying; S2, Premixing and Dispersion: The raw materials that have been dried in step S1 are fed into a high-energy ball mill for high-energy ball milling to refine the raw materials and form a preliminary mixture. S3, the preliminary mixture is added to an organic solvent and then ultrasonically dispersed to form a suspension; S4, the suspension is centrifuged to obtain precipitate, and the precipitate is dried to obtain mixed powder; S5, the mixed powder is transferred into a graphite mold and cold-pressed to form a blank; S6. The blank is sintered to densify it, resulting in high-temperature resistant nano-copper material.

[0010] As a further embodiment of the present invention, in step S1, the nano copper powder is dried at a temperature of 80-120°C for 2-4 hours; the high-temperature resistant additives, grain boundary stabilizers, dispersants and antioxidants are dried at a temperature of 60-100°C for 1-3 hours.

[0011] As a further embodiment of the present invention, in step S2, the raw material is subjected to high-energy ball milling under an argon protective atmosphere, using stainless steel balls with a diameter of 5-15 mm as the ball milling medium, with a ball-to-material ratio of 15:1, a high-energy ball mill speed of 200-500 r / min, and a ball milling time of 2-6 h.

[0012] As a further embodiment of the present invention, in step S3, the organic solvent is anhydrous ethanol or acetone, and the amount of organic solvent used is 5-15 times the mass of the initial mixture; ultrasonic dispersion is performed using an ultrasonic wave with a frequency of 20-40kHz and a power of 100-300W for 10-30 minutes.

[0013] As a further embodiment of the present invention, in step S4, the suspension is placed in a centrifuge and centrifuged for 10-30 minutes at a speed of 3000-8000 r / min, and the supernatant is discarded to obtain the precipitate.

[0014] As a further embodiment of the present invention, in step S5, a layer of release agent is first uniformly applied to the inner wall of the graphite mold, and then the mixed powder is transferred in. The cold pressing pressure is 100-300 MPa, and the holding time is 5-15 min.

[0015] As a further embodiment of the present invention, in step S6, the billet is placed in a hot-press sintering furnace filled with hydrogen for sintering treatment. A segmented heating sintering method is adopted. First, the temperature is raised to 400-500℃ at a heating rate of 5-10℃ / min and held for 30-60min. Then, the temperature is raised to 800-950℃ at a heating rate of 3-8℃ / min, and a pressure of 20-50MPa is applied simultaneously. The temperature and pressure are then maintained for 1-3h.

[0016] The beneficial effects of this invention are as follows: 1. The addition of high-temperature resistant additives effectively improves the stability of the material in high-temperature environments. Under high-temperature conditions, these high-temperature resistant additives can form a stable structure in the copper matrix, hindering the movement of grain boundaries and the diffusion of dislocations, thereby inhibiting the growth of copper grains and the softening of the material, and significantly improving the high-temperature resistance of the material.

[0017] 2. High-energy ball milling refines the raw materials and forms a preliminary mixture, while ultrasonic dispersion further ensures uniform dispersion of the raw materials in an organic solvent, forming a suspension. Centrifugation then yields the precipitate. These steps effectively solve the problem of easy agglomeration of nanoparticles, allowing components such as nano-copper powder, high-temperature additives, grain boundary stabilizers, dispersants, and antioxidants to be uniformly distributed within the material. This uniform microstructure helps improve the overall performance of the material, making the performance of different parts more consistent under high-temperature conditions. This avoids material failure caused by localized performance differences, thus improving the material's reliability and service life. 3. The addition of grain boundary stabilizers plays an important role in enhancing the mechanical properties of materials. Grain boundary stabilizers can stabilize the grain boundary structure, reduce defects and stress concentration at the grain boundaries, thereby improving the strength and toughness of the materials.

[0018] 4. The addition of antioxidants effectively improves the material's antioxidant capacity. Under high temperature conditions, copper is prone to oxidation reaction with oxygen to form copper oxide, which leads to a decline in the material's performance. Antioxidants can form a protective film on the material surface to prevent oxygen from contacting copper, thereby inhibiting the occurrence of oxidation reaction. Attached Figure Description

[0019] To more clearly illustrate the technical solution of the present invention, the accompanying drawings used in the description of the specific embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 A flowchart of a method for preparing high-temperature resistant copper nanomaterials; Figure 2 : A schematic diagram of the composition of a high-temperature resistant nano-copper material; Figure 3 Parameter diagram of high-energy ball milling process; Figure 4 Product route diagram for the preparation of high-temperature resistant copper nanomaterials; Figure 5 Flowchart of sintering process. Detailed Implementation

[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] like Figure 1-5 As shown, a high-temperature resistant nano-copper material comprises the following components by weight percentage: The nano-copper powder comprises 85%–95%, specifically, the weight ratio of nano-copper powder is 90%, the particle size range of nano-copper powder is 10nm-100nm, and the purity is not less than 99.5%. The high-temperature resistant additive is 3% to 7%, specifically, the weight ratio of the high-temperature resistant additive is 5%, and the high-temperature resistant additive is one of yttrium oxide, zirconium oxide and aluminum oxide; The grain boundary stabilizer is 1% to 3%, specifically, the weight ratio of the grain boundary stabilizer is 2%, and the grain boundary stabilizer is one of yttrium, lanthanum and cerium; The dispersant is 1% to 2%, specifically, the weight ratio of the dispersant is 1.5%, and the dispersant is one of polyvinylpyrrolidone or sodium dodecylbenzenesulfonate; Antioxidants 1% to 2%, specifically, the weight ratio of antioxidants is 1.5%, and the antioxidants are vitamin E or tea polyphenols.

[0023] Nano-copper powder serves as the main component in this material, providing it with basic electrical and thermal conductivity, as well as a certain mechanical strength. Specifically: The particle size range of nano copper powder is 10nm-100nm. This particle size range enables the copper powder to have a large specific surface area, enhances the interaction with other components, and ensures the uniformity and stability of the material in microstructure. With a purity of not less than 99.5%, high-purity nano-copper powder can reduce the interference of impurities on material properties and improve the material's electrical conductivity, thermal conductivity, and high-temperature resistance.

[0024] High-temperature resistant additives interact with nano-copper powder under high-temperature conditions to form stable compounds or solid solutions, inhibiting the growth and coarsening of copper grains, thereby improving the high-temperature strength and stability of the material. Specifically, the high-temperature resistant additive is one of yttrium oxide, zirconium oxide, and alumina. When yttrium oxide is used, its particle size should be controlled between 50nm and 200nm. Too fine a particle size may lead to agglomeration, while too coarse a particle size will make it difficult to disperse uniformly in the nano-copper powder. Zirconia needs to be stabilized, such as partially stabilized zirconium oxide (PSZ) or fully stabilized zirconium oxide (FSZ), to avoid phase transformation at high temperatures that would cause volume changes and affect material properties. Alumina should have high purity (not less than 99.9%), and its surface needs to be specially treated to enhance its interfacial bonding ability with nano-copper powder.

[0025] Grain boundary stabilizers can adsorb at the grain boundaries of copper grains, reduce grain boundary energy, inhibit grain boundary migration and grain growth, and further improve the high-temperature stability and mechanical properties of the material. Specifically, grain boundary stabilizers are one of yttrium, lanthanum, and cerium. Yttrium is added in the form of yttrium nitrate, yttrium oxide, etc., and needs to be purified before addition to remove impurity ions. Lanthanum can be added in the form of metallic lanthanum or lanthanum compounds (such as lanthanum nitrate). Metallic lanthanum needs to be surface treated to prevent oxidation. Cerium is generally added in the form of cerium oxide. The particle size of cerium oxide should be uniform and have good dispersibility.

[0026] Dispersants enable other raw materials to be uniformly dispersed during the mixing process, preventing agglomeration and ensuring the uniformity of the material's microstructure, thereby improving the material's overall performance. Specifically, the dispersant is either polyvinylpyrrolidone or sodium dodecylbenzenesulfonate. The molecular weight of polyvinylpyrrolidone should be between 10,000 and 50,000. If the molecular weight is too low, the dispersion effect will be poor; if it is too high, it may lead to an increase in the viscosity of the material, affecting subsequent processing. Sodium dodecylbenzenesulfonate must be of industrial grade or higher purity and must be dissolved and diluted before use to achieve the best dispersion effect.

[0027] Antioxidants can effectively prevent nano-copper materials from undergoing oxidation reactions with oxygen at high temperatures, extending the service life of the materials and ensuring the performance stability of the materials under high temperature conditions. Specifically, vitamin E should be natural and have a purity of not less than 90%. It needs to be dissolved before being added to ensure that it can be evenly dispersed in the materials. Tea polyphenols can be high-purity products extracted from tea leaves.

[0028] A method for preparing high-temperature resistant copper nanomaterials includes the following steps: S1, raw material pretreatment: nano copper powder, high temperature resistant additives, grain boundary stabilizers, dispersants and antioxidants are placed in a vacuum drying oven for drying.

[0029] The nano-copper powder is dried at 80-120℃ for 2-4 hours. This temperature range and drying time setting are based on the characteristics of nano-copper powder. If the temperature is too low, the moisture and organic impurities adsorbed on the surface of the nano-copper powder cannot be effectively removed. These impurities may participate in the reaction during subsequent preparation, affecting the purity and performance of the material. If the temperature is too high or the drying time is too long, the nano-copper powder may undergo oxidation or agglomeration, changing its particle size distribution and microstructure, thereby affecting the material's electrical conductivity, thermal conductivity, and mechanical properties.

[0030] High-temperature resistant additives, grain boundary stabilizers, dispersants, and antioxidants are dried at 60-100℃ for 1-3 hours. These additives and auxiliaries differ in properties from nano-copper powder; their thermal stability is relatively poor, and excessively high temperatures may cause them to decompose or deteriorate, affecting their effectiveness in actual materials. For example, the dispersant polyvinylpyrrolidone may partially decompose at temperatures exceeding 100℃, reducing its dispersing ability; the antioxidant vitamin E is also easily oxidized at high temperatures, losing its antioxidant effect. Therefore, choosing a temperature range of 60-100℃ and a drying time of 1-3 hours effectively removes moisture and volatile impurities from these substances while ensuring their chemical stability.

[0031] S2, Premixing and Dispersion: The raw materials that have been dried in step S1 are fed into a high-energy ball mill for high-energy ball milling to refine the raw materials and form a preliminary mixture.

[0032] The raw materials are subjected to high-energy ball milling under an argon protective atmosphere, using stainless steel balls with a diameter of 5-15mm as the ball milling medium, with a ball-to-material ratio of 15:1, a high-energy ball mill speed of 200-500r / min, and a ball milling time of 2-6h.

[0033] When adding raw materials, first add nano copper powder, and then add other raw materials in sequence.

[0034] After the raw materials are fed in and the ball mill jar is sealed, connect the ball mill jar to the argon supply system. First, evacuate the ball mill jar by using a vacuum pump to remove the air inside the jar, so that the vacuum degree inside the jar reaches above -0.09MPa, in order to remove impurities such as oxygen and moisture from the jar and prevent the raw materials from undergoing oxidation during the ball milling process.

[0035] After vacuuming is complete, slowly fill the ball mill jar with high-purity argon gas (purity not less than 99.99%). During the filling process, closely monitor the pressure changes inside the ball mill jar to ensure a slightly positive pressure of 0.05-0.1 MPa. This slightly positive pressure prevents outside air from entering the ball mill jar during the milling process, ensuring a protective argon atmosphere for the process.

[0036] S3, the preliminary mixture is added to an organic solvent and then ultrasonically dispersed to form a suspension.

[0037] The organic solvent is anhydrous ethanol or acetone, and the amount of organic solvent is 5-15 times the mass of the initial mixture. Ultrasonic dispersion is performed using an ultrasonic wave with a frequency of 20-40kHz and a power of 100-300W for 10-30 minutes.

[0038] Anhydrous ethanol has low surface tension and good solubility, effectively wetting the surface of the initial mixture and making it easier to disperse. It also has moderate volatility, making it easy to remove in subsequent processing, and relatively low toxicity, making it friendly to operators and the environment. However, anhydrous ethanol has limited solubility for some highly polar additives. Acetone is a highly polar solvent with good solubility for many organic and inorganic substances. It can quickly penetrate into the interior of the initial mixture, disrupting the agglomeration structure between particles. Its high volatility allows it to accelerate solvent turnover and improve dispersion efficiency during ultrasonic dispersion. However, acetone has a certain degree of toxicity and flammability, requiring enhanced ventilation and fire prevention measures during operation.

[0039] Choose clean, dry glass beakers or plastic containers with good corrosion resistance as mixing containers. Glass beakers have high transparency, making it easy to observe the phenomena during the mixing process; plastic containers have the advantages of being lightweight and not easily broken. The volume of the container should be selected according to the total volume of the initial mixture and solvent, and generally 20%-30% margin should be left to prevent liquid from overflowing during stirring.

[0040] S4. The suspension is centrifuged to obtain a precipitate, and the precipitate is dried to obtain a mixed powder.

[0041] The suspension was placed in a centrifuge and centrifuged for 10-30 minutes at a speed of 3000-8000 r / min. The supernatant was discarded to obtain the precipitate.

[0042] Before transferring the suspension to centrifuge tubes, gently stir the suspension with a glass rod or magnetic stirrer to achieve homogenization, thus avoiding poor centrifugation results due to uneven particle distribution in the suspension. Accurately measure and transfer the homogenized suspension into centrifuge tubes, ensuring that the volume of suspension in each centrifuge tube is basically the same, generally not exceeding 2 / 3 of the centrifuge tube's volume, to prevent liquid overflow during centrifugation.

[0043] S5, the mixed powder is transferred into a graphite mold and cold-pressed to form a blank.

[0044] First, evenly coat the inner wall of the graphite mold with a layer of release agent, then transfer the mixed powder into it. The cold pressing pressure is 100-300MPa, and the holding time is 5-15min.

[0045] First, place the graphite mold in a cleaning tank and clean it with a suitable cleaning agent (such as alcohol, acetone, etc.) to remove oil, dust, and other impurities from the mold surface. After cleaning, dry the mold with clean compressed air to ensure that there is no moisture residue inside or on the surface of the mold.

[0046] Graphite emulsion is selected as the release agent. The thickness of the release agent should be controlled between 0.01-0.05mm. After application, the mold is placed in a well-ventilated environment to dry, so that the release agent forms a uniform and dense film.

[0047] S6. The blank is sintered to densify it, resulting in high-temperature resistant nano-copper material.

[0048] The billet is placed in a hot-press sintering furnace filled with hydrogen for sintering. A segmented heating sintering method is adopted. First, the temperature is raised to 400-500℃ at a heating rate of 5-10℃ / min and held for 30-60min. Then, the temperature is raised to 800-950℃ at a heating rate of 3-8℃ / min, and a pressure of 20-50MPa is applied simultaneously. The billet is held at this temperature and pressure for 1-3h.

[0049] The first stage, the low-temperature holding stage (heating at 5-10℃ / min to 400-500℃, holding for 30-60min): 1. The billet may still contain binder, moisture, and organic solvent residues. If the temperature rises too quickly, pores will form inside the billet, affecting the material's density and performance. This holding stage also helps these substances to completely volatilize, ensuring the purity of the billet. 2. During the process of heating the billet from room temperature to a higher temperature, thermal stress may occur due to differences in the heating rate of different parts. Slowly heating to 400-500℃ and holding at this temperature can gradually make the temperature of each part of the billet more uniform, reducing thermal stress caused by temperature gradients and lowering the risk of billet cracking. 3. During the low-temperature holding stage, the copper particles begin to have some thermal movement. Although the amplitude of movement is small, it can still cause a certain degree of rearrangement between the particles, eliminating some uneven contact between particles and laying a good foundation for the subsequent high-temperature densification process.

[0050] The second stage: High-temperature and high-pressure holding stage (heating to 800-950℃ at 3-8℃ / min, simultaneously applying 20-50MPa pressure and holding for 1-3 hours): 1. When the temperature rises to 800-950℃, copper atoms have higher energy and a faster diffusion rate. Simultaneously applying 20-50MPa pressure further increases the contact area between particles, promoting the diffusion and migration of copper atoms. Under the combined effect of high temperature and high pressure, the pores in the billet are gradually filled, and the bonding between particles becomes tighter, thus achieving densification of the billet and improving the density and strength of the material. 2. After high-temperature and high-pressure holding treatment, the microstructure of the material becomes more uniform and dense, reducing the presence of internal defects and pores. This can significantly improve the material's electrical conductivity, thermal conductivity, and other physical properties. For high-temperature resistant nano-copper materials, good electrical and thermal conductivity help maintain stable performance under high-temperature environments, reducing performance degradation caused by heat accumulation.

[0051] The entire sintering process is carried out in a hot pressurized sintering furnace filled with hydrogen, which acts as a protective atmosphere. Copper is prone to oxidation with oxygen at high temperatures, forming copper oxide, which affects the material's properties. Hydrogen has reducing properties and can react with any copper oxide that may be present on the surface of the green body, reducing it back to copper. This prevents the green body from being oxidized during sintering and ensures the purity and quality of the material.

[0052] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to any specific implementation. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention.

Claims

1. A high-temperature resistant nano-copper material, characterized in that, By weight percentage, it includes the following components: 85%–95% nano copper powder, 3%–7% high-temperature resistant additives, 1%–3% grain boundary stabilizers, 1%–2% dispersants, and 1%–2% antioxidants.

2. The high-temperature resistant nano-copper material according to claim 1, characterized in that, The nano-copper powder has a particle size range of 10nm-100nm and a purity of not less than 99.5%; the high-temperature resistant additive is one of yttrium oxide, zirconium oxide, and aluminum oxide; the grain boundary stabilizer is one of yttrium, lanthanum, and cerium; the dispersant is one of polyvinylpyrrolidone and sodium dodecylbenzenesulfonate; and the antioxidant is vitamin E or tea polyphenols.

3. The high-temperature resistant nano-copper material according to claim 1, characterized in that, By weight percentage, it includes the following components: 90% nano copper powder, 5% high-temperature resistant additive, 2% grain boundary stabilizer, 1.5% dispersant and 1.5% antioxidant.

4. A method for preparing high-temperature resistant nano-copper material as described in any one of claims 1-3, characterized in that, Includes the following steps: S1, raw material pretreatment, the nano copper powder, high temperature resistant additives, grain boundary stabilizers, dispersants and antioxidants are placed in a vacuum drying oven for drying; S2, Premixing and Dispersion: The raw materials that have been dried in step S1 are fed into a high-energy ball mill for high-energy ball milling to refine the raw materials and form a preliminary mixture. S3, the preliminary mixture is added to an organic solvent and then ultrasonically dispersed to form a suspension; S4, the suspension is centrifuged to obtain precipitate, and the precipitate is dried to obtain mixed powder; S5, the mixed powder is transferred into a graphite mold and cold-pressed to form a blank; S6. The blank is sintered to densify it, resulting in high-temperature resistant nano-copper material.

5. The method for preparing a high-temperature resistant nano-copper material according to claim 4, characterized in that, In step S1, the nano-copper powder is dried at 80-120°C for 2-4 hours; the high-temperature resistant additives, grain boundary stabilizers, dispersants, and antioxidants are dried at 60-100°C for 1-3 hours.

6. The method for preparing a high-temperature resistant nano-copper material according to claim 4, characterized in that, In step S2, the raw material is subjected to high-energy ball milling under an argon protective atmosphere, using stainless steel balls with a diameter of 5-15 mm as the ball milling medium, with a ball-to-material ratio of 15:1, a high-energy ball mill speed of 200-500 r / min, and a ball milling time of 2-6 h.

7. The method for preparing a high-temperature resistant nano-copper material according to claim 4, characterized in that, In step S3, the organic solvent is anhydrous ethanol or acetone, and the amount of organic solvent used is 5-15 times the mass of the initial mixture; ultrasonic dispersion is performed using an ultrasonic wave with a frequency of 20-40kHz and a power of 100-300W for 10-30 minutes.

8. The method for preparing a high-temperature resistant nano-copper material according to claim 4, characterized in that, In step S4, the suspension is placed in a centrifuge and centrifuged for 10-30 minutes at a speed of 3000-8000 r / min, and the supernatant is discarded to obtain the precipitate.

9. The method for preparing a high-temperature resistant nano-copper material according to claim 4, characterized in that, In step S5, a layer of release agent is first evenly applied to the inner wall of the graphite mold, and then the mixed powder is transferred in. The cold pressing pressure is 100-300 MPa, and the holding time is 5-15 min.

10. The method for preparing a high-temperature resistant nano-copper material according to claim 4, characterized in that, In step S6, the billet is placed in a hot-press sintering furnace filled with hydrogen for sintering treatment. A segmented heating sintering method is adopted. First, the temperature is raised to 400-500℃ at a heating rate of 5-10℃ / min and held for 30-60min. Then, the temperature is raised to 800-950℃ at a heating rate of 3-8℃ / min, and a pressure of 20-50MPa is applied simultaneously. The temperature and pressure are then maintained for 1-3h.