A method for high-precision 3D printing of Ti-6Al-4V high-strength and high-toughness thin-walled hexahedron by using six laser symmetrical coaxial heat sources

By combining a six-beam symmetrical coaxial heat source with central filament feeding, the problem of uneven heat input in traditional laser filament feeding 3D printing of thin-walled hexahedrons is solved, achieving high-precision and stable thin-walled hexahedron forming, and improving the overall forming accuracy and material utilization.

CN123149558APending Publication Date: 2026-11-24SHANDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611433298.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

When using traditional laser filament feeding to 3D print thin-walled hexahedrons, the directional heat input causes changes in the size and flow state of the molten pool, affecting the forming accuracy. In particular, in the closed contour area, there is local repeated heating and heat accumulation, which leads to local collapse, contour distortion and overall decrease in accuracy.

Method used

A six-beam laser symmetrical coaxial heat source is used, which is symmetrically arranged around the central wire feeding axis to form a circumferentially balanced heat input. Combined with central wire feeding and molten pool monitoring, the molten pool state is stabilized, and heat accumulation and forming errors are reduced.

Benefits of technology

It improves the overall forming accuracy and printing stability of thin-walled hexahedrons, reduces local collapse and contour distortion, and realizes high-precision 3D printing of high-strength and tough Ti-6Al-4V thin-walled hexahedrons.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149558A_ABST
    Figure CN123149558A_ABST
Patent Text Reader

Abstract

When printing thin-walled hexahedrons layer by layer, significant heat accumulation occurs at the starting and ending points, and the stability of the molten pool at corners is poor. Continuous deposition commonly suffers from problems such as local collapse and interlayer forming deviations. This invention arranges six laser beams symmetrically around a central filament feed axis. The Ti-6Al-4V filament is stably fed axially to the molten pool region formed by the six lasers, and continuous multi-layer deposition is carried out according to the contour of the thin-walled hexahedron. This method utilizes the symmetrical heat input of the six lasers to reduce the influence of the thermal state in various directions and closed regions on the molten pool, ensuring controllable filament feeding and molten pool state, and achieving stable forming of each edge, corner, and interlayer of the hexahedron. The Ti-6Al-4V thin-walled hexahedron component prepared by this method is complete without collapse, has high surface forming accuracy, high strength, and good toughness. This invention is beneficial for continuous use of filaments and fine 3D printing, and is suitable for the high-precision manufacturing of complex thin-walled Ti-6Al-4V components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal 3D printing technology, specifically relating to a method for high-precision 3D printing of Ti-6Al-4V high-strength and tough thin-walled hexahedrons using a six-laser symmetrical coaxial heat source. Background Technology

[0002] Ti-6Al-4V (TC4) titanium alloys possess high specific strength, good corrosion resistance, and high service reliability, making them widely used in aerospace and high-end equipment manufacturing. However, for complex components with thin walls, closed profiles, and multi-directional sidewalls, traditional casting, forging, and machining methods often suffer from low material utilization, long processing cycles, large machining allowances, and difficulties in machining complex thin-walled areas.

[0003] Metal 3D printing technology can directly obtain complex three-dimensional structures through layer-by-layer construction. Currently, powder-layout 3D printing technologies such as laser bed fusion offer high forming accuracy, but they typically require metal powder layup and a closed forming environment, resulting in relatively high costs for raw material preparation and equipment systems. Furthermore, for large, thin-walled components, their forming efficiency and size are easily limited by the equipment's forming space. In contrast, laser filament-fed 3D printing uses metal filaments as a continuous feeding material, offering advantages such as high material utilization, high continuous deposition efficiency, and convenient raw material use, giving it a significant advantage in the direct manufacturing of medium to large-sized thin-walled metal components.

[0004] However, traditional laser-fed 3D printing typically uses a single laser or a highly directional localized heat source. When the printing trajectory changes direction, the relative heating state between the laser, filament, and molten pool easily changes, resulting in differences in molten pool size, flow state, and solidification behavior in different directions. For thin-walled hexahedrons, this directional heat input affects the forming differences between edges and corners, causing fluctuations in local deposition width, layer height, and contour position, thus impacting overall geometric accuracy.

[0005] Thin-walled hexahedrons also possess a closed contour characteristic that distinguishes them from open straight-walled structures. During each layer of continuous printing, the printing trajectory has a starting and ending position, which converge during contour closure. Since the starting region has already undergone previous thermal cycling, when the printing trajectory returns to this region, localized repeated heating and heat accumulation can easily occur, causing changes in the molten pool size and the flow state of the liquid metal. Especially during continuous multi-layer printing, the continuous accumulation of heat in the closed region can easily lead to shape defects such as excessive local molten pool expansion, abnormal height, wall bulging, or collapse.

[0006] Furthermore, thin-walled hexahedrons are constructed using a layer-by-layer accumulation method. When local deviations occur in layer height, wall thickness, or contour position during single-layer deposition, these errors are propagated and accumulated layer by layer along the construction direction, ultimately leading to misalignment between different layers, reduced sidewall straightness, and decreased overall dimensional accuracy. Therefore, the key to filament-fed 3D printing of thin-walled hexahedrons lies not only in obtaining a complete structure but also in simultaneously controlling the heat accumulation in the closed contour region, the stability of the molten pool in different directions and at corners, and the accumulation of dimensional errors during continuous multi-layer construction, to achieve forming accuracy close to that required for precision 3D printing.

[0007] Therefore, it is necessary to provide a high-precision 3D printing method suitable for Ti-6Al-4V thin-walled hexahedrons to improve the problems of local collapse, contour distortion and reduced forming accuracy caused by directional heat input, local heat accumulation in closed contours and interlayer error accumulation in traditional filament feeding printing process. Summary of the Invention

[0008] The purpose of this invention is to provide a method for high-precision 3D printing of Ti-6Al-4V high-strength and tough thin-walled hexahedrons using a six-laser symmetrical coaxial heat source. By symmetrically arranging six laser beams around the central filament feed axis, the filament can maintain a relatively balanced heating state under different printing directions and continuous corner conditions, reducing the influence of traditional directional heat input on the molten pool morphology and deposition trajectory. At the same time, through stable central filament feed and multi-layer continuous printing process control, abnormal heat accumulation in the merging region of the closed contour of the thin-walled hexahedron is reduced, decreasing local collapse, contour distortion, and interlayer accuracy accumulation deviation, thereby improving the overall forming accuracy and printing stability of the thin-walled hexahedron.

[0009] To achieve the above objectives, the present invention adopts the following technical solution:

[0010] Six laser beams are used as a symmetrical and synergistic heat source. The six laser beams are arranged circumferentially around the central wire feeding axis and converge on the printing area, forming a circumferentially symmetrical heat input to the Ti-6Al-4V metal wire and the printing area. The Ti-6Al-4V metal wire is transported to the converging area formed by the six laser beams along the central wire feeding axis by the wire feeding mechanism. Under the action of the synergistic heat input of the six lasers, it melts to form a molten pool and forms a continuous metallurgical bond with the printed material.

[0011] The printing process is carried out continuously layer by layer according to the preset thin-walled hexahedral closed contour, so that the printing trajectory passes through each sidewall and corner in sequence, and the contour is closed at the end of each layer printing. The six-laser symmetrical heat input is used to reduce the change of the thermal state of the molten pool during the printing direction change and contour closure process, and improve the deposition consistency of each sidewall, corner and the start-end convergence area.

[0012] During the printing process, the laser power, wire feed speed, and scanning speed are kept stable, and the position of the wire feed nozzle is adjusted according to the building height to ensure that the Ti-6Al-4V metal wire continuously enters the center area of ​​the molten pool, thereby reducing the fluctuation of layer height and wall thickness caused by the wire deviating from the center of the molten pool.

[0013] During the printing process, a molten pool monitoring camera is used to observe the molten pool morphology, wire feeding status and deposition behavior in real time, in order to determine the stability of the molten pool in the sidewall, corner and closed contour confluence areas.

[0014] Preferably, the diameter of the Ti-6Al-4V metal wire is 1.0 to 1.4 mm.

[0015] Preferably, the six laser beams operate synchronously, with a total laser power of 1000–1200 W.

[0016] Preferably, the wire feeding speed of the Ti-6Al-4V metal wire is 10-14 mm / s, and the scanning speed is 9-13 mm / s.

[0017] Preferably, high-purity argon is used as the protective gas, the wire feeding gas flow rate is 10-14 L / min, and the side blowing gas flow rate is 12-18 L / min.

[0018] Preferably, continuous multi-layer printing is performed according to the closed contour of a thin-walled hexahedron, with 40 to 60 layers printed, an average layer height of 0.6 to 1.0 mm, and a total forming height of 30 to 50 mm.

[0019] The above parameter ranges are the preferred process ranges of the present invention and can be adjusted according to specific equipment conditions, component size and printing requirements. They should not be construed as limiting the scope of protection of the present invention.

[0020] Compared with traditional laser filament feeding printing methods with obvious directional heat input characteristics, the present invention has at least the following advantages:

[0021] (1) Six laser beams are symmetrically arranged around the central wire feeding axis, so that the metal wire and the molten pool can obtain a relatively balanced circumferential heat input under different printing directions, reduce the fluctuation of molten pool morphology and deposition width caused by the change of scanning direction, and improve the forming consistency between different sidewalls of the thin-walled hexahedron.

[0022] (2) In response to the problem of repeated heating at the starting and ending positions and obvious local heat accumulation during the printing of thin-walled hexahedron closed contours, the six laser symmetrical heat sources are beneficial to maintain the stability of the molten pool in the closed area, reduce local over-melting, material spreading and the resulting shape defects such as bulging, depression and collapse.

[0023] (3) The coaxial wire feeding method enables the Ti-6Al-4V metal wire to continuously enter the central region of the molten pool formed by the combined action of six laser beams, reducing the wire feeding position deviation caused by changes in printing direction and angle, which is beneficial to stabilizing the single-layer deposition height and wall thickness.

[0024] (4) By stabilizing the laser, wire feeding and scanning states during the multi-layer continuous construction process, the continuous accumulation of single-layer forming error along the construction direction can be reduced, and the contour overlap between different printing layers and the overall flatness and dimensional consistency of the thin-walled hexahedron sidewall can be improved.

[0025] (5) The Ti-6Al-4V thin-walled hexahedron prepared according to the specific embodiments of the present invention still maintains a complete and stable geometric contour after continuous multilayer construction, and no obvious local collapse is observed. The surface height change is controlled within 40 μm, indicating that the present invention can achieve high surface forming accuracy.

[0026] (6) This invention uses Ti-6Al-4V metal wire as a continuous feeding material, without the need for layer-by-layer powder laying. While maintaining high forming accuracy, it has the characteristics of continuous feeding, high material utilization and suitability for rapid construction of thin-walled components. It provides a 3D printing method that balances forming quality and manufacturing efficiency for medium and large-sized high-precision Ti-6Al-4V thin-walled structures.

[0027] (7) The Ti-6Al-4V thin-walled hexahedron obtained by the specific embodiment of the present invention mainly consists of a small number of isolated micropores, without forming continuous defect channels, and forms a relatively uniform α+β structure and a weak crystallographic texture, which further ensures the structural integrity and performance consistency of the printed thin-walled hexahedron in different directions. Attached Figure Description

[0028] Figure 1 This is a schematic diagram of the six-laser symmetrical coaxial filament feeding 3D printing system used in this invention, wherein, Figure 1 (a) is a schematic diagram of the overall structure and printing process of the 3D printing system, including six laser print heads, a filament feeding mechanism, a protective gas supply device, a robotic arm, and a molten pool monitoring system. Figure 1 (b) is a schematic diagram of a six-laser symmetrical coaxial printhead structure.

[0029] Figure 2 The surface height profile characterization results of the Ti-6Al-4V thin-walled hexahedral component prepared by the method of the present invention are shown. The surface height changes obtained along the predetermined scanning path of the inner and outer surfaces of the component are shown, which are used to evaluate the surface profile stability and interlayer forming consistency after continuous layer-by-layer construction.

[0030] Figure 3The results show the characterization of the internal quality and defects of the Ti-6Al-4V thin-walled hexahedral component prepared by the method of this invention. Figure 3 (a) shows the X-ray inspection results of the component. Figure 3 (b) Micro-CT cross-sectional images from different directions. Figure 3 (c) shows the three-dimensional spatial distribution of internal pores. Figure 3 (d) represents the relationship between the equivalent diameter of the pores and the pore volume.

[0031] Figure 4 The X-ray diffraction pattern of the Ti-6Al-4V thin-walled hexahedral component prepared by the method of the present invention is used to characterize the phase composition of the obtained component.

[0032] Figure 5 The optical microstructure of a Ti-6Al-4V thin-walled hexahedral component prepared using the method of this invention is shown below. Figure 5 (a) shows the low-magnification tissue morphology. Figure 5 (b) is the high-magnification morphology, used to characterize the microstructure of grain boundaries, α phase, and the transformation β region.

[0033] Figure 6 The above are the statistical results of electron backscattering diffraction of Ti-6Al-4V thin-walled hexahedral components prepared by the method of this invention, wherein... Figure 6 (a) and Figure 6 (b) Statistical results of geometrically necessary dislocation density and grain size in the low-magnification observation region, respectively. Figure 6 (c) and Figure 6 (d) shows the statistical results of geometrically necessary dislocation density and grain size in the high-magnification observation area, respectively.

[0034] Figure 7 The stress-strain curves along the X and Z directions of the Ti-6Al-4V thin-walled hexahedral component prepared by the method of this invention are used to evaluate the consistency of the mechanical properties of the component in different directions. Detailed Implementation

[0035] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. These embodiments are used to illustrate the technical solutions of the present invention and should not be construed as limiting the scope of protection of the present invention.

[0036] like Figure 1 As shown, this embodiment uses a six-laser symmetrical coaxial filament feeding 3D printing system to fabricate a Ti-6Al-4V thin-walled hexahedral component. Six laser beams are arranged circumferentially symmetrically around the central filament feeding axis and converge in the printing area; the Ti-6Al-4V metal filament enters the molten pool formed by the combined action of the six laser beams along the central filament feeding direction. A high-temperature resistant copper backplate is used as a temporary support and heat dissipation component during the printing process.

[0037] This embodiment uses 1.2 mm diameter Ti-6Al-4V metal wire as raw material, high-purity argon gas as protective gas, wire feeding gas flow rate of 12 L / min, and side blowing gas flow rate of 15 L / min. Six laser beams work synchronously, with a total laser power of 1100 W, a wire feeding speed of 12 mm / s, and a scanning speed of 11 mm / s.

[0038] During the printing process, the position of the filament feeding nozzle is adjusted according to the height of the structure to ensure that the Ti-6Al-4V metal filament continuously enters the central area of ​​the molten pool. A molten pool monitoring camera is used to observe the molten pool morphology, filament feeding status and deposition behavior in real time to maintain the stability of the printing process.

[0039] The printing process proceeds continuously, layer by layer, according to a pre-defined thin-walled hexahedral closed contour. Each layer's printing trajectory passes sequentially through the sidewalls and corners, completing contour closure upon returning to the starting area. Because the starting and ending segments of the closed contour experience repeated thermal cycles, localized heat accumulation is easily formed. This embodiment utilizes six lasers for symmetrical and coordinated heat input and a centrally stable wire feed to reduce differences in the molten pool state between different printing directions, corners, and contour closure areas, thereby minimizing forming defects such as localized build-up, depressions, and collapses.

[0040] In this embodiment, approximately 50 layers were printed, with an average layer height of approximately 0.8 mm and a total forming height of approximately 40 mm. After printing, the component was allowed to cool naturally to room temperature, and corresponding samples were prepared according to the needs of subsequent characterization.

[0041] like Figure 2 As shown, the surface of the obtained thin-walled hexahedron was characterized using laser scanning confocal microscopy. The deposition trajectory on the component surface was continuous, and the overall surface height variation was controlled within 40 μm. No obvious local protrusions, depressions, or collapses were observed, indicating that the present invention can maintain good interlayer consistency and surface forming accuracy during continuous multi-layer construction.

[0042] like Figure 3 As shown, X-ray and Micro-CT results indicate that the obtained thin-walled hexahedron mainly contains a small number of isolated micropores and does not form continuous defect channels, indicating that the component has good internal integrity. Figures 4 to 6 Further evidence shows that the obtained components are mainly composed of α-Ti phase and a small amount of β-Ti phase, forming a relatively uniform basket structure and exhibiting refined grain characteristics.

[0043] like Figure 7As shown, the engineering stress-strain curves of the obtained thin-walled hexahedrons along the X and Z directions are generally similar, with a maximum tensile strength of approximately 1180 MPa and an elongation after fracture exceeding 11%. This indicates that the present invention can achieve high-precision and stable forming of thin-walled hexahedrons while obtaining relatively consistent mechanical properties in different directions, especially with excellent high strength and high toughness.

[0044] The above results demonstrate that by combining a six-laser symmetrical coaxial heat source with central filament feeding, this invention can reduce the differences in heat input and local heat accumulation in different sidewalls, continuous corners, and the convergence areas of closed contours of thin-walled hexahedrons, suppressing local collapse and the accumulation of layer-by-layer forming errors, thereby achieving stable and high-precision 3D printing of Ti-6Al-4V thin-walled hexahedrons.

[0045] The laser power, wire feed speed, scanning speed, protective gas flow rate, number of deposition layers, layer height, and component height used in this embodiment are for illustrating a specific implementation of the present invention. Those skilled in the art can adjust the above process parameters according to specific equipment conditions and component dimensions without departing from the technical concept of the present invention.

Claims

1. A method for high-precision 3D printing of Ti-6Al-4V high-strength and tough thin-walled hexahedrons using a six-laser symmetrical coaxial heat source, characterized in that, Includes the following steps: (1) Ti-6Al-4V metal wire is used as the printing material, and the Ti-6Al-4V metal wire is fed to the printing area along the central wire feeding axis by the wire feeding mechanism; (2) Six laser beams are arranged circumferentially around the central wire feeding axis and converge on the printing area, so that the six laser beams form a symmetrical and coordinated heat input to the Ti-6Al-4V metal wire and the printing area; (3) Activate the six laser beams and the wire feeding mechanism to melt the Ti-6Al-4V metal wire under the action of the symmetrical synergistic heat input to form a molten pool and form a continuous metallurgical bond with the printed material; (4) Print continuously layer by layer according to the preset thin-walled hexahedron closed contour, so that the printing trajectory passes through each side wall and corner of the thin-walled hexahedron in sequence, and completes the single-layer contour closure after returning to the printing start area. (5) Repeat the layer-by-layer printing process until a Ti-6Al-4V thin-walled hexahedral component is formed.

2. The 3D printing method according to claim 1, characterized in that, During the printing process, the position of the filament feeding nozzle is adjusted according to the height of the structure to ensure that the Ti-6Al-4V metal wire continuously enters the central area of ​​the molten pool, and a molten pool monitoring camera is used to monitor the morphology of the molten pool and the filament feeding status in real time.

3. The 3D printing method according to claim 1 or 2, characterized in that, The Ti-6Al-4V metal wire has a diameter of 1.0–1.4 mm, the total power of the six laser beams is 1000–1200 W, the wire feeding speed is 10–14 mm / s, and the scanning speed is 9–13 mm / s.