A liquid cooling plate vacuum brazing method for preventing flow channel blockage

By filling the flow channels of the copper-aluminum composite liquid cooling plate with a thermally decomposable solder resist medium and employing a segmented temperature-controlled brazing process, the flow channel blockage problem was solved, the product qualification rate was improved, and the production cost was reduced. This method is suitable for heat dissipation systems of high heat flux density GPU chips.

CN123149507APending Publication Date: 2026-11-24JIANGSU HUIHE DIGITAL ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611471999.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the existing vacuum brazing process for copper-aluminum composite liquid cooling plates, molten Al-Si brazing filler metal easily penetrates into the micro-gap flow channels of the spade teeth and the interior of the copper tube, causing flow channel blockage, affecting the weld airtightness and heat dissipation performance, resulting in low first-pass yield and high cost.

Method used

The flow channel is filled with a thermally decomposable solder resist medium suspension. A segmented temperature-controlled brazing process is used to prevent the solder from seeping into the flow channel, ensuring the strength and airtightness of the copper-aluminum dissimilar weld and avoiding flow channel blockage.

Benefits of technology

It has increased the first-pass yield of liquid cooling plates to over 90%, reduced production scrap and losses, ensured heat dissipation performance and smooth flow channels, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149507A_ABST
    Figure CN123149507A_ABST
Patent Text Reader

Abstract

This invention discloses a processing method for preventing flow channel blockage during vacuum brazing of liquid-cooled plates, belonging to the field of heat dissipation component manufacturing technology for high-power electronic devices. The method includes the following steps: workpiece preparation, filling with solder resist medium, assembling and applying brazing filler metal, vacuum brazing, and post-weld treatment: pre-treating copper components and aluminum alloy shells; filling the copper flow channel components and copper tubes with PMMA micro powder-deionized water solder resist suspension, and drying to form a solid adhesion layer; assembling the workpieces and applying Al-Si based brazing filler metal; using segmented temperature control in a vacuum environment, first completely vaporizing and expelling the solder resist medium at 280-380℃, and then raising the temperature to 580℃ to complete the copper-aluminum dissimilar vacuum brazing; finally purging the flow channels and conducting continuity and airtightness tests.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of heat dissipation component manufacturing technology for high-power electronic devices, and particularly relates to a processing method for preventing flow channel blockage by vacuum brazing of liquid cooling plates, specifically applicable to the production and preparation of copper-aluminum composite liquid cooling plates used in high heat flux density GPU chips such as NVIDIA RTX 5090. Background Technology

[0002] As the computing power of GPU chips continues to increase, the heat flux density of components such as chips, memory, and inductors continues to rise. Copper-aluminum composite liquid coolers, with their combination of lightweight aluminum alloy casing and high thermal conductivity copper channels, are widely used in the cooling systems of high heat flux density GPUs. These liquid coolers are generally made of 6061-T6 aluminum alloy casing and T2 copper channel structure components connected by vacuum brazing. They also feature both toothed copper channels and copper tube channels inside. The toothed copper channels have a tooth thickness of 0.25mm and a tooth spacing of only 0.25mm. The copper tubes are CNC bent, and the coolant circulates between the toothed channels and inside the copper tubes to remove the heat from the devices.

[0003] Vacuum brazing of dissimilar copper and aluminum materials commonly uses Al-Si brazing filler metals. During the welding process, the molten filler metal flows under capillary action. Current manufacturing processes involve inserting the toothed copper flow channel component and copper tube into an aluminum alloy shell, then directly placing Al-Si brazing filler metal foil or paste on the mating surface, and finally heating it in a vacuum brazing furnace to 580-600℃ to complete the welding. To prevent molten brazing filler metal from seeping into the flow channel and causing blockage, the industry currently mainly adopts the following methods: The first is to reduce the amount of brazing filler metal used, relying on workers' experience to control the amount of brazing filler metal applied. However, copper-aluminum dissimilar welding requires sufficient brazing filler metal to fill the weld seam to ensure airtightness. Insufficient brazing filler metal can easily lead to incomplete welds, incomplete weld seams, and product leakage failure. The second is physical sealing, using ceramic plugs, graphite rods, or high-temperature resistant cotton to fill the flow channel or copper tube opening. However, the gap between the teeth of the shovel-tooth flow channel is narrow, and the plug cannot be inserted into the gap between the teeth and is easy to damage the thin teeth. After the copper tube is bent, the path is bent, and the plug cannot reach the deep inside the copper tube. The third is to weld directly without protection. Once blockage occurs after welding, high-pressure water guns or acid washing are used to clear the blockage. The 0.25mm thin teeth are easily bent and deformed under high pressure, and the brazing filler metal that has seeped into the inner wall of the copper tube is almost impossible to clean, and the whole product must be scrapped.

[0004] Constrained by the aforementioned issues, the first-pass yield of existing copper-aluminum composite liquid cooling plates in vacuum brazing is only 60%-70%. The T2 copper and 6061-T6 aluminum alloy blanks used in GPU liquid cooling plates are expensive, and the costs of tooth removal and CNC precision machining are also high. Product scrapping results in significant economic losses. Therefore, there is an urgent need to develop a processing technology that can balance weld airtightness with effectively preventing the precision flow channels from being blocked by the brazing filler metal. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of existing vacuum brazing processes for copper-aluminum composite liquid cooling plates and to provide a processing method for preventing flow channel blockage during vacuum brazing of liquid cooling plates. This method solves the problem of flow channel blockage caused by molten Al-Si brazing filler metal penetrating into the micro-gap flow channels of the spade teeth and the interior of the copper tube in existing processes. While ensuring the welding strength and airtightness of the dissimilar copper-aluminum weld, it improves the first-pass yield of products, reduces production scrap losses, and is suitable for mass production of GPU liquid cooling plates with composite flow channels.

[0006] A method for preventing flow channel blockage during vacuum brazing of a liquid cooling plate includes the following steps: S1. Workpiece preparation: Prepare copper components including copper flow channel parts with spade teeth and copper tubes, as well as aluminum alloy shells. Perform degreasing, pickling to remove oxide film, pure water cleaning, and drying pretreatment on all workpieces. S2, Solder resist medium filling: The gap between the teeth of the copper flow channel component and the inner flow channel of the copper tube are filled with a thermally decomposable and vaporizable solder resist medium suspension. After drying, a solid adhesion layer is formed on the inner wall of the flow channel. The solder resist medium is a suspension prepared by PMMA micro powder and deionized water, and its thermal decomposition temperature is lower than the melting temperature of Al-Si brazing filler metal. S3. Assemble the brazing filler metal: Assemble the copper components into the aluminum alloy shell and apply Al-Si brazing filler metal to the weld joint surface between the copper components and the aluminum alloy shell. S4. Vacuum Brazing: The workpiece is placed in a vacuum environment and a segmented temperature-controlled brazing process is adopted. First, the temperature is raised to the decomposition temperature range of the welding resist medium and held to allow the welding resist medium to fully decompose, vaporize and be discharged. Then, the temperature is raised to the melting temperature of Al-Si brazing filler metal to complete the copper-aluminum dissimilar vacuum brazing. After that, it is cooled and taken out of the furnace. S5. Post-weld treatment: Purge the flow channel to remove trace residues, and perform flow channel continuity and airtightness tests.

[0007] Furthermore, in step S2, a differentiated filling method is adopted for different flow channels: vacuum impregnation filling is used for the shovel-tooth copper flow channel component, and pressure injection filling is used for the copper tube.

[0008] Furthermore, the segmented temperature-controlled brazing process described in step S4 includes: a preheating and heat preservation stage, a solder resist medium decomposition and heat preservation stage, a brazing heating stage, a brazing heat preservation stage, a temperature homogenization stage, and a cooling stage; wherein the solder resist medium decomposition and heat preservation temperature is 280-380℃, and the brazing heat preservation temperature is 580℃.

[0009] Furthermore, the solid content of the solder resist medium suspension is 30%-50%, and the mass ratio of PMMA micro powder to deionized water is (3-5):(7-5).

[0010] Furthermore, during the preheating stage, the temperature is raised to 200℃ and held for 15-20 minutes during the decomposition stage of the solder resist medium; after brazing, the temperature is raised to 600℃ for homogenization treatment.

[0011] Furthermore, the thickness of the toothed copper flow channel component is 0.25mm and the tooth spacing is 0.25mm; the aluminum alloy shell material is 6061-T6, and the copper component material is T2 copper.

[0012] The present invention also provides the application of the processing method for preventing flow channel blockage by vacuum brazing of the liquid cooling plate described in any of the preceding claims in the preparation of GPU liquid cooling plates. The GPU liquid cooling plate is a copper-aluminum composite liquid cooling plate, which integrates a spade-tooth micro-gap flow channel and a copper tube flow channel for heat dissipation of high heat flux density GPU chips.

[0013] This invention provides a processing method for preventing flow channel blockage during vacuum brazing of liquid cooling plates, which has the following beneficial effects: (1) Thoroughly prevent blockage of composite flow channels and ensure heat dissipation performance: The solder resist medium is completely decomposed and vaporized before 380℃ and discharged by the vacuum system, forming a clean cavity in the flow channel. When the temperature rises to 580℃, the Al-Si solder melts, but at this time there is no capillary penetration path on the inner wall of the flow channel. The solder only flows in the weld gap between the copper part and the aluminum shell 2, and will not enter the 0.25mm tooth gap and the interior of the φ6-10mm copper tube. After welding, the tooth spacing of the toothed flow channel remains unchanged, the inner diameter of the copper tube does not shrink, and the coolant flow rate and flow resistance fully meet the design specifications (pressure drop 4.5-5.5KPa).

[0014] (2) Allowing normal filler metal usage to ensure the quality of copper-aluminum dissimilar welding: Copper-aluminum dissimilar material welding requires sufficient filler metal to ensure a full weld and airtightness. Existing technologies often reduce filler metal due to concerns about clogging, resulting in incomplete welds. This invention isolates the flow channel through a welding barrier medium, allowing the use of sufficient Al-Si-based filler metal at the weld, ensuring both weld strength and airtightness (no leakage after holding at 0.6MPa for 5 minutes) while completely avoiding flow channel blockage.

[0015] (3) Improve product yield and reduce production costs: After adopting this method, the first-pass yield of vacuum brazing can be increased from 60%-70% to over 90%. It avoids the scrapping of the entire part due to flow channel blockage. Especially for high-cost copper T2 toothed flow channel parts, precision CNC machining costs and aluminum alloy 6061-T6 shells, a single part can save hundreds of yuan in rework / scrap losses.

[0016] (4) It does not damage the precision flow channel structure and is suitable for mass production: The solder resist medium is a flexible liquid filler, which does not exert mechanical pressure on the thin toothed plate (0.25mm thick) of the spade and will not cause deformation of the toothed plate; the liquid form can fill any position of the curved copper tube. After welding, there is no need to manually remove the plugs one by one as in the physical plugging method. Only high-pressure gas purging is required. The process is simple and suitable for automated mass production. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the method flow of the present invention. Detailed Implementation

[0018] The embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and should not be construed as limiting the scope of the invention.

[0019] In the description of this invention, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," "outer," "front end," "rear end," "head," "tail," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0020] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "connected" and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0021] Example 1 A method for vacuum brazing liquid-cooled plates to prevent flow channel blockage, such as... Figure 1 As shown, the copper-aluminum composite liquid cooler plate used to fabricate a device compatible with the RTX 5090 GPU includes the following steps: S1. Workpiece Preparation: Prepare a 6061-T6 aluminum alloy shell and T2 copper components; the copper components include serrated copper flow channels and bent copper tubes with specifications of φ8×1mm and φ12×1mm; the serrated copper flow channel has a tooth thickness of 0.25mm, a tooth spacing of 0.25mm, and a tooth height of 3-8mm; the aluminum alloy shell is pre-machined with a deep cavity flow channel and a copper tube mounting groove, with a fitting clearance of 0.05-0.1mm between the copper tube and the mounting groove. All workpieces are degreased, pickled to remove the surface oxide film, rinsed with pure water, and then dried for later use.

[0022] S2. Solder resist filling: Prepare a solder resist suspension by mixing PMMA micro powder and deionized water at a mass ratio of 4:6, with a solid content of 40%. The decomposition temperature range of this medium is 280-380℃, lower than the melting temperature of 4047 solder at 577℃. The decomposition products are methyl methacrylate monomer, a small amount of carbon dioxide and water vapor, with no corrosive residue. Immerse the copper channel component with spade teeth in the suspension using vacuum impregnation at a vacuum degree of -0.09MPa for 8 minutes to allow the suspension to fully penetrate the 0.25mm gap between the teeth. Remove and drain. Press the copper tube into the copper tube mounting groove of the shell, and inject the suspension from the copper tube end at a pressure of 0.2MPa, filling the inner cavity of the copper tube and the tiny gap between the outer wall of the copper tube and the groove. Place the filled workpiece in an oven and dry at 100℃ for 45 minutes. After the moisture evaporates, the PMMA micro powder forms a continuous solid adhesion layer on the inner wall of all channels.

[0023] S3. Assemble the brazing filler metal: Assemble and position the copper flow channel component and copper tube into the aluminum alloy shell; lay 4047 brazing filler metal foil at the contact weld between the copper component and the aluminum alloy shell, and place the brazing filler metal only on the weld joint surface, avoiding the flow channel opening.

[0024] S4. Vacuum Brazing: The assembled workpiece is placed into a vacuum brazing furnace, and a vacuum of ≤10°C is drawn. -2 Pa; Segmented temperature control: Preheating and holding stage: heating rate 4℃ / min, from room temperature to 200℃, holding for 30min, removing residual moisture from the workpiece and solder resist medium; Solder resist medium decomposition and holding stage: heating rate 4℃ / min, from 200℃ to 380℃, holding for 18min, PMMA solid layer fully decomposes and vaporizes, gas is pumped out of the furnace by the vacuum system along the flow channel; Brazing heating stage: heating rate 4℃ / min, from 380℃ to 580℃; Brazing holding stage: holding at 580℃ for 10min, 4047 brazing filler melts, capillary action fills the weld gap between copper and aluminum; Isostatic stage: heating to 600℃, isostatic holding for 5min, ensuring uniform weld temperature across the entire batch of workpieces; Cooling stage: cooling with the furnace to below 200℃, removing the workpiece for air cooling.

[0025] S5. Post-weld treatment: Use 0.5MPa high-pressure dry nitrogen to purge the flow channel from the inlet and outlet of the copper tube to remove trace residues; After assembly, conduct testing: Air tightness test: no leakage after holding pressure at 0.6MPa for 5 minutes; Water flow test: flow rate 1.2L / min, actual measured pressure drop in the flow channel 4.9KPa, meeting the qualified standard of ≤5.5KPa, the flow channel is unblocked, and the finished GPU liquid cooling plate is obtained.

[0026] Example 2 This embodiment is largely the same as the process in Embodiment 1, except for the solder resist medium ratio: PMMA micro powder: deionized water mass ratio 3:7, suspension solid content 30%; vacuum impregnation vacuum degree -0.08MPa, held for 10 min; drying temperature 80℃, drying for 60 min; solder resist medium decomposition stage 380℃ holding for 15 min; pressure injection pressure 0.1MPa. The finished product has qualified airtightness, flow channel pressure drop 5.1KPa, and no flow channel blockage.

[0027] Example 3 This embodiment is largely the same as Embodiment 1 in terms of process, except for the solder resist medium ratio: PMMA micro powder: deionized water mass ratio 5:5, suspension solid content 50%; vacuum impregnation vacuum degree -0.09MPa, held for 5 min; drying temperature 120℃, drying for 30 min; solder resist medium decomposition stage 380℃ holding for 20 min; pressure injection pressure 0.3MPa. The finished product has qualified airtightness, flow channel pressure drop 4.7KPa, and no flow channel blockage.

[0028] Comparative Example Using traditional processes, the workpiece pretreatment and brazing filler metal assembly are the same as in Example 1, without filling with solder resist medium or applying flow channel protection; direct vacuum brazing is performed. Post-weld sampling inspection showed a first-pass yield of 66%. Some samples exhibited issues such as gaps between the toothed plates, brazing filler metal blockage inside the copper tube, and excessive flow channel pressure drop, resulting in the direct scrapping of some workpieces.

[0029] As can be seen from the comparison of Examples 1-3 and the comparative examples, the process of the present invention can effectively avoid the blockage of brazing filler metal in the micro-gap flow channel of the spade teeth and the flow channel of the copper tube while ensuring the airtightness of the welding, thus significantly improving the product yield.

[0030] The device embodiments described above are merely illustrative. The units described as separate components may or may not be physically separate. The components shown as units may or may not be physical units; that is, they may be located in one place or distributed across multiple network units. Some or all of the modules can be selected to achieve the purpose of this embodiment according to actual needs. Those skilled in the art can understand and implement this without any creative effort.

[0031] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for processing a liquid cooling plate vacuum brazing anti-flow channel blockage, characterized in that, Includes the following steps: S1. Workpiece preparation: Prepare copper components including copper flow channel parts with spade teeth and copper tubes, as well as aluminum alloy shells. Perform degreasing, pickling, cleaning, and drying pretreatment on all workpieces. S2, Solder resist medium filling: The gap between the teeth of the shovel-tooth copper flow channel component and the internal flow channel of the copper tube are filled with a thermally decomposable and vaporizable solder resist medium suspension. After drying, a solid adhesion layer is formed on the inner wall of the flow channel. The solder resist medium is a suspension prepared by PMMA micro powder and deionized water, and its thermal decomposition temperature is lower than the melting temperature of Al-Si brazing filler metal. S3. Assemble the brazing filler metal: Assemble the copper components into the aluminum alloy shell and apply Al-Si brazing filler metal to the weld joint surface between the copper components and the aluminum alloy shell. S4. Vacuum Brazing: The workpiece is placed in a vacuum environment and a segmented temperature-controlled brazing process is adopted. First, the temperature is raised to the decomposition temperature range of the welding resistance medium and held to allow the welding resistance medium to fully decompose, vaporize and be discharged. Then, the temperature is raised to the melting temperature of Al-Si brazing filler metal to complete the copper-aluminum dissimilar vacuum brazing. After that, it is cooled and taken out of the furnace. S5. Post-weld treatment: Purge the flow channel to remove trace residues, and perform flow channel continuity and airtightness tests.

2. The processing method for preventing flow channel blockage of vacuum brazing of a liquid cold plate according to claim 1, characterized in that, In step S2, a differentiated filling method is adopted for different flow channels: vacuum impregnation filling is used for the shovel-tooth copper flow channel component, and pressure injection filling is used for the copper tube.

3. The method of claim 1, wherein the liquid cold plate is vacuum brazed. The segmented temperature-controlled brazing process described in step S4 includes: a preheating and heat preservation stage, a solder resist medium decomposition and heat preservation stage, a brazing heating stage, a brazing heat preservation stage, a temperature homogenization stage, and a cooling stage; wherein the solder resist medium decomposition and heat preservation temperature is 280-380℃, and the brazing heat preservation temperature is 580℃.

4. The method of claim 1, wherein the liquid cold plate is vacuum brazed. The solid content of the solder resist medium suspension is 30%-50%, and the mass ratio of PMMA micro powder to deionized water is (3-5):(7-5).

5. The method of claim 3, wherein the liquid cold plate is vacuum brazed. During the preheating stage, the temperature is raised to 200℃ and held. During the decomposition stage of the solder resist medium, the temperature is raised to 380℃ and held for 15-20 minutes. After brazing, the temperature is raised to 600℃ for homogenization treatment.

6. The method of processing according to any one of claims 1-5, wherein, The thickness of the copper shovel teeth is 0.25mm and the tooth spacing is 0.25mm; the aluminum alloy shell is made of 6061-T6 and the copper components are made of T2 copper.

7. Use of the process for vacuum brazing of liquid cold plate without flow channel clogging according to any one of claims 1 to 6 for the production of GPU liquid cold plates, characterized in that, The GPU liquid cooling plate is a copper-aluminum composite liquid cooling plate, which integrates a spade-tooth micro-gap flow channel and a copper tube flow channel for heat dissipation of high heat flux density GPU chips.