Laser welding method of glass and metal and brazing filler metal
By using a brazing filler metal composed of sodium heptahydrate, α-terpineol, and glass powder, combined with laser welding and a grid-like groove structure, the problems of low efficiency, high energy consumption, and poor bonding strength in glass-to-metal connections are solved, achieving a high-efficiency and environmentally friendly welding effect, suitable for connecting temperature-sensitive components.
Patent Information
- Application Number
- CN202611497305.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies for joining glass and metal suffer from problems such as low welding efficiency, high energy consumption, poor joint strength, insufficient weather resistance, failure to meet environmental protection requirements, and high equipment costs.
A brazing filler metal composed of sodium heptahydrate, α-terpineol, and glass powder is coated onto the surface of a metal substrate and laminated with a glass substrate using a laser welding method. Multiple welding passes are performed using laser scanning, and a grid-like groove structure is combined to enhance the bonding force and release stress.
It achieves efficient and environmentally friendly glass-to-metal welding, with high weld strength, excellent acid and alkali resistance and weather resistance, suitable for connecting temperature-sensitive components, meeting environmental protection requirements, and reducing energy consumption and equipment costs.
Smart Images

Figure CN123149506A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser welding technology, and more particularly to a laser welding method for glass and metal and a brazing filler metal. Background Technology
[0002] Glass is widely used due to its stability, transparency, and corrosion resistance. In some applications, it is necessary to connect glass and metal. Existing methods for connecting glass and metal mainly include the following: 1. Adhesive Bonding: Currently, the bonding of glass and metal largely relies on organic adhesives such as epoxy. Organic adhesives have poor high-temperature resistance, with long-term operating temperatures generally not exceeding 200℃. Under high and low temperature cycling environments, they are prone to aging, becoming brittle, cracking, and detaching, resulting in poor long-term joint reliability. The adhesive layer has limited resistance to acids, alkalis, and salt spray, exhibiting poor weather resistance in outdoor or harsh conditions, and is prone to yellowing and failure. During curing and service, organic adhesives release volatile small molecules, contaminating optical and electronic devices. The adhesive layer cannot achieve high airtightness, allowing moisture and gas to slowly penetrate along the layer, leading to seal failure. Furthermore, the adhesive layer is relatively thick and highly visible, affecting the appearance quality of light-transmitting devices. 2. Direct laser connection: Glass has a low absorption rate for commonly used near-infrared lasers, and the physical and chemical properties of glass and metals are very different. When lasers are directly connected, the interface is prone to cracking and has many pores, resulting in low joint strength and poor sealing. Smooth metal surfaces have poor wettability, making it difficult to obtain a reliable connection. 3. In-furnace overall heating brazing: When using glass brazing filler metal to connect glass and metal, the traditional process requires placing the workpiece coated with brazing filler metal into a heating furnace, heating it to above 400℃ and holding it at that temperature for a long time (the entire cycle usually takes more than 2 hours), which is energy-intensive and inefficient; the overall heating heat-affected zone is large, and temperature-sensitive components (electronic devices, polymer parts, magnetic materials, etc.) inside the component may be damaged or even fail due to overall heating, which limits its application range; in multi-step packaging processes, subsequent heating steps may also cause previously connected parts to soften and detach. Furthermore, traditional leaded glass brazing alloys do not meet environmental regulations such as RoHS and are being phased out. The mismatch in thermal expansion coefficients between traditional brazing alloys and glass or metal leads to significant residual stress during cooling, making the joint prone to cracking along the interface. High porosity within the brazed layer results in low joint strength and poor sealing. When using active brazing alloys such as Ag-Cu-Ti to braze glass and metal, the brazing temperature is high (typically above 780℃), requiring a vacuum or high-purity protective atmosphere, resulting in high equipment and process costs and low efficiency.
[0003] Furthermore, on the one hand, there are differences in understanding among those skilled in the art; on the other hand, the inventors studied a large number of documents and patents when making this invention, but due to space limitations, not all details and contents were listed in detail. However, this does not mean that the present invention does not possess the features of these prior art. On the contrary, the present invention already possesses all the features of the prior art, and the applicant reserves the right to add relevant prior art to the background art. Summary of the Invention
[0004] In view of the shortcomings of the existing technology, one object of the present invention is to provide a laser welding method for glass and metal, which has high welding efficiency, low energy consumption and reliable welding.
[0005] Another objective of this invention is to provide a brazing filler metal that is environmentally friendly and can effectively improve the bonding strength between glass and metal in glass-to-metal welding applications, as well as enhance the acid and alkali resistance and weather resistance of the weld layer.
[0006] The embodiments of the present invention are achieved through the following technical solutions: A laser welding method for glass and metal includes the following steps: Coating Step: Apply solder to the surface of the metal substrate to be soldered to form a solder coating. The solder is composed of sodium heptahydrate, α-terpineol, and glass powder, with the mass percentages of sodium heptahydrate, α-terpineol, and glass powder being 10%~20%, 30%~50%, and 40%~60%, respectively. Overlay step: Cover the side of the metal substrate coated with solder with the glass substrate, and clamp and position the glass substrate and the metal substrate; Welding steps: Welding operation is performed by shining a welding laser from one side of the glass substrate.
[0007] According to a preferred embodiment, before the coating step, a surface treatment step is further included. The surface treatment step includes: opening a groove on the surface of the metal substrate to be welded for accommodating the brazing filler metal. The groove includes a plurality of first grooves arranged in parallel with each other and a plurality of second grooves arranged in parallel with each other, wherein the first grooves intersect with the second grooves.
[0008] According to a preferred embodiment, after the coating step, a drying step is further included, which includes: using hot air to blow and dry the solder coating, so that α-terpineol evaporates and the solder coating is cured and shaped.
[0009] According to a preferred embodiment, the hot air temperature is controlled at 40°C to 60°C.
[0010] According to a preferred embodiment, in the welding step, the wavelength of the welding laser is 800nm-980nm, the core diameter of the laser fiber is 100μm-400μm, the power of the welding laser is 80W-300W, and the scanning speed is 50mm / s-80mm / s.
[0011] According to a preferred embodiment, the welding step employs multi-pass scanning welding, with 3 to 10 scan passes.
[0012] According to a preferred embodiment, in the welding step, the power of the welding laser in the first 1-2 passes is lower than the power of the welding laser in subsequent passes.
[0013] According to a preferred embodiment, the welding laser scanning trajectory follows the contour of the area to be welded, and the scanning paths of adjacent passes are the same.
[0014] A brazing filler metal, wherein the brazing filler metal is composed of sodium heptahydrate, α-terpineol and glass powder, wherein the mass percentages of sodium heptahydrate, α-terpineol and glass powder are 10%~20%, 30%~50% and 40%~60% respectively.
[0015] According to a preferred embodiment, the mass percentages of sodium heptahydrate, α-terpineol, and glass powder are 15%~20%, 35%~45%, and 40%~50%, respectively.
[0016] The technical solutions of the embodiments of the present invention have at least the following advantages and beneficial effects: This invention enables reliable welding of glass and metal, resulting in a high-strength weld joint. The brazing filler metal is lead-free, meeting environmental protection requirements. Laser welding is more energy-efficient and effective than furnace-heated brazing, and it uses localized heating, resulting in a small overall temperature rise between the glass and metal. It can be used for connecting components containing temperature-sensitive elements and is also suitable for multi-step packaging processes. Attached Figure Description
[0017] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 A flowchart illustrating a laser welding method for glass and metal provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the assembly structure of the metal substrate, the solder coating, and the glass substrate provided in an embodiment of the present invention. Figure 3 A top view of the surface of a metal substrate to be welded, provided in an embodiment of the present invention; Figure 4 This is a schematic diagram of the welded 304 stainless steel and quartz glass in Embodiment 1 of the present invention. Figure 5 This is a schematic diagram of the TC4 titanium alloy and sapphire glass after welding in Embodiment 2 of the present invention.
[0019] Icons: 1-Metal substrate, 11-First groove, 12-Second groove, 2-Banger filler coating, 3-Glass substrate, 4-Welding laser. Detailed Implementation
[0020] To better understand and implement this invention, the technical solutions in the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0022] A laser welding method for glass and metal includes the following steps: Step S1, Surface Treatment Step: The surface of the metal substrate 1 to be welded is cleaned, decontaminated, and dried. Then, grooves for accommodating solder are formed on the surface of the metal substrate 1 to be welded. The grooves include a plurality of first grooves 11 and a plurality of second grooves 12 arranged in parallel with each other, and the first grooves 11 and the second grooves 12 intersect each other. Preferably, the first grooves 11 and the second grooves 12 intersect perpendicularly, forming a grid-like groove structure on the surface of the metal substrate 1 to be welded.
[0023] Step S2, Coating Step: Apply solder to the surface of the metal substrate 1 to be soldered to form a solder coating 2. The solder is composed of sodium heptahydrate (Na2Si3O7), α-terpineol, and glass powder, with the mass percentages of sodium heptahydrate, α-terpineol, and glass powder being 10%~20%, 30%~50%, and 40%~60%, respectively. Figure 2As shown, in this step, the brazing filler metal coated on the metal substrate 1 fills the first groove 11 and the second groove 12, and extends upwards to a certain thickness. The grid-like groove structure can increase the contact area between the brazing filler metal and the metal substrate 1; after the molten brazing filler metal solidifies in the grid-like groove structure, it forms a mechanical interlock (anchoring effect), which can significantly improve the interfacial bonding force between the glass substrate 3 and the metal substrate 1; at the same time, the grid-like groove structure can divide the continuous interface into grid units, which can release the residual stress during the cooling process of the weld layer and inhibit the propagation of interfacial cracks, thereby simultaneously improving the connection strength and crack resistance of the joint.
[0024] Step S3, Drying Step: Hot air is used to blow and dry the solder coating 2, causing α-terpineol to evaporate and the solder coating 2 to solidify and set. In this step, the hot air temperature is controlled at 40℃~60℃ to allow α-terpineol to evaporate slowly, avoiding rapid heating that could cause violent solvent evaporation and form bubbles in the solder coating 2.
[0025] Step S4, Overlapping step: Cover the side of the metal substrate 1 coated with solder with the glass substrate 3, and clamp and position the glass substrate 3 and the metal substrate 1.
[0026] Step S5, Welding Step: Welding operation is performed by incident welding laser 4 from one side of the glass substrate 3. In this step, a 915nm wavelength laser is used to output welding laser 4. The welding laser 4 passes through the glass substrate 3 and is absorbed by the brazing filler metal coating 2. The brazing filler metal coating 2 is heated and melts, simultaneously wetting the surfaces of both the glass substrate 3 and the metal substrate 1 to be welded. The fiber core diameter of the laser is 100μm~400μm, the power of the welding laser 4 is 80W~300W, and the scanning speed is 50mm / s~80mm / s. In this step, multi-pass scanning welding is used, with 3~10 scans. This ensures that the brazing filler metal is fully melted. In this step, the power of the welding laser 4 in the first 1~2 passes is lower than that in subsequent passes. This setting allows the lower power welding laser 4 in the first 1~2 passes to pre-sinter and degas the brazing filler metal coating 2, allowing residual organic components in the brazing filler metal slurry to be fully discharged and tiny bubbles to overflow one pass at a time. Subsequent passes then use the high power welding laser 4 to complete the full melting and welding of the brazing filler metal coating 2. Multiple thermal cycles can also slow down the heating and cooling rate of the brazing filler coating 2, i.e. the welding layer, release thermal stress, and prevent the brazing filler coating 2 and glass substrate 3 from cracking due to rapid cooling and heating, ultimately obtaining a dense welding layer without pores.
[0027] It should be noted that during the welding process, the welding laser 4 scans along the contour of the area to be welded, and the scanning paths of adjacent passes are the same. This ensures a uniform and dense weld layer.
[0028] Step S6, Cooling Step: After welding, allow for natural cooling. The brazing filler metal coating 2 solidifies, achieving the welding of the glass substrate 3 and the metal substrate 1.
[0029] Through the above steps, reliable welding of glass and metal can be achieved, resulting in a high-strength weld joint. The brazing filler metal is lead-free, meeting environmental protection requirements. Laser welding is more energy-efficient and effective than furnace-heated brazing, and it is a localized heating method, resulting in a small overall temperature rise between the glass and metal. It can be used for connecting components containing temperature-sensitive elements and is also suitable for multi-step packaging processes.
[0030] Next, we will explain how to perform welding operations using specific materials and following the steps outlined above. Example 1
[0031] Metal substrate 1 is 304 stainless steel, and glass substrate 3 is quartz glass (SiO2 glass). Sodium heptahydrate, α-terpineol, and FD56 glass powder were weighed out in weight percentages of 20%, 40%, and 40% respectively, and stirred evenly to obtain a brazing filler slurry. A first groove 11 and a second groove 12 were formed on the 304 stainless steel surface to be welded using laser etching. The depth of the first groove 11 and the second groove 12 was approximately 30 μm. The spacing between two adjacent first grooves 11 was set to 50 μm, and the spacing between two adjacent second grooves 12 was also 50 μm. The brazing filler slurry was coated onto the groove surface and flattened to form a brazing filler coating 2. The brazing filler coating 2 was dried with hot air at 50°C. A quartz glass cover was then installed and clamped for positioning. A 915nm laser with a fiber core diameter of 400 μm was used, with a scanning speed of 80 mm / s and a concentric scanning trajectory. Four passes were used for welding. The laser power for the first two passes was 80 W, and the laser power for the last two passes was 200 W. Welding was completed after cooling. The joint was tested and found to have a connection strength of 36 MPa. The joint has good oxidation / reduction resistance and has passed the tests for acid and alkali resistance, salt spray resistance and high weather resistance, and can achieve airtight sealing. Example 2
[0032] The metal substrate 1 is TC4 titanium alloy, and the glass substrate 3 is sapphire glass. Sodium heptahydrate, α-terpineol, and FD56 glass powder are weighed out in percentages of 20%, 40%, and 40% respectively, and stirred evenly to obtain a solder slurry. A first trench 11 and a second trench 12 are formed on the TC4 surface to be soldered using laser etching. The depth of the first trench 11 and the second trench 12 is approximately 55 μm. The spacing between two adjacent first trenches 11 is set to 130 μm, and the spacing between two adjacent second trenches 12 is also 130 μm. The solder slurry is coated onto the trench surface and flattened to form a solder coating 2, which is then dried with hot air at 50°C. The sapphire glass is then covered and clamped for positioning. A 915nm laser with a fiber core diameter of 400 μm is used, with a scanning speed of 80 mm / s and a concentric scanning trajectory. Six passes are used for soldering. The first two passes use a laser power of 80W, and the last four passes use a laser power of 200W. After cooling, the connection is complete. The joint was tested and found to have a connection strength of 18.9 MPa. The joint has good oxidation / reduction resistance and has passed the tests for acid and alkali resistance, salt spray resistance and high weather resistance, and can achieve airtight sealing.
[0033] The present invention also provides a brazing filler metal for the aforementioned laser welding operation between glass and metal. Specifically, the brazing filler metal is composed of sodium heptahydrate, α-terpineol, and glass powder, wherein the mass percentages of sodium heptahydrate, α-terpineol, and glass powder are 10%~20%, 30%~50%, and 40%~60%, respectively.
[0034] In this embodiment, preferably, the glass powder is grade FD56, a lead-free low-melting-point glass powder, whose main components are: bismuth oxide (Bi2O3) as the main network forging / modifying agent, supplemented by boron oxide (B2O3), zinc oxide (ZnO), silicon dioxide (SiO2), and containing small amounts of lithium oxide (Li2O) and sodium oxide (Na2O). Bismuth oxide can significantly reduce the softening temperature of the glass and adjust the thermal expansion coefficient of the solder to between that of glass and metal, alleviating the interfacial thermal expansion mismatch stress; boron oxide can reduce the melting point of the solder and improve its chemical stability; zinc oxide can improve the chemical durability of the solder and help adjust the thermal expansion coefficient; silicon dioxide, as a network forging agent, improves the strength and stability of the solder layer; lithium oxide and sodium oxide act as fluxing agents, further reducing the soldering temperature between the glass substrate 3 and the metal substrate 1; the bismuth-based component system has a higher absorption rate of 915nm wavelength laser than the transparent glass substrate, which can selectively concentrate the laser energy on the solder layer to achieve local heating.
[0035] Sodium heptahydrate, as an inorganic binder, on the one hand, ensures that the glass powder is uniformly suspended in the brazing filler slurry and prevents sedimentation and stratification; on the other hand, it participates in the formation of the Si-O network structure during laser heating, enhancing the chemical bond between the brazing filler coating 2, i.e. the welding layer, and the glass substrate 3, and improving the acid and alkali resistance and weather resistance of the welding layer.
[0036] α-Terpineol: As an organic solvent carrier, it imparts suitable viscosity, leveling and thixotropy to the slurry, making it easy to coat and fill grooves; its high boiling point allows it to be slowly evaporated and removed under low-temperature drying conditions of 40~60℃, avoiding violent evaporation that could form bubbles and pores in the brazing filler coating 2.
[0037] Furthermore, in the brazing filler metal, the mass percentages of sodium heptahydrate, α-terpineol, and glass powder are 15%~20%, 35%~45%, and 40%~50%, respectively. This results in higher welding strength between the glass substrate 3 and the metal substrate 1.
[0038] The following are experiments on laser welding of quartz glass and 304 stainless steel using brazing filler metals with different component ratios: 1. The solder contains 10% sodium heptahydrate, 30% α-terpineol, and 60% glass powder by mass. When this solder is applied to the welded quartz glass and 304 stainless steel, the joint strength measured is 15.7 MPa.
[0039] 2. The solder contains 10% sodium heptahydrate, 40% α-terpineol, and 50% glass powder by mass. When applied to a joint between quartz glass and 304 stainless steel, the brazing filler metal in this ratio achieves a joint strength of 20.1 MPa.
[0040] 3. The solder contains 20% sodium heptahydrate, 30% α-terpineol, and 50% glass powder by mass. When this solder was applied to the weld between quartz glass and 304 stainless steel, the joint strength measured was 25.4 MPa.
[0041] 4. The solder contains 20% sodium heptahydrate, 40% α-terpineol, and 40% glass powder by mass. When this solder is applied to the welded joint between quartz glass and 304 stainless steel, the joint strength measured is 36 MPa.
[0042] 5. The solder contains 20% sodium heptahydrate, 50% α-terpineol, and 30% glass powder by mass. When this solder is applied to the welded joint between quartz glass and 304 stainless steel, the joint strength measured is 5.2 MPa.
[0043] 6. The solder contains 30% sodium heptahydrate, 40% α-terpineol, and 30% glass powder by mass. When this solder was applied to the weld between quartz glass and 304 stainless steel, the joint strength measured was 10.4 MPa.
[0044] 7. The solder contains 30% sodium heptahydrate, 50% α-terpineol, and 20% glass powder by mass. When this solder is used to weld quartz glass to 304 stainless steel, insufficient glass powder prevents the formation of a continuous weld layer.
[0045] 8. The solder contains 40% sodium heptahydrate, 40% α-terpineol, and 20% glass powder. When this solder is used to weld quartz glass to 304 stainless steel, insufficient glass powder and excessive binder prevent the formation of a continuous weld layer.
[0046] The above experiments show that when the mass percentage of sodium heptahydrate tris(II)-siliconium is 20%, the mass percentage of α-terpineol is 40%, and the mass percentage of glass powder is 40%, this brazing filler metal can enable quartz glass and 304 stainless steel to achieve good welding strength.
[0047] The technical means disclosed in this invention are not limited to those disclosed in the above embodiments, but also include technical solutions composed of any combination of the above technical features. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this invention, and these improvements and modifications are also considered within the scope of protection of this invention.
Claims
1. A method of laser welding glass to metal, characterized by, Includes the following steps, Coating Step: Apply solder to the surface of the metal substrate to be soldered to form a solder coating. The solder is composed of sodium heptahydrate, α-terpineol, and glass powder, with the mass percentages of sodium heptahydrate, α-terpineol, and glass powder being 10%~20%, 30%~50%, and 40%~60%, respectively. Overlay step: Cover the side of the metal substrate coated with solder with the glass substrate, and clamp and position the glass substrate and the metal substrate; Welding steps: Welding operation is performed by shining a welding laser from one side of the glass substrate.
2. The method of laser welding glass to metal according to claim 1, wherein, Prior to the coating step, a surface treatment step is also included, which includes: A groove is formed on the surface of the metal substrate to be welded to accommodate the brazing filler metal. The groove includes a plurality of first grooves arranged in parallel with each other and a plurality of second grooves arranged in parallel with each other, wherein the first grooves intersect with the second grooves.
3. The method of laser welding glass to metal of claim 1, wherein, Following the coating step, a drying step is also included, which includes: The solder coating is dried by blowing hot air to evaporate α-terpineol and solidify the solder coating.
4. The method of laser welding glass to metal according to claim 3, wherein, The hot air temperature is controlled between 40℃ and 60℃.
5. The method of laser welding glass to metal of claim 1, wherein, In the welding step, the wavelength of the welding laser is 800nm-980nm, the core diameter of the laser fiber is 100μm-400μm, the power of the welding laser is 80W-300W, and the scanning speed is 50mm / s-80mm / s.
6. The method of laser welding glass to metal of claim 1, wherein, In the welding process, multi-pass scanning welding is used, with 3 to 10 scan passes.
7. The method of laser welding glass to metal according to claim 6, wherein, In the welding process, the power of the welding laser in the first 1-2 passes is lower than the power of the welding laser in subsequent passes.
8. The method of laser welding glass to metal of claim 6, wherein, The welding laser scanning trajectory follows the contour of the area to be welded, and the scanning paths of adjacent passes are the same.
9. A brazing material, characterized by The brazing filler metal is composed of sodium heptahydrate, α-terpineol and glass powder, with the mass percentages of sodium heptahydrate, α-terpineol and glass powder being 10%~20%, 30%~50% and 40%~60% respectively.
10. The brazing material according to claim 9, characterized in that, The mass percentages of sodium heptahydrate, α-terpineol, and glass powder are 15%~20%, 35%~45%, and 40%~50%, respectively.