Microfine high purity sponge ruthenium powder, process for its preparation and use
The preparation of three-dimensional interconnected sponge-like ruthenium powder by ammonia hydrolysis and plasma reduction process has solved the problem of preparing high-purity ruthenium powder, and achieved high-purity, fine-particle-size, sponge-like ruthenium powder, which improves sputtering performance and production efficiency and reduces energy consumption.
Patent Information
- Application Number
- CN202611020024.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-09
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to produce high-purity, fine-particle-size, sponge-like ruthenium powder, leading to abnormal discharges and decreased film uniformity during sputtering. Furthermore, traditional processes suffer from impurity introduction and high energy consumption.
Using ammonia as the solvent for hydrolyzing and precipitating ruthenium, combined with low-temperature aging and plasma reduction processes, a fine, high-purity sponge ruthenium powder with a three-dimensional interconnected sponge-like continuous network structure was prepared. This avoided ball milling and air jet milling, and improved the purity and dispersibility of the ruthenium powder.
The preparation of high-purity ruthenium powder was achieved, avoiding abnormal discharge during the sputtering process, ensuring uniform film deposition, and significantly improving the direct recovery rate and production efficiency of precious metals while reducing energy consumption.
Smart Images

Figure CN123149403A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of powder metallurgy technology, specifically relating to fine high-purity sponge ruthenium powder, its preparation method, and its application. Background Technology
[0002] Ruthenium metal possesses a high melting point, excellent thermal stability, and chemical inertness, making it suitable for high-purity, high-precision coating in advanced semiconductor processes and widely used as a high-performance thin-film sputtering target. As semiconductors evolve towards miniaturization and high density, the technical requirements for diffusion barrier layer materials are continuously increasing, leading to a growing demand for ruthenium targets. Domestically produced ruthenium powder generally falls short of the purity requirements for sputtering targets, and bottlenecks such as uneven powder particle size distribution and insufficient control over particle morphology in existing processes urgently need to be addressed. Innovation in purification processes is needed to overcome these bottlenecks in high-end ruthenium targets and meet the electronics industry's demand for high-performance materials.
[0003] Currently, the preparation of spherical ruthenium powder suffers from insufficient purity and low density due to immature domestic technology. High impurities can lead to abnormal discharge during sputtering and reduced film uniformity. In contrast, sponge ruthenium, with its irregular porous structure, exhibits good overall dispersion and is less prone to agglomeration. This makes it easier to achieve a uniform structure through mixing during target processing, and high-density targets can be obtained after hot-pressing and sintering. Traditional tube furnace hydrogenation reduction processes have low direct recovery rates for precious metals and introduce new impurities and free oxygen. Therefore, this application optimizes and improves the morphology of ruthenium powder prepared by existing technologies while addressing the issue of low product purity. Summary of the Invention
[0004] In view of the problems existing in the background art, this application provides a fine high-purity sponge ruthenium powder, its preparation method and application.
[0005] To achieve the above objectives, this application adopts the following technical solution: In a first aspect, a fine high-purity sponge ruthenium powder is provided. The sponge ruthenium powder is a three-dimensional interconnected sponge-like continuous network structure. The sponge-like continuous network structure is formed by several ruthenium grains being fused together by neck-shaped connections. The ruthenium grains have smooth surfaces and clear grain boundaries. Micron-level pores are distributed inside the continuous network. The purity of the sponge ruthenium powder is above 99.9%.
[0006] Furthermore, the ruthenium grains have a grain size of 0.5 μm to 3 μm.
[0007] Furthermore, the width of the neck-shaped connection is 0.3 μm to 2 μm.
[0008] Furthermore, the lateral dimensions of the sponge ruthenium powder are 5μm to 15μm.
[0009] Furthermore, the purity of the sponge ruthenium powder is 99.99% or higher, preferably 99.995% or higher.
[0010] Secondly, a method for preparing fine, high-purity sponge ruthenium powder is provided, comprising: (1) Add ruthenium trichloride solution dropwise to ammonia solution under stirring conditions, and keep the reaction at 50~80℃ to obtain reaction slurry; (2) The reaction slurry is rapidly cooled and aged in a low-temperature environment to obtain an aged slurry. The aged slurry is then subjected to solid-liquid separation to obtain a solid. The solid is then washed and dried to obtain a dark brown powder. (3) The dark brown powder was reduced under a high-temperature reducing atmosphere of plasma to obtain fine high-purity sponge ruthenium powder.
[0011] Thirdly, a ruthenium target is provided, which is prepared by using the fine high-purity sponge ruthenium powder described in the first aspect or the fine high-purity sponge ruthenium powder prepared by the preparation method described in the second aspect.
[0012] The micro-fine high-purity sponge ruthenium powder provided in this application has a three-dimensional interconnected sponge-like continuous network structure, formed by neck-shaped fusion of ruthenium grains. It has a smooth surface, clear grain boundaries, and micron-level pores distributed internally, with a purity ≥99.9%. The high purity of this sponge ruthenium powder ensures no abnormal discharge during sputtering, guaranteeing uniform film deposition. The porous network structure endows the powder with excellent dispersibility and anti-agglomeration ability, resulting in uniform target mixing and high hot-pressing density. It directly forms a micro-fine sponge morphology, eliminating the need for ball milling or airflow pulverization, thus avoiding the introduction of impurities and free oxygen from the source and significantly improving the direct recovery rate of precious metals.
[0013] The provided preparation process uses a suitable ruthenium precipitation precursor, ammonia as the solvent for hydrolyzing ruthenium precipitation, hydrolyzes and precipitates ruthenium at a certain temperature, and combines it with subsequent low-temperature aging and plasma reduction processes to prepare high-purity, fine-particle-size, sponge-like ruthenium powder. This preparation process requires only one precipitation step, does not require additional purification treatment, generates less wastewater, and is environmentally friendly.
[0014] Ammonia exhibits variable-temperature evaporation characteristics in power cycles. Increasing the ammonia concentration can optimize its thermal matching with the heat source and reduce heat exchange temperature difference losses. Applying this characteristic to the ruthenium precipitation process, ammonia may reduce external heating requirements by regulating the temperature distribution of the reaction system, thereby lowering energy consumption. Simultaneously, timely collection and recycling of ammonia volatilization during the reaction can reduce resource waste and improve overall process efficiency.
[0015] Low-temperature aging can directionally regulate hydrolysis by extending the reaction time, reducing the influence of temperature on the system, overcoming thermodynamic limitations, maintaining a high-polarity water temperature environment, avoiding random nucleation and lattice defects caused by high temperature, and making the overall grain size distribution uniform.
[0016] Plasma reduction powdering activates ruthenium dioxide with high-energy plasma, significantly accelerating the reduction reaction kinetics, thereby shortening the powdering cycle and improving production efficiency. This speed improvement stems from the high electron density and active particles of plasma, directly enhancing the reaction rate, while traditional methods (hydrogen reduction or carbothermic reduction) require prolonged high-temperature treatment, and the reaction rate is limited by thermal diffusion. Furthermore, the plasma process achieves high-efficiency energy conversion through optimized energy transfer, significantly reducing the energy consumption per unit of ruthenium powder produced. Existing technologies (such as electric arc furnaces or chemical reduction furnaces) require maintaining a high-temperature environment, resulting in high energy consumption and low thermal efficiency. The reaction atmosphere under plasma conditions is controllable, effectively avoiding the introduction of impurities, and the oxygen content can be reduced to below 200 ppm. By adjusting plasma parameters (power, gas flow rate), the preparation requirements for nanoscale powders can be met. Under the influence of surface tension, the molten droplets form powders with good flowability and a certain increase in bulk density. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a schematic diagram of the process flow for preparing fine, high-purity sponge ruthenium powder.
[0019] Figure 2 The image shows the XRD pattern of the dark brown powder obtained in step S3 of Example 1.
[0020] Figures 3~4 The images show SEM images of the fine, high-purity sponge ruthenium powder prepared in Example 1 at different magnifications.
[0021] Figure 5 The volume distribution particle size curve of the fine high-purity sponge ruthenium powder prepared in Example 1 is shown.
[0022] Figure 6 The image shows a SEM image of the ruthenium powder prepared in Comparative Example 1.
[0023] Figure 7 The volume distribution particle size curve of ruthenium powder prepared for Comparative Example 1.
[0024] Figure 8 The image shows a SEM image of the ruthenium powder prepared in Comparative Example 2.
[0025] Figure 9 The volume distribution particle size curve of ruthenium powder prepared for Comparative Example 2.
[0026] Figure 10The image shows a SEM image of the ruthenium powder prepared in Comparative Example 3.
[0027] Figure 11 The volume distribution particle size curve of ruthenium powder prepared for Comparative Example 3.
[0028] Figure 12 The image shows a SEM image of the ruthenium powder prepared in Comparative Example 4. Detailed Implementation
[0029] A typical embodiment of this application provides fine, high-purity sponge ruthenium powder, wherein the sponge ruthenium powder is a three-dimensional interconnected sponge-like continuous network structure, wherein the sponge-like continuous network structure is formed by several ruthenium grains being fused together with each other through neck-shaped connections, the ruthenium grains having smooth surfaces and clear grain boundaries; micron-level pores are distributed inside the continuous network; the purity of the sponge ruthenium powder is above 99.9%.
[0030] The fine, high-purity sponge ruthenium powder with the above-mentioned characteristics, with its three-dimensional interconnected sponge-like continuous network structure and the smooth surface and clear grain boundary morphology formed by the neck-like fusion between ruthenium grains, effectively avoids abnormal discharge during sputtering through its high purity of over 99.9%, ensuring the uniformity of the film. On the other hand, the porous network structure endows the powder with good dispersibility and anti-agglomeration ability, making it easy to distribute evenly during target mixing and obtain a high-density target after subsequent hot pressing and sintering. At the same time, since it directly forms a fine sponge-like morphology without mechanical crushing, it avoids the ball milling or air jet milling process introduced by grain growth in traditional hydrogenation reduction, thereby significantly reducing the introduction of impurities and free oxygen, improving the direct recovery rate of the precious metal ruthenium, and comprehensively achieving a unity of sputtering performance, processing adaptability and economy.
[0031] In some preferred embodiments, the ruthenium grains have a particle size of 0.5~3μm, such as 0.5μm, 0.8μm, 1μm, 1.2μm, 1.5μm, 1.8μm, 2μm, 2.2μm, 2.5μm, 2.8μm, 3μm, etc., preferably 0.8μm~2.2μm. Ruthenium grains within this particle size range have uniform size and moderate sintering activity, ensuring good dispersibility and anti-agglomeration ability of the sponge ruthenium powder, while also achieving sufficient densification during hot pressing sintering, avoiding abnormal grain growth, thereby obtaining a sputtering target with uniform structure and high density.
[0032] In some preferred embodiments, the width of the neck-shaped connection is 0.3~2μm, such as 0.3μm, 0.5μm, 0.8μm, 1μm, 1.2μm, 1.5μm, 1.8μm, 2μm, etc., preferably 0.5μm~1.5μm. This neck-shaped connection width ensures the intergranular welding strength, preventing powder breakage during mixing or sintering, while maintaining the loose and porous characteristics of the sponge-like network structure. This facilitates the uniform elimination of pores during subsequent hot pressing densification, avoids local closed-cell defects, and thus improves the target density and sputtering performance.
[0033] In some preferred embodiments, the lateral dimensions of the sponge ruthenium powder are 5μm to 15μm, such as 5μm, 8μm, 10μm, 12μm, 15μm, etc. This lateral size range avoids the problems of excessively fine powder agglomeration and difficulty in mixing, while also preventing excessively coarse particles from reducing sintering activity. Its moderate size facilitates uniform dispersion during target mixing and results in a highly dense target material with uniform structure and no macroscopic segregation during hot pressing sintering.
[0034] In some preferred embodiments, the purity of the sponge ruthenium powder is 99.99% or higher, preferably 99.995% or higher. Higher purity (≥99.99%) can further suppress abnormal discharge and particle splashing during sputtering, significantly improve the uniformity and density of the film, and reduce inclusion defects in the target material, thus meeting the stringent requirements of high-end semiconductors and optical coatings for ruthenium targets.
[0035] Another typical embodiment of this application provides a method for preparing fine, high-purity sponge ruthenium powder, comprising: (1) Add ruthenium trichloride solution dropwise to ammonia solution under stirring conditions, and keep the reaction at 50~80℃ to obtain reaction slurry; (2) The reaction slurry is rapidly cooled and aged in a low-temperature environment to obtain an aged slurry. The aged slurry is then subjected to solid-liquid separation to obtain a solid. The solid is then washed and dried to obtain a dark brown powder. (3) The dark brown powder was reduced under a high-temperature reducing atmosphere of plasma to obtain fine high-purity sponge ruthenium powder.
[0036] In some preferred embodiments, during step (1), the pH of the reaction system is controlled to be 7-9 during the heat preservation reaction. It should be noted that when the pH of the reaction system is insufficient to maintain 7-9, ammonia is added during the reaction to maintain this pH value.
[0037] In some preferred embodiments, step (1) is performed with ultrasonic assistance. Ultrasonic assistance is beneficial to improving the microscopic mass transfer and heat transfer effect of the system, and improving the ruthenium yield, etc. Preferably, the power of the ultrasound is 30~50kW, such as 30kW, 35kW, 40kW, 45kW, 50kW, etc.
[0038] In some preferred embodiments, in step (1), the stirring speed is 400~600 rpm, for example 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, etc.
[0039] In some preferred embodiments, in step (1), the duration of the heat preservation reaction is 3 to 5 hours, for example, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, etc.
[0040] In some preferred embodiments, the concentration of ruthenium in the ruthenium trichloride solution is 20~30 g / L.
[0041] In some preferred embodiments, the concentration of the ammonia solution is 10-25 wt%.
[0042] In some preferred embodiments, in step (2), the temperature of the low-temperature environment is 5~10℃; the low-temperature environment is an ice-water bath.
[0043] In some preferred embodiments, the aging time in step (2) is 3 to 5 hours.
[0044] In some preferred embodiments, in step (2), the washing is performed until the chloride ion content is not higher than 20 mg / kg.
[0045] In some preferred embodiments, step (3) includes: placing the dark brown powder in a plasma chamber, using argon as the working gas to carry the dark brown powder into the high-temperature zone of the plasma core, using hydrogen as the reducing gas, and heating and reducing the dark brown powder under the conditions of high-temperature reducing atmosphere of plasma. After the reduction reaction is completed, the powder is collected through a filter bag to obtain fine high-purity sponge ruthenium powder.
[0046] In some preferred embodiments, in step (3), the pressure of the working gas argon is controlled to be 0.7~0.9MPa.
[0047] In some preferred embodiments, in step (3), the pressure of the reducing gas hydrogen is controlled to be 0.3~0.6MPa.
[0048] In some preferred embodiments, in step (3), the feeding rate of the dark brown powder is controlled to be 10-20 g / min.
[0049] In some preferred embodiments, in step (3), the central gas flow rate of the argon is controlled at 100-300 L / h.
[0050] In some preferred embodiments, in step (3), plasma is generated by an induction coil, and the working power of the induction coil is 30~50kW, such as 30kW, 35kW, 40kW, 45kW, 50kW, etc.
[0051] In some preferred embodiments, in step (3), the capacitor and inductor are adjusted in real time during the restoration process to keep the standing wave ratio at 0.8~1.2, such as 0.8, 0.9, 1.0, 1.1, 1.2, etc.
[0052] Another typical embodiment of this application provides a ruthenium target material, which is prepared by using the aforementioned fine high-purity sponge ruthenium powder or the fine high-purity sponge ruthenium powder prepared by the aforementioned preparation method.
[0053] To facilitate understanding of this application, the following description will be more comprehensive and detailed in conjunction with the accompanying drawings and preferred embodiments, but the scope of protection of this application is not limited to the following specific embodiments.
[0054] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of this application.
[0055] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application are available on the market or can be prepared by existing methods.
[0056] Example 1 A method for preparing fine, high-purity sponge ruthenium powder, the process flow diagram is as follows: Figure 1 As shown, proceed with the following steps in sequence: Step S1: Add deionized water to the beaker containing solid ruthenium trichloride until all ruthenium trichloride is dissolved, and control the ruthenium content of the solution to 30 g / L; slowly add 20% ammonia solution dropwise to the prepared ruthenium trichloride solution, with excess ammonia to ensure complete ruthenium precipitation, and control the pH of the solution to 7.5. Add ammonia promptly when the pH shows a downward trend; use ultrasonic stirring during the process, with a stirring speed of 450 r / min and ultrasonic power controlled at 40 kHz to improve dispersibility, and keep the temperature at 80℃ for 5 hours.
[0057] Step S2: Place the ruthenium-containing solution obtained in step S1 into ice water at 5°C for rapid cooling and aging for 4 hours.
[0058] Step S3: Filtration and washing. The aged mother liquor obtained in step S2, after removing the supernatant, is centrifuged to separate the solid and liquid components. The centrifuge speed is controlled at 4000 r / min for 5 min. The XRD pattern of the water and dark brown powder obtained after centrifugation is shown below. Figure 2As shown (confirmed as ruthenium dioxide by color and XRD composition qualitative analysis), it was repeatedly washed with deionized water until the Cl ion content was no higher than 20 mg / kg, and finally placed in an oven to dry at 100℃ for 8 hours.
[0059] Step S4: Plasma Reduction. The ruthenium dioxide powder dried in Step S3 is placed in a plasma chamber and then carried by argon gas into the high-temperature zone of the plasma core for heating and reduction. The working gas argon pressure is controlled at 0.9 MPa, the reducing gas hydrogen pressure at 0.6 MPa, the induction coil power at 50 kW, and the capacitor and inductor are constantly adjusted to maintain a standing wave ratio of 1. The central gas flow rate is controlled at 300 L / h, and the ruthenium dioxide powder feed rate is controlled at 10 g / min. After passing through the high-temperature reducing atmosphere, fine high-purity ruthenium powder can be collected in the filter bag.
[0060] The purity of the high-purity ruthenium powder prepared in Example 1 was analyzed by GDMS, as shown in Table 1. Its microstructure and particle size were also examined. Figures 3~5 As shown.
[0061] The results of GDMS (Glow Discharge Mass Spectrometry), SEM (Scanning Electron Microscopy), and PSD (Particle Size Distribution) analysis show that the ruthenium powder purity is above 99.995%, with a yield of 97.64%. This meets the quality standards for target-grade ruthenium powder, and the removal of alkali metal cations and Cl ions is effective. The microstructure of the sponge ruthenium powder exhibits a sponge-like sheet structure, namely a three-dimensional interconnected sponge-like continuous network structure. The continuous network is formed by several ruthenium grains fused together by neck-shaped connections. The ruthenium grains have smooth surfaces and clear grain boundaries. The continuous network contains micron-sized pores. The ruthenium grains have a particle size of 0.8–2.2 μm, the neck-shaped connections have a width of 0.5–1.5 μm, and the lateral dimension of the sponge ruthenium powder is 5–15 μm, which is beneficial to the processing requirements of sputtering targets. The powder particle sizes D10 and D50 are 0.832 μm and 2.143 μm, respectively, meeting the particle size requirements of micron-sized powders. The overall particle size distribution is narrow, and the particle size uniformity is good.
[0062] Table 1. GDMS test results of high-purity ruthenium powder (unit: mg / kg) Comparative Example 1 The only difference between this comparative example and Example 1 is that step S2 is omitted.
[0063] The GDMS detection results are shown in Table 2, and the SEM detection results are shown in Table 3. Figure 6 As shown in the figure, the volume distribution particle size curve of the obtained ruthenium powder is as follows. Figure 7As shown in the figure, the GDMS and SEM results, along with the particle size distribution curve, indicate that the removal of Cl ions is poor, and the microstructure exhibits an agglomerated appearance. Analysis reveals that omitting the aging step leads to the continuous dissolution of fine crystals and abnormal growth of large crystals in the high-temperature mother liquor, resulting in severe hard agglomeration between crystals and the formation of numerous dense, blocky, and flocculent agglomerates. Under high-temperature conditions, the ruthenium dioxide precipitate undergoes continuous Oswald ripening, resulting in rapid and dense crystal accumulation. The precipitate forms a closed porous structure that strongly encapsulates chloride ions, residual ammonia complexes, and trace amounts of mother liquor impurities. These encapsulated impurities cannot be completely removed by conventional washing and drying processes and remain in the ruthenium dioxide precursor. Ultimately, the purity of the ruthenium powder can reach over 99%, with a yield of 90.64%.
[0064] Table 2. GDMS test results of ruthenium powder (unit: mg / kg) Comparative Example 2 The only difference between this comparative example and Example 1 is that, in step S2, the ruthenium-containing solution obtained in step S1 is placed in a water bath at room temperature for aging for 4 hours.
[0065] The GDMS detection results are shown in Table 3, and the SEM detection results are shown in Table 4. Figure 8 As shown in the figure, the volume distribution particle size curve of the obtained ruthenium powder is as follows. Figure 9 As shown in the figure, the detection results of GDMS and SEM indicate that the chloride ion removal effect has been improved to some extent, but not completely. The grain size is uneven, with obvious mixing of large and small particles. The precursor exhibits both slightly soft agglomerates and locally hard agglomerates. Analysis suggests that the excessively high aging temperature caused chloride ions to be trapped between grain boundaries, making them difficult to remove. Figure 9 It can be seen that the overall particle size distribution is wider, and the D50 and D90 particle sizes are significantly larger than those in Example 1, resulting in a significant decrease in powder uniformity. The final ruthenium powder purity can reach over 99.9%, with a yield of 94.86%.
[0066] Table 3. GDMS Detection Results of Ruthenium Powder (Unit: mg / kg) Comparative Example 3 The only difference between this comparative example and Example 1 is that step S4 is different. Specifically, step S4 uses conventional hydrogen reduction, which includes: transferring ruthenium dioxide powder to a crucible and placing it in a tube furnace, and reducing it with a nitrogen-hydrogen mixture at 550°C for 10 hours to obtain ruthenium powder.
[0067] The GDMS detection results are shown in Table 4, and the SEM detection results are shown in Table 5. Figure 10 As shown in the figure, the volume distribution particle size curve of the obtained ruthenium powder is as follows. Figure 11As shown in the image. The GDMS test results indicate that the final ruthenium powder purity is low, failing to meet the purity requirements for high-purity ruthenium powder. Analysis suggests this may be because the tube furnace and crucible materials easily introduce foreign metallic impurities such as Fe, Si, Al, and Co under prolonged high-temperature static atmosphere conditions, increasing the total impurity content of the powder. Simultaneously, the chlorides and ammonia produced by the decomposition of impurities within ruthenium dioxide are difficult to remove through continuous purging with a nitrogen-hydrogen mixture, resulting in significantly higher residual levels of chlorine and nitrogen impurities. Figures 10~11 It is known that ruthenium powder with large particle size differences and severe agglomeration is prone to localized abnormal grain growth during subsequent high-temperature sintering. The purity of ruthenium powder can reach over 99%, with a yield of 97.56%.
[0068] Table 4. GDMS Detection Results of Ruthenium Powder (Unit: mg / kg) Comparative Example 4 The only difference between this comparative example and Example 1 is that, in step S1, the temperature is maintained at 40°C.
[0069] The GDMS detection results are shown in Table 5, and the SEM detection results are shown in Table 6. Figure 12 As shown in the figure, the GDMS results indicate significantly low purity and yield. The direct recovery rate of ruthenium powder was 96.21%, and the purity was above 99%. Analysis revealed that the reaction temperature was too low, significantly reducing the hydrolysis precipitation kinetics and resulting in incomplete hydrolysis. A large amount of unprecipitated soluble ruthenium ammonia complex ions remained in the system, leading to significant ruthenium loss in the mother liquor. Simultaneously, a large amount of amorphous colloidal precipitate was generated. This colloid strongly adsorbed chloride ions and free ammonium ions from the solution, which were difficult to completely remove with conventional water washing, resulting in a significant increase in the residual chloride and nitrogen impurities in the precursor. Figure 12 It can be seen that the obtained ruthenium powder is a sponge-like powder.
[0070] Table 5. GDMS Detection Results of Ruthenium Powder (Unit: mg / kg) Example 2 A method for preparing fine, high-purity sponge ruthenium powder, the process flow is as follows: Figure 1 As shown, proceed with the following steps in sequence: Step S1: Add deionized water to a beaker containing solid ruthenium trichloride until all ruthenium trichloride is dissolved. Control the ruthenium content of the solution to 20 g / L. Slowly add 25% ammonia solution dropwise to the prepared ruthenium trichloride solution. Add excess ammonia to ensure complete precipitation of ruthenium. Control the pH of the solution to 8. Add ammonia promptly when the pH shows a downward trend. Use ultrasonic stirring during the process, with the ultrasonic power controlled at 40 kHz to improve dispersibility. Keep the temperature at 70°C for 4 hours.
[0071] Step S2: Place the ruthenium-containing solution obtained in step S1 into ice water at 10°C for rapid cooling and aging for 5 hours.
[0072] Step S3: Filtration and washing. After removing the supernatant, the aged mother liquor obtained in step S2 is centrifuged to separate the solid and liquid components. The centrifuge speed is controlled at 4000 r / min for 5 min. The resulting water and ruthenium dioxide are repeatedly washed with deionized water until the Cl ion content is no higher than 20 mg / kg. Finally, the mixture is placed in an oven and dried at 100℃ for 8 h.
[0073] Step S4: Plasma Reduction. The ruthenium dioxide powder dried in Step S3 is placed in a plasma chamber and then carried by argon gas into the high-temperature zone of the plasma core for heating and reduction. The working gas argon pressure is controlled at 0.8 MPa, the reducing gas hydrogen pressure at 0.5 MPa, the induction coil power at 45 kW, and the capacitor and inductor are constantly adjusted to maintain a standing wave ratio of 1. The central gas flow rate is controlled at 100 L / h, and the ruthenium dioxide powder feed rate is controlled at 20 g / min. After passing through the high-temperature reducing atmosphere, fine high-purity ruthenium powder can be collected in the filter bag. The purity of the ruthenium powder can reach over 99.995%, and the yield is 97.37%.
[0074] Example 3 A method for preparing fine, high-purity sponge ruthenium powder comprises the following steps: Step S1: Add deionized water to a beaker containing solid ruthenium trichloride until all ruthenium trichloride is dissolved, and control the ruthenium content of the solution to 30 g / L; slowly add 15% (w / w) ammonia solution dropwise to the prepared ruthenium trichloride solution, with excess ammonia to ensure complete ruthenium precipitation, and control the pH of the solution to 7. If the pH shows a downward trend, add ammonia promptly; use ultrasonic stirring during the process, with the ultrasonic power controlled at 40 kHz to improve dispersibility, and keep the temperature at 50°C for 5 hours.
[0075] Step S2: Place the ruthenium-containing solution obtained in step S1 into ice water at 8°C for rapid cooling and aging for 4 hours.
[0076] Step S3: Filtration and washing. After removing the supernatant, the aged mother liquor obtained in step S2 is centrifuged to separate the solid and liquid components. The centrifuge speed is controlled at 4000 r / min for 4 min. The resulting water and ruthenium dioxide are repeatedly washed with deionized water until the Cl ion content is no higher than 20 mg / kg. Finally, the mixture is placed in an oven and dried at 100℃ for 8 h.
[0077] Step S4: Plasma Reduction. The ruthenium dioxide powder dried in Step S3 is placed in a plasma chamber and then carried by argon gas into the high-temperature zone of the plasma core for heating and reduction. The working gas argon pressure is controlled at 0.8 MPa, the reducing gas hydrogen pressure at 0.6 MPa, the induction coil power at 30 kW, and the capacitor and inductor are constantly adjusted to maintain a standing wave ratio of 1. The central gas flow rate is controlled at 200 L / h, and the ruthenium dioxide powder feed rate is controlled at 15 g / min. After passing through the high-temperature reducing atmosphere, fine high-purity ruthenium powder can be collected in the filter bag. The purity of the ruthenium powder can reach over 99.9%, and the yield is 96.85%.
[0078] The above description is only a preferred embodiment of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of this application, and these improvements and modifications should also be considered within the scope of protection of this application.
Claims
1. Fine, high-purity sponge ruthenium powder, characterized in that, The sponge ruthenium powder has a three-dimensional interconnected sponge-like continuous network structure. The sponge-like continuous network structure is formed by several ruthenium grains being fused together by neck-shaped connections. The ruthenium grains have smooth surfaces and clear grain boundaries. Micron-sized pores are distributed inside the continuous network. The purity of the sponge ruthenium powder is above 99.9%.
2. The fine, high-purity sponge ruthenium powder as described in claim 1, characterized in that, The fine, high-purity sponge ruthenium powder satisfies at least one of the following characteristics: (a) The ruthenium grains have a grain size of 0.5 μm to 3 μm; (b) The width of the neck-shaped connection is 0.3 μm to 2 μm; (c) The lateral dimensions of the sponge ruthenium powder are 5μm to 15μm; (d) The purity of the sponge ruthenium powder is 99.99% or higher, preferably 99.995% or higher.
3. A method for preparing fine, high-purity sponge ruthenium powder, characterized in that, include: (1) Add ruthenium trichloride solution dropwise to ammonia solution under stirring conditions, and keep the reaction at 50~80℃ to obtain reaction slurry; (2) The reaction slurry is rapidly cooled and aged in a low-temperature environment to obtain an aged slurry. The aged slurry is then subjected to solid-liquid separation to obtain a solid. The solid is then washed and dried to obtain a dark brown powder. (3) The dark brown powder was reduced under a high-temperature reducing atmosphere of plasma to obtain fine high-purity sponge ruthenium powder.
4. The method for preparing fine, high-purity sponge ruthenium powder as described in claim 3, characterized in that, In step (1), during the heat preservation reaction, the pH value of the reaction system is controlled to be 7~9; And / or, in step (1), the stirring speed is 400~600 rpm; And / or, step (1) is performed with ultrasound assistance; the power of the ultrasound is 30~50kW; And / or, in step (1), the duration of the heat preservation reaction is 3~5h.
5. The method for preparing fine, high-purity sponge ruthenium powder as described in claim 3, characterized in that, The concentration of ruthenium in the ruthenium trichloride solution is 20~30 g / L; And / or, the concentration of the ammonia solution is 10~25wt%.
6. The method for preparing fine, high-purity sponge ruthenium powder as described in claim 3, characterized in that, In step (2), the temperature of the low-temperature environment is 5~10℃; the low-temperature environment is an ice-water solution.
7. The method for preparing fine, high-purity sponge ruthenium powder as described in claim 3, characterized in that, In step (2), the aging time is 3-5 hours; In step (2), the washing continues until the chloride ion content is no higher than 20 mg / kg.
8. The method for preparing fine, high-purity sponge ruthenium powder as described in claim 3, characterized in that, Step (3) includes: placing the dark brown powder in a plasma chamber, using argon as the working gas to carry the dark brown powder into the high-temperature zone of the plasma core, using hydrogen as the reducing gas, and heating and reducing the dark brown powder under the high-temperature reducing atmosphere of the plasma. After the reduction reaction is completed, fine high-purity sponge ruthenium powder is collected.
9. The method for preparing fine, high-purity sponge ruthenium powder as described in claim 3 or 8, characterized in that, In step (3), the pressure of the working gas argon is controlled to be 0.7~0.9MPa; And / or, in step (3), the pressure of the reducing gas hydrogen is controlled to be 0.3~0.6MPa; And / or, in step (3), the feed rate of the dark brown powder is controlled to be 10-20 g / min; And / or, in step (3), the central gas flow rate of argon is controlled at 100-300 L / h; And / or, in step (3), plasma is generated by an induction coil, the operating power of which is 30~50kW; And / or, in step (3), the capacitor and inductor are adjusted in real time during the restoration process to keep the standing wave ratio at 0.8~1.
2.
10. A ruthenium target, characterized in that, The fine high-purity sponge ruthenium powder is prepared by the method described in claim 1 or 2, or by any one of claims 3 to 9.