A bismuth / copper core-shell nanoparticle and a method for preparing the same
By combining ultrasonic liquid phase exfoliation and solvothermal methods to prepare bismuth nanoparticles, and then forming bismuth/copper core-shell nanoparticles through in-situ liquid phase reduction, the problems of uneven preparation and low yield of bismuth nanoparticles in existing technologies have been solved, and efficient and low-cost industrial production has been achieved.
Patent Information
- Application Number
- CN202611265226.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are difficult to efficiently prepare bismuth nanoparticles and bismuth/copper core-shell nanoparticles with uniform particle size and high yield, and the preparation methods are complex and costly, making them unsuitable for industrialization.
Bismuth nanoparticles were prepared by combining ultrasonic liquid phase exfoliation and solvothermal methods through synergistic effects. Then, bismuth/copper core-shell nanoparticles were formed by in-situ liquid phase reduction. The morphology and size of the particles were controlled by combining water bath ultrasound and high-temperature reaction, and morphology control agents were used to prevent agglomeration.
This method achieves high yield, size uniformity, and monodispersity of bismuth/copper core-shell nanoparticles, simplifies the preparation process, reduces costs, and is suitable for low-cost industrial production.
Smart Images

Figure CN123149407A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of two-dimensional materials, and in particular relates to a bismuth / copper core-shell nanoparticle and its preparation method. Background Technology
[0002] Two-dimensional materials are those in which electrons can move freely (planarly) only in two dimensions at a non-nanoscale (1-100 nm) scale, such as nanofilms. In 2004, two scientists at the University of Manchester, Andrei Geim and Kestya Novoselov, first synthesized graphene using a tape method. Since then, a series of quasi-two-dimensional materials with only a single atomic layer thickness, such as black phosphorus (phosphene), silicene, germanene, antimonene, boron nitride, and molybdenum disulfide, have been discovered.
[0003] Bismuthene is a two-dimensional material derived from bulk metallic bismuth, possessing a structure similar to graphene. However, bismuthene is a direct bandgap semiconductor with a bandgap of 0.99 eV (the bottom of the conduction band and the top of the valence band are at the same position), allowing for direct coupling with light and exhibiting a wide absorption spectrum. Furthermore, due to bismuth's strong biocompatibility and low biotoxicity, bismuthene has broad application potential in optics, electronics, and biomedicine. Bismuth nanoparticles, on the other hand, are a potential biomedical substrate material for drug delivery, photothermal therapy, and photodynamic therapy.
[0004] Currently, bismuth nanoparticles are prepared using techniques such as mechanical exfoliation (e.g., transparent tape tearing) and chemical vapor deposition. However, mechanical exfoliation yields low-yield bismuth nanoparticles with inconsistent morphology and particle size, making it unsuitable for commercial production; it is also cumbersome and time-consuming. Chemical vapor deposition produces relatively small quantities of bismuth nanoparticles, and reproducibility is difficult. Ultrasonic liquid phase exfoliation yields relatively large quantities, but the product morphology and particle size uniformity are poor. Although gradient centrifugation can yield more uniform bismuth nanoparticles, it significantly reduces the overall yield. While solvothermal high-temperature treatment of bismuth powder can produce more uniform bismuth nanoparticles, the yield remains low.
[0005] Core-shell nanoparticles possess physicochemical properties distinct from those of the core and shell, and these properties can be controlled by altering or adjusting the chemical composition, size, or morphology of the core and shell, thereby expanding the range of applications for these particles. Currently, the main methods for preparing core-shell nanoparticles include ion implantation, ion exchange, deposition, and sol / gel methods, all of which suffer from drawbacks such as complex operation procedures, long reaction times, and high costs. Summary of the Invention
[0006] In view of this, the present invention provides bismuth / copper core-shell nanoparticles and their preparation method. This method combines ultrasonic liquid-phase exfoliation and solvothermal methods, achieving synergistic exfoliation and morphological reshaping of bismuth powder to obtain bismuth nanoparticles with good monodispersity and uniform size. Then, bismuth / copper core-shell nanoparticles are obtained through in-situ liquid-phase reduction. This method is simple to operate, has a short preparation cycle, good reproducibility, and high yield or efficiency of bismuth / copper core-shell nanoparticles, making it easy to achieve low-cost industrial production.
[0007] This invention provides a method for preparing bismuth / copper core-shell nanoparticles, comprising the following steps: (1) Disperse bismuth powder in an organic solvent to obtain a dispersion; wherein the concentration of bismuth powder in the dispersion is 0.5-10 mg / mL; (2) First, the dispersion is subjected to water bath ultrasound with a power of 400-600W for 24-96 hours; then the ultrasound liquid is transferred to a hydrothermal reactor for high-temperature reaction to obtain a high-temperature treatment liquid; wherein the temperature of the high-temperature reaction is 160-200℃ and the time is 12-24 hours. (3) Allow the high-temperature treatment liquid to cool naturally to room temperature, and then centrifuge it at 33000-35000xg for the first time to collect the precipitate; (4) The precipitate was washed with anhydrous ethanol and then redispersed in anhydrous ethanol. (5) Add lithium tetrachlorocopper oxide and polyvinylpyrrolidone (PVP), followed by reduction with sodium borohydride; (6) The above mixed dispersion was centrifuged for the second time at 33000-35000xg, and the precipitate was collected. The precipitate obtained is bismuth / copper core-shell nanoparticles.
[0008] Optionally, the organic solvent includes, but is not limited to, one or more of N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetone, tetrahydrofuran, anhydrous ethanol, methanol, isopropanol, chloroform, and dichloromethane. The surface energy of the organic solvent used matches the surface energy of the bismuthene material, and there is a certain interaction between the two to balance the energy required to strip the bismuth powder.
[0009] Optionally, the morphology control agent includes one or more of polyvinylpyrrolidone (PVP), hexadecyltrimethylammonium chloride (CTAC), sodium dodecyl sulfate (SDS), sodium dodecylbenzenesulfonate (SDBS), polyether P123, and polyether F127, but is not limited thereto. The morphology control agent used can rapidly, stably, and efficiently bind to the surface of bismuth nanoparticles, preventing particle aggregation and precipitation during the preparation process.
[0010] Optionally, the particle size of the bismuth powder does not exceed 12.7 mm. More preferably, the particle size of the bismuth powder is 1-12.7 mm. In other embodiments of the present invention, the bismuth powder may also be ground to a particle size of less than 100 μm before use.
[0011] In this embodiment of the invention, the power of the water bath ultrasound can be 400W, 450W, 500W, 550W, 580W, or 600W. Optionally, the power of the first water bath ultrasound is 400-600W.
[0012] Optionally, the water bath ultrasound is performed under ice bath conditions with a temperature not exceeding 10°C. Preferably, the temperature during the water bath ultrasound is 0-10°C, and more preferably 4-10°C. The ice bath conditions refer to placing the container containing the solution to be ultrasoundd in another container (such as a beaker or test tube) containing ice during the water bath ultrasound process.
[0013] Optionally, the first water bath ultrasound is performed at a temperature of 5-10℃.
[0014] The temperature of the high-temperature reaction can be 160℃, 170℃, 180℃, 190℃, and 200℃. Optionally, the temperature of the high-temperature reaction is 160-200℃.
[0015] In this embodiment of the invention, the high-temperature reaction time can be 12h, 15h, 20h or 24h.
[0016] Optionally, the centrifugation time of the high-speed centrifuge is 15-30 min. For example, 12, 15, 20, 25 or 30 min.
[0017] Optionally, the rotation speed of the high-speed centrifuge is 33,000-35,000 x g.
[0018] The precipitate obtained after high-speed centrifugation (i.e., bismuth nanoparticles or bismuth / copper core-shell nanoparticles) can be redispersed in a second solvent to obtain a solution containing bismuth nanoparticles or bismuth / copper core-shell nanoparticles. Optionally, the second solvent includes one or more of N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetone, tetrahydrofuran, anhydrous ethanol, methanol, and isopropanol.
[0019] Preparation mechanism explanation: In this invention, the water bath ultrasonic treatment of the bismuth powder dispersion initially breaks down the bismuth powder through the ultrasonic cavitation effect, causing it to partially dissolve in the organic solvent, resulting in an organic solvent dispersion containing a large number of bismuth nanosheets. The subsequent high-temperature treatment allows the bismuth atoms in the dispersion to gain sufficient energy, reshaping their morphology with the help of the solvent, forming bismuth nanoparticles with relatively uniform morphology and particle size. During the high-temperature reaction, NMP molecules adsorbed on the particle surface ensure that the particles do not agglomerate, facilitating subsequent centrifugal purification.
[0020] In the subsequent in-situ liquid-phase reduction process, bismuth nanoparticles are redispersed in ethanol. The nitrogen atoms in the NMP molecules coating the particle surface have lone pairs of electrons, which can coordinate with and bind hydrogen ions dissociated from trace amounts of water molecules in the solvent, giving the particle surface a positive charge. The negatively charged tetrachlorocuprate ions formed by lithium tetrachlorocuprate dissolved in ethanol can be adsorbed onto the surface of the bismuth nanoparticles via electrostatic interactions. Upon the addition of sodium borohydride, the tetrachlorocuprate ions are reduced in situ to elemental copper, thereby forming bismuth / copper core-shell nanoparticles. PVP can be adsorbed and bound to the particle surface during the reduction process, ensuring that the particles do not aggregate, facilitating subsequent centrifugal purification.
[0021] The method for preparing bismuth / copper core-shell nanoparticles provided in the first aspect of this invention involves first preparing bismuth nanoparticles using a combination of liquid-phase exfoliation and solvothermal methods, and then preparing bismuth / copper core-shell nanoparticles using an in-situ liquid-phase reduction method. This method is simple to operate, has a high yield, and has significant advantages over current mechanical exfoliation and chemical vapor deposition methods. It can obtain bismuth / copper core-shell nanoparticles with controllable size and good monodispersity, and is easy to achieve low-cost industrial production. This lays the foundation for the application of bismuth nanosheets in the biomedical field.
[0022] Second aspect: Products This invention also provides bismuth / copper core-shell nanoparticles prepared by the above-described method. The thickness of the bismuth / copper core-shell nanoparticles is less than 20 nm, and the lateral dimensions of the bismuth nanosheets are 60 nm to 120 nm. The lateral dimensions refer to the length, width, or diameter of the bismuth / copper core-shell nanoparticles.
[0023] Optionally, the lateral dimensions of the bismuth / copper core-shell nanoparticles are 60 nm to 120 nm. For example, they are 60 nm, 75 nm, 80 nm, 95 nm, 100 nm, 115 nm, or 120 nm.
[0024] The bismuth / copper core-shell nanoparticles consist of a bismuth core encapsulated in a copper shell.
[0025] Optionally, the thickness of the bismuth / copper core-shell nanoparticles is 0.3-20 nm.
[0026] Optionally, the bismuth / copper core-shell nanoparticles have a thickness of 1-64 atomic layers. That is, their core is composed of 1-64 layers of stacked monolayer bismuthene. More optionally, the thickness of the bismuth / copper core-shell nanoparticles is 3.1-19.84 nm.
[0027] Optionally, the bismuth / copper core-shell nanoparticles may have shapes including, but not limited to, square, circular, triangular, polygonal, etc.
[0028] Optionally, the monodispersity index (PDI) of the bismuth / copper core-shell nanoparticles is 0.097-0.143, for example 0.097, 0.105, 0.110, 0.115, 0.120, 0.125, 0.130, 0.135, 0.140 or 0.143.
[0029] The bismuth / copper core-shell nanoparticles provided by this invention have relatively regular shapes, uniform sizes, good dispersibility, and low toxicity, making them suitable for fields such as optics, electronics, and biomedicine (e.g., preparation of photothermal therapy drugs and optically labeled drugs). Attached Figure Description
[0030] Figure 1 This is a high-resolution transmission electron microscope (HRTEM) image of bismuth / copper core-shell nanoparticles prepared according to an embodiment of the present invention.
[0031] Figure 2 This is an elemental mapping diagram of the bismuth / copper core-shell nanoparticles prepared according to an embodiment of the present invention.
[0032] Figure 3 The results of atomic force microscopy (AFM) analysis of bismuth / copper core-shell nanoparticles prepared in the embodiments of the present invention are shown.
[0033] Figure 4 The images show the UV-Vis-NIR absorption spectra of the bismuth nanoparticle precursor and the bismuth / copper core-shell nanoparticle final product prepared in anhydrous ethanol solvent according to embodiments of the present invention. Detailed Implementation
[0034] The preferred embodiments of the present invention will be further described in detail below with reference to the accompanying drawings: The following embodiments are provided to better understand the present invention, but are not intended to limit the invention. Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods. Example 1
[0035] A method for preparing bismuth / copper core-shell nanoparticles includes the following steps: (1) Take a 250mL Shu Niu glass bottle, put in 200mL of NMP solvent, add 200mg of 200 mesh (200 particles / square inch, that is, a particle size of 0.074mm) bismuth powder, and obtain a dispersion with an initial concentration of 1mg / mL (or 1000ppm) of bismuth powder. (2) Place the glass bottle in (1) into the Xinzhi Ultrasonic Constant Temperature Cleaner SBL-22DT and use it at a constant temperature of 10℃ with 70% of the maximum power (600W) (i.e., 420W power) for 48 hours in a water bath. (3) After ultrasonication in a water bath, take 140 mL of the obtained supernatant and place it in a 200 mL reaction vessel produced by Shanghai Yushen Instrument Co., Ltd., and use a Shanghai Boxun GZX-9076MBE constant temperature drying oven (1200W maximum power) to react at 160℃ for 12 hours. The supernatant is the high temperature reaction liquid. (4) Divide the high-temperature reaction solution into 6 equal portions, transfer them into 50mL centrifuge tubes, and centrifuge them for 20 minutes at 18000rpm (34050xg centrifugal force) using a Hunan Hexi HR20MW floor-standing refrigerated centrifuge. The precipitate in the tube is bismuth nanoparticle. Wash the precipitate twice with anhydrous ethanol, redisperse it in anhydrous ethanol and store it. (5) Take 50 mg of the obtained bismuth nanoparticles and dilute them in 68.5 mL of anhydrous ethanol. Stir magnetically at 200 rpm for 1 min at room temperature. Then add 1.6 mL of lithium tetrachlorocopper ethanol solution with a concentration of 100 mmol / L and stir for 1 min. Increase the stirring speed to 1000 rpm and add 9.9 mL of PVP ethanol solution with a concentration of 2 mol / L. Stir for 1 min and quickly add 20 mL of sodium borohydride ethanol dispersion with a concentration of 2.5 mg / mL. Stir for 2 min. Then, evenly transfer the obtained dispersion into four 50 mL centrifuge tubes and centrifuge at 34050 x g for 20 min. Collect the precipitate in the tubes, which is the desired bismuth / copper core-shell nanoparticles. Wash them twice with anhydrous ethanol, bottle and seal them, and store them at room temperature away from light.
[0036] Calculations show that in Example 1 of this invention, the yield of the bismuth / copper core-shell nanoparticles is 65mg / 140mL = 46.4%, and the monodispersity index (PDI) measured by dynamic light scattering (DLS) is 0.097. Example 2
[0037] A method for preparing bismuth / copper core-shell nanoparticles includes the following steps: (1) Take a 500mL Shu Niu glass bottle, put in 450mL of NMP solvent, add 900mg of 200 mesh (200 particles / square inch, that is, a particle size of 0.074mm) bismuth powder, and obtain a dispersion with an initial bismuth powder concentration of 2mg / mL. (2) Place the glass bottle in (1) into the Xinzhi Ultrasonic Constant Temperature Cleaner SBL-22DT and use it at a constant temperature of 10℃ with 80% of the maximum power (600W) (i.e., 480W) for 96 hours of ultrasonic water bath. (3) After ultrasonication in a water bath, take 400 mL of the obtained supernatant and place it in a 500 mL reaction vessel produced by Shanghai Yushen Instrument Co., Ltd., and use a Shanghai Boxun GZX-9076MBE constant temperature drying oven (1200W maximum power) to react at 180℃ for 24 hours. The supernatant is the high temperature reaction liquid. (4) Divide the high-temperature reaction solution into 16 equal portions, transfer them into 50mL centrifuge tubes, and centrifuge them for 30 minutes at 18000rpm (34050xg centrifugal force) using a Hunan Hexi HR20MW floor-standing refrigerated centrifuge. The precipitate in the tube is bismuth nanoparticle. Wash the precipitate twice with anhydrous ethanol, redisperse it in anhydrous ethanol and store it. (5) Take 200 mg of the obtained bismuth nanoparticles and dilute them in 274 mL of anhydrous ethanol. Stir magnetically at 200 rpm for 1 min at room temperature. Then add 6.4 mL of lithium tetrachlorocopper ethanol solution with a concentration of 100 mmol / L and stir for 1 min. Increase the stirring speed to 1000 rpm and add 39.6 mL of PVP ethanol solution with a concentration of 2 mol / L. Stir for 1 min and quickly add 80 mL of sodium borohydride ethanol dispersion with a concentration of 2.5 mg / mL. Stir for 2 min. Then, evenly distribute the obtained dispersion into 16 50 mL centrifuge tubes and centrifuge at 34050 x g for 30 min. Collect the precipitate in the tubes, which is the desired bismuth / copper core-shell nanoparticles. Wash them twice with anhydrous ethanol, bottle and seal them, and store them at room temperature away from light.
[0038] Calculations show that in Example 2 of the present invention, the yield of the bismuth / copper core-shell nanoparticles is 282.3 mg / 400 mL = 70.5%, and the monodispersity index (PDI) measured by dynamic light scattering (DLS) is 0.126.
[0039] Figure 1 This is a high-resolution transmission electron microscope (HRTEM) image of bismuth / copper core-shell nanoparticles prepared according to an embodiment of the present invention. Figure 1 As can be seen in the image, there are multiple rough-edged regular hexagonal or circular particles, which are bismuth / copper core-shell nanoparticles. Under magnification, obvious lattice fringes are visible.
[0040] Figure 2This is an elemental mapping diagram of the bismuth / copper core-shell nanoparticles prepared according to an embodiment of the present invention. As can be seen from the diagram, bismuth, copper, carbon, and oxygen are uniformly distributed on the particles. Furthermore, in the merged diagram, bismuth and copper are obscured by carbon and oxygen, thus proving that the obtained product is indeed bismuth / copper core-shell nanoparticles. The carbon and oxygen on their surface originate from solvents and morphology control agents left on the surface during the preparation process, or from unavoidable contamination during the preparation process.
[0041] Figure 3 The image shows the atomic force microscopy (AFM) analysis results of the bismuth / copper core-shell nanoparticles prepared according to an embodiment of the present invention. The image reveals the presence of numerous sheet-like structures less than 2 nm thick, indicating that the bismuth core in the obtained bismuth / copper core-shell nanoparticles is composed of approximately 10 stacked monolayers of bismuthene, meaning the thickness of the bismuth / copper core-shell nanoparticles is approximately equivalent to 10 bismuth atomic layers.
[0042] Figure 4 The images show the UV-Vis-NIR absorption spectra of the bismuth nanoparticle precursor and the bismuth / copper core-shell nanoparticle final product prepared in anhydrous ethanol solvent according to embodiments of the present invention. As can be seen from the figures, the bismuth / copper core-shell nanoparticles provided by the present invention exhibit stronger absorption characteristics than bismuth nanoparticles in the 300-800 nm region, making them more suitable for UV-Vis applications.
[0043] Comparative Example To highlight the beneficial effects of the present invention, the present invention also provides the following comparative embodiments for Embodiment 1: Comparative Example 1: The difference from Example 1 is that in step (2), only water bath ultrasound is performed and no high-temperature reaction is performed.
[0044] Comparative Example 2: The difference from Example 1 is that in step (2), only the high-temperature reaction is carried out and the water bath ultrasound is not performed.
[0045] Compared with the bismuth / copper core-shell nanoparticles of Example 1, the product prepared in Comparative Example 1 has a particle size of over 200 nm and an irregular morphology.
[0046] Compared with Example 1, the product prepared in Comparative Example 2 had a yield of 5.8 mg / 140 mL = 4.14% of the bismuth / copper core-shell nanoparticles.
[0047] The above comparative results demonstrate that the synergistic effect of water bath ultrasound and high-temperature reaction is key to obtaining high-yield, uniformly sized products. When ultrasound is used alone without high-temperature reaction, the particle size is large and the morphology is irregular; when high-temperature reaction is used alone without ultrasound, the yield is extremely low. This invention achieves a simultaneous improvement in yield and uniformity through the synergistic combination of the two.
[0048] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention.
Claims
1. A method for preparing bismuth / copper core-shell nanoparticles, characterized in that, Includes the following steps: (1) Disperse bismuth powder in an organic solvent to obtain a dispersion; wherein the concentration of bismuth powder in the dispersion is 0.5-10 mg / mL; (2) First, the dispersion is subjected to a first water bath ultrasonic treatment, and then the ultrasonic liquid is transferred to a hydrothermal reactor for high-temperature reaction to obtain a high-temperature treatment liquid; (3) Allow the high-temperature treatment liquid to cool naturally to room temperature, then centrifuge at high speed for the first time and collect the precipitate; (4) The precipitate obtained from the first high-speed centrifugation was washed twice with anhydrous ethanol and redispersed in anhydrous ethanol to obtain a dispersion. (5) The anhydrous ethanol dispersion was magnetically stirred at room temperature, and then lithium tetrachlorocopper oxide ethanol solution was added, and stirring was continued. (6) The mixed dispersion is rapidly stirred magnetically at room temperature, then an ethanol solution of polyvinylpyrrolidone is added and stirred continuously, then a sodium borohydride ethanol dispersion is rapidly added and stirred continuously. (7) The above mixed dispersion was centrifuged at high speed for the second time, and the precipitate was collected. The precipitate obtained was bismuth / copper core-shell nanoparticles.
2. The preparation method according to claim 1, characterized in that, The particle size of the bismuth powder does not exceed 12.7 mm.
3. The preparation method according to claim 1, characterized in that, The organic solvent includes one or more of N-methylpyrrolidone, dimethylformamide, dimethyl sulfoxide, acetone, tetrahydrofuran, anhydrous ethanol, methanol, isopropanol, chloroform, and dichloromethane.
4. The preparation method according to claim 1, characterized in that, In step (1), the power of the water bath ultrasound is 400-600W, the time is 24-96 hours, and it is carried out at a temperature of 5-10℃.
5. The preparation method according to claim 1, characterized in that, In step (2), the high-temperature reaction temperature is 160-200℃ and the time is 12-24 hours.
6. The preparation method according to claim 1, characterized in that, In step (3), the speed of high-speed centrifugation is 33000-35000 x g.
7. Bismuth / copper core-shell nanoparticles, characterized in that, The thickness of the bismuth / copper core-shell nanoparticles is less than 20 nm, the lateral size of the bismuth / copper core-shell nanoparticles is 60 nm-120 nm, and the monodispersity index (PDI) of the bismuth / copper core-shell nanoparticles is 0.097-0.
143.
8. The bismuth / copper core-shell nanoparticles as described in claim 7, characterized in that, The bismuth / copper core-shell nanoparticles consist of a bismuth core encapsulated in a copper shell.
9. The bismuth / copper core-shell nanoparticles as described in claim 7, characterized in that, The bismuth / copper core-shell nanoparticles have a thickness of 0.3-20 nm and are composed of bismuthene stacked with a thickness of 1-64 atomic layers.
10. The bismuth / copper core-shell nanoparticles as described in claim 7, characterized in that, The bismuth / copper core-shell nanoparticles can be square, circular, triangular, or polygonal in shape.