Method for manufacturing an adhesive sheet
By combining low-energy and high-energy processes to cut the adhesive layer, the problem of film layer decomposition during laser cutting is solved, achieving high-quality semi-cutting of the adhesive sheet, which is suitable for the manufacturing of adhesive sheets for foldable display panels.
Patent Information
- Application Number
- CN202610695768.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-23
- Filing Date
- 2026-05-20
- Publication Date
- 2026-11-24
AI Technical Summary
During the laser cutting process of adhesive sheets, the laser passes through the adhesive layer and acts on the film layer, causing the film layer to decompose or vaporize, creating voids and affecting the cutting quality and depth. This is especially true when soft adhesive sheets are used in foldable display panels, where problems such as adhesion are easily generated.
A combination of low-energy and high-energy processes is used. First, the target area of the adhesive layer is cured by irradiating it with a low-energy laser. Then, the target area is cut with high energy to ensure the cutting quality of the adhesive layer and inhibit the cutting of the film layer, forming a semi-cut groove of appropriate depth.
This technology enables the formation of semi-cut grooves of appropriate depth on the adhesive sheet, improving processing quality, avoiding improper cutting of the film layer, and is suitable for the manufacture of adhesive sheets for foldable display panels.
Smart Images

Figure CN123149591A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing adhesive sheets. Background Technology
[0002] Display panels, for example, have a laminated structure comprising elements such as pixel panels, polarizing films, touch panels, and cover films. In the manufacturing process of such a display panel, optically transparent adhesive sheets (optical adhesive sheets) are used, for example, to bond the elements contained in the laminated structure together. These adhesive sheets are manufactured, for example, in a form where both sides of the sheet are covered by release liner (a form of adhesive sheet with an adhesive layer).
[0003] Conventional manufacturing methods for adhesive sheets used in display panels include, for example, those known as... Figure 5 The invention shown is a manufacturing method involving a stamping process using a die (blade). In this manufacturing method, firstly, as... Figure 5 As shown in (a), a workpiece film W' is prepared, comprising an adhesive sheet 90 as a long, unprocessed sheet and a long carrier film C' supporting the adhesive sheet 90 (preparation step). Then, as... Figure 5 As shown in (b), an adhesive sheet 90 having a first film layer 91, an adhesive layer 92, and a second film layer 93 in sequence is stamped to form multiple sheet-like (leaf-like) adhesive layers 92A and second film layers 93A (stamping process). The above stamping process is representatively shown in... Figure 6 The diagram shows the process of pressing the cutting edge 101 of the die 100 into the first film layer 91 from the second film layer 93 side onto the adhesive sheet 90. Following this stamping process, as... Figure 5 As shown in (c), the surrounding portions 92a and 93a are removed from the first film layer 91 (removal process). Afterwards, as... Figure 5 As shown in (d), the long first film layer 91 is cut into a single sheet of first film layer 91A (cutting process). This yields a single sheet of adhesive sheet Y' [first film layer 91A / adhesive layer 92A / second film layer 93A] having an adhesive layer. It should be noted that, in order to form protruding ends on the second film layer for easy peeling, a manufacturing method is also known that includes a step between the above-described removal process and the above-described cutting process of peeling off the second film layer 93A and then bonding the long film layer (film bonding replacement process) (illustration omitted).
[0004] Incidentally, in recent years, for example in smartphones and tablets, there has been development of display panels that can be repeatedly bent (foldable). Specifically, foldable display panels can repeatedly deform between curved and flat, non-curved shapes. In such foldable display panels, the components in the stacked structure are manufactured in a manner that allows for repeated bending, and thin optical adhesive sheets are used to join such components.
[0005] In particular, the adhesive sheet used for foldable display panels is required to be highly flexible in order to provide adequate conformability to the adhered object during bending and excellent stress relaxation properties. However, the softer the adhesive sheet, the more difficult it becomes to manufacture in the aforementioned conventional methods, such as... Figure 7 As shown by the single-dot dashed line, the end edges T and T' formed by stamping are more prone to deforming outwards, thus causing problems such as adhesion. Therefore, a manufacturing method using laser cutting to a specified shape has been proposed (for example, Patent Document 1 to Patent Document 2).
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: Japanese Patent Application Publication No. 2024-051400
[0009] Patent Document 2: Japanese Patent Application Publication No. 2024-143048 Summary of the Invention
[0010] The problem that the invention aims to solve
[0011] However, in the cutting of laminates using lasers, due to the nature of the laser, sometimes a portion of the laser light passes through the object being cut. For example, when cutting an adhesive sheet with an adhesive layer laminated on top of a film by irradiating it with a laser from the adhesive layer side, sometimes a portion of the irradiated laser light passes through the adhesive layer and acts on the film layer. Furthermore, for example, if the adhesive layer is photocurable, in the laser irradiation area, sometimes the curing reaction competes with the laser cutting, or the curing reaction occurs before the cutting. In these cases, although the laser is irradiated from the adhesive layer side of the adhesive sheet, the laser light that has passed through the adhesive layer acts on the film layer during the curing reaction of the adhesive layer. Thus, in the film layer below the laser irradiation area, the laser energy causes the film layer to decompose and vaporize, thereby creating voids in the film layer. As a result, sometimes the cutting of the film layer occurs before the cutting of the adhesive layer. Therefore, in the cutting of adhesive sheets using lasers, new processing quality problems sometimes arise, such as poor cutting of the adhesive layer, or the problem of the half-cut groove depth exceeding the expected depth due to the preemptive cutting of the film layer; etc.
[0012] The present invention was made in view of the above-mentioned problems, and its object is to provide a manufacturing method in which a half-cut groove formed on an adhesive sheet having an adhesive layer laminated on a film layer is properly cut and the cutting of the film layer is suppressed, thereby enabling the half-cut groove formed on the adhesive sheet to have an appropriate depth, that is, a manufacturing method that enables the half-cut adhesive sheet to be manufactured with excellent processing quality.
[0013] means for solving problems
[0014] In order to achieve the above objectives, the inventors conducted in-depth research and found that in a specific manufacturing method, in an adhesive sheet on which an adhesive layer is stacked on a film layer, the adhesive layer can be cut well and the cutting of the film layer can be suppressed. Therefore, a semi-cut groove of appropriate depth can be formed on the adhesive sheet, resulting in excellent processing quality.
[0015] That is, the present invention provides a method for manufacturing an adhesive sheet, wherein the method for manufacturing an adhesive sheet that has been partially cut is a method for manufacturing an adhesive sheet having a laminated structure in which a photocurable adhesive layer and a film layer are stacked in the thickness direction. The method for manufacturing an adhesive sheet includes: a low-energy step in which a laser is irradiated on a curing target area of the adhesive layer from the adhesive layer side to cure the curing target area; and a high-energy step in which a laser is irradiated on a cutting target area of the adhesive layer from the adhesive layer side to cut the adhesive layer along the cutting target area, thereby partially cutting the adhesive sheet, wherein a portion or all of the curing target area overlaps with the cutting target area, wherein when the irradiation energy of the laser in the low-energy step is set to E1 (μJ / mm) and the irradiation energy of the laser in the high-energy step is set to E2 (μJ / mm), E1 < E2.
[0016] The preferred manufacturing method described above involves cutting the adhesive layer using the high-energy process, resulting in an adhesive layer whose end faces do not have photocurability.
[0017] The preferred embodiment of the above manufacturing method is that when the scanning speed of the laser in the low-energy process is set to R1 (mm / s) and the scanning speed of the laser in the high-energy process is set to R2 (mm / s), R2 < R1.
[0018] The preferred embodiment of the above manufacturing method is that the ratio of the laser scanning speed R1 in the low-energy process to the laser scanning speed R2 in the high-energy process is R1:R2 = 1.5:1 to 50:1.
[0019] The above manufacturing method preferably involves the laser irradiated in the low-energy process satisfying one or more of the following conditions (1) or (2): (1) The laser is an ultraviolet laser; (2) The laser is a short-pulse laser.
[0020] Invention Effects
[0021] According to the manufacturing method of the adhesive sheet of the present invention, in the adhesive sheet on which the adhesive layer is stacked on the film layer, the adhesive layer can be cut well and the cutting of the film layer can be suppressed. Therefore, a semi-cut groove of appropriate depth can be formed on the adhesive sheet, resulting in excellent processing quality. Attached Figure Description
[0022] Figure 1 This is a flowchart of a method for manufacturing the adhesive sheet of the present invention.
[0023] Figure 2 This describes one embodiment of the method for manufacturing the adhesive sheet of the present invention. Figure 2 (a) indicates the preparation process. Figure 2 (b) indicates the external machining process. Figure 2 (c) indicates the removal process. Figure 2 (d) indicates the cutting process.
[0024] Figure 3 For the shape processing steps in the workpiece film ( Figure 2 A schematic top view of an example of the area following (b)).
[0025] Figure 4 To pass Figure 2 An enlarged cross-sectional view of the end of the adhesive sheet manufactured by the manufacturing method shown.
[0026] Figure 5 This represents an example of a conventional method for manufacturing adhesive sheets. Figure 5 (a) indicates the preparation process. Figure 5 (b) indicates the stamping process. Figure 5 (c) indicates the removal process. Figure 5 (d) indicates the cutting process.
[0027] Figure 6 This refers to the stamping process performed using a die.
[0028] Figure 7 This is a partially enlarged cross-sectional view of the cut area after the stamping process.
[0029] Label Explanation
[0030] W workpiece film
[0031] X Adhesive sheet (long size)
[0032] Y. Adhesive sheet (single sheet)
[0033] C carrier membrane
[0034] G Half-cut groove
[0035] H Thickness direction
[0036] D-side direction
[0037] D1 flow direction (flow direction)
[0038] D2 Width Direction
[0039] 10 First film layer (long dimension)
[0040] 11 First membrane layer (single sheet)
[0041] 11A Extended end
[0042] 20 adhesive layers (long dimension)
[0043] 21. Adhesive layer (single sheet)
[0044] 30 Second film layer (long dimension)
[0045] 31 Second membrane layer (single sheet)
[0046] L laser Detailed Implementation
[0047] [Manufacturing method of adhesive sheet]
[0048] The method for manufacturing the adhesive sheet of the present invention is a method for manufacturing an adhesive sheet that has undergone half-cutting. Hereinafter, using... Figures 1-4 One embodiment of the method for manufacturing the adhesive sheet of the present invention will be described.
[0049] Figure 1 The manufacturing method shown is a method of manufacturing a single-sheet adhesive sheet with an adhesive layer in a roll-to-roll manner. For example... Figure 1 As shown, the manufacturing method described above includes a preparation step S1, a low-energy step S2, a high-energy step S3, a removal step S4, and a cutting step S5. It should be noted that in this specification, the low-energy step S2 and the high-energy step S3 are sometimes collectively referred to as the "shape processing step." Furthermore, the manufacturing method of the adhesive sheet of the present invention is sometimes referred to as the "manufacturing method of the present invention," and the adhesive sheet obtained by the manufacturing method of the present invention is sometimes referred to as the "adhesive sheet of the present invention."
[0050] <Preparation Process>
[0051] In preparation step S1, such as Figure 2 As shown in (a), a long workpiece film W is prepared. The workpiece film W comprises a long adhesive sheet X and a carrier film C. The adhesive sheet X is a single-sheet adhesive sheet Y, described later. Figure 2 (d) The unprocessed sheet. Carrier film C supports adhesive sheet X.
[0052] The adhesive sheet X has, sequentially along the thickness direction H, a film layer 10 (first film layer), an adhesive layer 20, and a film layer 30 (second film layer). The adhesive layer 20 has a first surface 20a and a second surface 20b opposite to the first surface 20a. The film layer 10 is in contact with the first surface 20a. The film layer 30 is in contact with the second surface 20b. The adhesive sheet X extends in a plane direction orthogonal to the thickness direction H. It should be noted that when film layer 10 or film layer 30 is a substrate film, the laminate composed of film layer 10 or film layer 30 and adhesive layer 20 can be used as the single-sided adhesive sheet described later.
[0053] The carrier film C is a single-sided adhesive film with an adhesive surface on one side in the thickness direction H. In the workpiece film W, the adhesive surface of the carrier film C is attached to the film layer 10 side of the adhesive sheet X. Specifically, the workpiece film W has a carrier film C, a film layer 10, an adhesive layer 20, and a film layer 30 in sequence in the thickness direction H.
[0054] Furthermore, in this embodiment, in the flow direction D1 (of the workpiece film W) Figure 3 Orthogonal width direction D2 ( Figure 3 The carrier film C is wider than the adhesive sheet X. The adhesive sheet X is disposed, for example, at the center of the carrier film C in the width direction D2. The width of the adhesive sheet X (length in the width direction D2) is preferably 200 mm or more, more preferably 280 mm or more, and even more preferably 400 mm or more. Furthermore, the aforementioned width is preferably 2000 mm or less, more preferably 1800 mm or less, and even more preferably 1600 mm or less. Such a workpiece film W flows on the production line.
[0055] (First membrane layer)
[0056] The film layer 10 is, for example, a release liner, a functional optical film, or a substrate film (support film).
[0057] Materials used as release liner materials include, for example, polyester, polyolefins, and polycarbonate. Examples of polyesters include, for example, polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate. Examples of polyolefins include, for example, polyethylene, polypropylene, and cyclic olefin polymers (COP). The film layer 10, serving as the release liner, is in peelable contact with the first surface 20a of the adhesive layer 20. The surface of such film layer 10 (the surface on the adhesive layer 20 side) preferably undergoes a release treatment. Examples of release treatments include, for example, silicone release treatment and fluorinated release treatment. From the viewpoint of ensuring the protective function of the adhesive layer, the thickness of the release liner is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. From the viewpoint of reducing the thickness of the laminated film X, the thickness of the release liner is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less.
[0058] Examples of functional optical films include polarizing films and retardation films. Functional optical films can also be other optical films such as panel reinforcement materials. In the case where film layer 10 is a functional optical film, the first surface 20a of adhesive layer 20 is bonded to such film layer 10. Film layer 10, as a functional optical film, and adhesive layer 20 form a functional optical film with an adhesive layer.
[0059] Examples of polarizing films include hydrophilic polymer films that have undergone dyeing treatment using a dichroic substance and subsequent stretching treatment. Examples of dichroic substances include iodine and dichroic dyes. Examples of hydrophilic polymer films include polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified films of ethylene-vinyl acetate copolymers. Examples of polarizing films also include polyene-oriented films. Examples of materials for polyene-oriented films include dehydration products of PVA and dehydrochlorination products of polyvinyl chloride. The polarizing film may have a protective film bonded by an adhesive on one and / or the other side in the thickness direction. From the viewpoint of ensuring the function, strength, and durability of the polarizing film, the thickness of the polarizing film is preferably 10 μm or more, more preferably 20 μm or more. From the viewpoint of reducing the thickness of the laminated film X, the thickness of the polarizing film is preferably 500 μm or less, more preferably 300 μm or less.
[0060] Examples of phase retardation films include, for example, λ / 2 wavelength films, λ / 4 wavelength films, and viewing angle compensation films. Examples of materials for phase retardation films include polymer films that have undergone birefringence treatment through stretching. Examples of polymer films include cellulose films and polyester films. Examples of cellulose films include, for example, triacetylcellulose films. Examples of polyester films include, for example, polyethylene terephthalate films, polyethylene naphthalate films, and polybutylene terephthalate films. Examples of phase retardation films also include films having a substrate such as a cellulose film and an alignment layer of a liquid crystal compound such as a liquid crystal polymer on that substrate. From the viewpoint of ensuring the function and strength of the phase retardation film, the thickness of the phase retardation film is preferably 1 μm or more, more preferably 2 μm or more. From the viewpoint of reducing the thickness of the laminated film X, the thickness of the phase retardation film is preferably 100 μm or less, more preferably 80 μm or less.
[0061] Materials used as the substrate film include, for example, the materials described above used as release liner materials. When film layer 10 is the substrate film, the first side 20a of adhesive layer 20 is bonded to such film layer 10. Film layer 10, as the substrate film, and adhesive layer 20 form a single-sided adhesive sheet. From the viewpoint of ensuring the strength of the substrate, the thickness of the substrate film is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. From the viewpoint of reducing the thickness of the laminated film X, the thickness of the substrate film is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less.
[0062] (Adhesive layer)
[0063] The adhesive layer 20 can be a known or conventional photocurable adhesive layer. The adhesive layer of the adhesive sheet of the present invention is sometimes referred to as the "adhesive layer of the present invention". As the adhesive layer 20, a solvent-free adhesive layer comprising a photopolymerizable polymer as the base polymer is preferred. Specifically, the adhesive layer 20 is preferably a sheet-like pressure-sensitive adhesive (solvent-free adhesive sheet) formed from a solvent-free adhesive composition. Therefore, the adhesive layer 20 (solvent-free adhesive composition) preferably comprises at least a photopolymerizable polymer as the base polymer. A photopolymerizable polymer is a polymer formed by a polymerization method in which polymerizable components are polymerized by irradiation with active energy rays such as ultraviolet light.
[0064] The adhesive layer 20 can be formed from an adhesive composition. Preferably, the adhesive composition is a solvent-free adhesive composition. Solvent-free adhesive compositions eliminate the need for a process of removing solvents by evaporation from the coating film during the manufacture of the adhesive layer. Therefore, adhesive sheets having the adhesive layer are suitable for reducing environmental impact.
[0065] The base polymer is the adhesive component that exhibits adhesive properties in the adhesive layer 20. It should be noted that, in this specification, the base polymer refers to the main component of the polymer composition in the adhesive constituting the adhesive layer, for example, a polymer component with a content greater than 50% by mass. Relative to 100% by mass of the total adhesive layer, the content of the base polymer in the adhesive layer is preferably 60% by mass or more, more preferably 75% by mass or more (e.g., 75% by mass to 99.9% by mass), and even more preferably 85% by mass or more (e.g., 85% by mass to 99.9% by mass).
[0066] From the viewpoint of ensuring cohesion in the adhesive layer 20, the weight-average molecular weight of the aforementioned base polymer is preferably 100,000 or more, more preferably 300,000 or more, and even more preferably 500,000 or more. The aforementioned weight-average molecular weight is preferably 5 million or less, more preferably 3 million or less, and even more preferably 2 million or less. The aforementioned weight-average molecular weight is determined using gel permeation chromatography (GPC) and calculated using polystyrene conversion.
[0067] There are no particular limitations on the base polymers mentioned above, and examples include: acrylic polymers, rubber polymers (natural rubber polymers, synthetic rubber polymers, etc.), silicone polymers, polyester polymers, polyurethane polymers, polyamide polymers, epoxy polymers, vinyl alkyl ether polymers, fluorinated polymers, etc. Only one of the above-mentioned base polymers may be used, or two or more may be used. From the viewpoint of ensuring good transparency and adhesion in the adhesive layer 20, the above-mentioned adhesive composition preferably contains an acrylic polymer as the base polymer.
[0068] The aforementioned acrylic polymers are polymers that contain acrylic monomers (monomers having a (meth)acryloyl group in the molecule) as the main monomer component of the polymer. That is, the aforementioned acrylic polymers are polymers containing (meth)acrylate monomers in a proportion greater than 50% by mass. It should be noted that the acrylic polymer may use only one type or two or more types of acrylic monomers. Furthermore, the aforementioned acrylic polymers may contain only one type of acrylic monomer as a monomer component or may contain two or more types. It should be noted that in this specification, "(meth)acrylic acid" means "acrylic acid" and / or "methacrylic acid" (either or both of "acrylic acid" and "methacrylic acid"), and so on.
[0069] It should be noted that, in this specification, the term "monomer component" refers to a compound having only one polymerizable functional group (monofunctional monomer), and does not include compounds having two or more polymerizable functional groups, such as polyfunctional (meth)acrylates (polyfunctional monomers).
[0070] There are no particular limitations on the above-mentioned (meth)acrylates, but alkyl (meth)acrylates are preferred, and alkyl (meth)acrylates with 1 to 20 carbon atoms in the alkyl group are more preferred.
[0071] Examples of alkyl methacrylates include, for instance, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, pentyl methacrylate, n-hexyl methacrylate, heptyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, isooctyl methacrylate, nonyl methacrylate, isononyl methacrylate, decyl methacrylate, isodecanyl methacrylate, undecyl methacrylate, dodecyl methacrylate (i.e., lauryl methacrylate), isotridecyl methacrylate, and tetradecyl methacrylate. Alkyl methacrylates can be used alone or in combination with two or more. Preferably, at least one is selected from the group consisting of 2-ethylhexyl acrylate (2EHA), lauryl acrylate (LA), and n-butyl acrylate (BA).
[0072] The content ratio of the aforementioned alkyl methacrylate is not particularly limited. From the viewpoint of appropriately exhibiting basic properties such as adhesion in the adhesive layer 20, it is preferably 60% by mass or more, more preferably 70% by mass or more (e.g., 70% by mass to 99.9% by mass), and even more preferably 90% by mass or more (e.g., 90% by mass to 99.9% by mass), relative to the total amount of monomer components constituting the aforementioned acrylic polymer (100% by mass). Alternatively, the aforementioned content ratio may be, for example, 99% by mass or less.
[0073] In the aforementioned acrylic polymers, in addition to the alkyl methacrylates mentioned above, the monomeric components constituting the polymer may also include copolymerizable functionalized monomers (polymerizable functionalized monomers). That is, acrylic polymers may contain functionalized monomers as monomeric components constituting the polymer. It should be noted that only one type of functionalized monomer may be used, or two or more types may be used.
[0074] As the aforementioned functionalized monomers, hydroxyl-containing monomers are preferred. When acrylic polymers contain hydroxyl-containing monomers as monomer units, the monomer components constituting the polymer polymerize more easily, and the cohesive strength is improved. Furthermore, the interaction with the interface of the adherends is enhanced. Therefore, strong adhesion is easily obtained.
[0075] The aforementioned hydroxyl-containing monomers refer to monomers that have at least one hydroxyl group within their molecule. Additionally, monomers that have both at least one hydroxyl group and at least one carboxyl group within their molecule are carboxyl-containing monomers, not hydroxyl-containing monomers. There are no particular limitations on the types of hydroxyl-containing monomers mentioned above; specifically, examples include: 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl) methacrylate, etc., which are hydroxyl-containing (meth)acrylates; vinyl alcohol, allyl alcohol, etc. Among these, from the viewpoint of easily obtaining good cohesive strength and adhesive reliability at high temperatures, hydroxyl-containing (meth)acrylates are preferred as the aforementioned hydroxyl-containing monomers, and more preferably at least one selected from the group consisting of 2-hydroxyethyl acrylate (HEA), 2-hydroxypropyl acrylate (HPA), and 4-hydroxybutyl acrylate (4HBA). It should be noted that only one hydroxyl-containing monomer may be used, or two or more may be used.
[0076] The content (ratio) of the hydroxyl-containing monomer relative to the total amount (100% by mass) of the monomer components constituting the acrylic polymer is not particularly limited. From the viewpoint of introducing a cross-linking structure into the acrylic polymer and ensuring the cohesiveness of the adhesive layer 20, it is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more. From the viewpoint of adjusting the polarity of the acrylic polymer, the above-mentioned content ratio is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less.
[0077] Furthermore, nitrogen-containing monomers are preferred as examples of the aforementioned functionalized monomers. When acrylic polymers contain nitrogen-containing monomers as monomer units, they readily exhibit moderate cohesiveness, thus readily achieving strong adhesion and excellent resistance to foaming and peeling.
[0078] A nitrogen-containing monomer is a monomer that has at least one nitrogen atom within a molecule. However, the above-mentioned hydroxyl-containing monomers do not include the above-mentioned nitrogen-containing monomers. That is, in this specification, monomers having both a hydroxyl group and a nitrogen atom within a molecule are included in nitrogen-containing monomers. In addition, monomers having at least one nitrogen atom and at least one carboxyl group within a molecule are carboxyl-containing monomers, not nitrogen-containing monomers.
[0079] From the viewpoint of exerting strong adhesive force, N-vinylcyclic amides and (meth)acrylamides are preferred as the aforementioned nitrogen-containing monomers. It should be noted that only one nitrogen-containing monomer may be used, or two or more may be used.
[0080] From the viewpoint that it is easy to obtain good cohesiveness and adhesive reliability at high temperatures, the N-vinyl cyclic amide represented by the following formula (1) is preferred as the above-mentioned N-vinyl cyclic amide.
[0081]
[0082] (In equation (1), R) 1 (This indicates a divalent organic group.)
[0083] R in the above formula (1) 1 It is a divalent organic group, preferably a divalent saturated hydrocarbon group or an unsaturated hydrocarbon group, more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms).
[0084] As an N-vinyl cyclic amide represented by the above formula (1), from the viewpoint of further enhancing strong adhesion, N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-azin-2-one, N-vinyl-3,5-morpholinedione, etc. are preferred, N-vinyl-2-pyrrolidone and N-vinyl-2-caprolactam are more preferred, and N-vinyl-2-pyrrolidone is even more preferred.
[0085] Examples of the aforementioned (meth)acrylamides include: (meth)acrylamide, N-alkyl (meth)acrylamide, and N,N-dialkyl (meth)acrylamide. Examples of the aforementioned N-alkyl (meth)acrylamides include: N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-n-butyl (meth)acrylamide, and N-octylacrylamide. Furthermore, the aforementioned N-alkyl (meth)acrylamides also include (meth)acrylamides containing an amino group, such as dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and dimethylaminopropyl (meth)acrylamide. Examples of N,N-dialkyl(methyl)acrylamides include N,N-dimethyl(methyl)acrylamide, N,N-diethyl(methyl)acrylamide, N,N-dipropyl(methyl)acrylamide, N,N-diisopropyl(methyl)acrylamide, N,N-di(n-butyl)(methyl)acrylamide, and N,N-di(tert-butyl)(methyl)acrylamide.
[0086] Furthermore, the aforementioned (meth)acrylamides also include various N-hydroxyalkyl (meth)acrylamides. Examples of such N-hydroxyalkyl (meth)acrylamides include: N-hydroxymethyl (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, N-methyl-N-2-hydroxyethyl (meth)acrylamide, etc.
[0087] Furthermore, the aforementioned (meth)acrylamide class also includes various N-alkoxyalkyl (meth)acrylamides. Examples of such N-alkoxyalkyl (meth)acrylamides include N-methoxymethyl (meth)acrylamide and N-butoxymethyl (meth)acrylamide.
[0088] In addition to the aforementioned N-vinylcyclic amides and (meth)acrylamides, examples of nitrogen-containing monomers other than these include: aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate, etc.; cyano monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazolium, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinylpyrazole, vinylisopyrazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Monomers containing heterocyclic groups, such as vinylpyrrolidone; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimid monomers such as N-methylitconimide, N-ethylitconimide, N-butylitconimide, N-octylitconimide, N-(2-ethylhexyl)itconimide, N-laurylitconimide, and N-cyclohexylitconimide; succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and isocyanate monomers such as 2-(meth)acryloyloxyethyl isocyanate.
[0089] The content (ratio) of the nitrogen-containing monomers relative to the total amount (100% by mass) of the monomer components constituting the acrylic polymer is not particularly limited. However, from the viewpoint of ensuring the cohesiveness of the adhesive layer 20 and the adhesion of the adhesive layer 20 to the adhered object, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. From the viewpoint of adjusting the glass transition temperature and polarity of the acrylic polymer, the above-mentioned content ratio is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less.
[0090] In addition to the nitrogen-containing and hydroxyl-containing monomers mentioned above, other monomers that can be copolymerized in acrylic polymers include those with alicyclic structures [e.g., cyclopropyl methacrylate, cyclobutyl methacrylate, cyclopentyl methacrylate, cyclohexyl methacrylate, 3,3,5-trimethylcyclohexyl methacrylate, cycloheptyl methacrylate, cyclooctyl methacrylate, isobornyl methacrylate, tetrahydrodicyclopentadienyl methacrylate]; and alkoxyalkyl methacrylates [e.g., 2-methoxyethyl methacrylate, 2-ethoxyethyl methacrylate, methoxytriethylene glycol methacrylate, 3-methoxypropyl methacrylate, 3-ethyl methacrylate]. [Oxypropyl ester, 4-methoxybutyl acrylate, 4-ethoxybutyl acrylate, etc.]; epoxy-containing monomers [e.g. glycidyl acrylate, methyl glycidyl acrylate, etc.]; sulfonic acid-containing monomers [e.g. sodium vinyl sulfonate, etc.]; phosphate-containing monomers; (meth)acrylates having aromatic hydrocarbon groups [e.g. phenyl methacrylate, phenoxyethyl methacrylate, benzyl methacrylate, etc.]; vinyl esters [e.g. vinyl acetate, vinyl propionate, etc.]; aromatic vinyl compounds [e.g. styrene, vinyltoluene, etc.]; olefins or dienes [e.g. ethylene, propylene, butadiene, isoprene, isobutylene, etc.]; vinyl ethers [e.g. vinyl alkyl ethers, etc.]; vinyl chloride, etc.
[0091] The aforementioned acrylic polymers preferably do not contain, or substantially do not contain, carboxyl-containing monomers as monomeric components constituting the polymer. By eliminating or substantially eliminating carboxyl-containing monomers, a corrosion-resistant effect on the metal wiring can be achieved in touch panels in which optical components (touch sensor films) with metal mesh films, silver nanowire films, or similar metal wiring are bonded. The content of carboxyl-containing monomers relative to the total amount of monomeric components constituting the polymer is preferably 1 ng / cm³. 2 Below (e.g., 0-1 ng / cm) 2 ), more preferably 0.8 ng / cm 2Below (e.g., 0–0.8 ng / cm) 2 ), further preferably 0.5 ng / cm 2 Below (e.g., 0–0.5 ng / cm) 2 It can be said that it does not actually contain any of these compounds. It should be noted that examples of the aforementioned carboxyl-containing monomers include (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid. Additionally, the aforementioned carboxyl-containing monomers also include anhydride-containing monomers such as maleic anhydride and itaconic anhydride.
[0092] There are no particular limitations on the content (proportion) of the aforementioned functionalized monomers. From the viewpoint of achieving adequate adhesion, the content is preferably 5% to 40% by mass, more preferably 7% to 35% by mass, and even more preferably 10% to 30% by mass, relative to the total amount of monomer components constituting the acrylic polymer (100% by mass). In addition, it is preferable that the total content of hydroxyl-containing monomers and nitrogen-containing monomers is within the above range.
[0093] When the aforementioned acrylic polymer contains hydroxyl-containing monomers and nitrogen-containing monomers as functional group monomer components constituting the polymer, the proportion of functional group monomers, which are more abundant among the hydroxyl-containing monomers and nitrogen-containing monomers, is preferably 60% by mass or more, more preferably 65% by mass or more (e.g., 65% by mass to 99.9% by mass), and even more preferably 70% by mass or more (e.g., 70% by mass to 99.9% by mass) relative to the total amount of hydroxyl-containing monomers and nitrogen-containing monomers (100% by mass).
[0094] From the viewpoint of ensuring the flexibility of the adhesive layer 20, the glass transition temperature (Tg) calculated from the monomer components constituting the acrylic polymer is preferably below 0°C, more preferably below -10°C, and even more preferably below -20°C. The aforementioned glass transition temperature (Tg) can, for example, be above -80°C.
[0095] It should be noted that the glass transition temperature (Tg) mentioned above is a calculated glass transition temperature derived from the following Fox formula. This calculated glass transition temperature is based on the type and amount of each monomer component constituting the aforementioned acrylic polymer, and therefore can be adjusted by selecting the type and amount of each monomer component.
[0096] The glass transition temperature (Tg) calculated above can be obtained by the following Fox formula [1].
[0097] 1 / Calculate Tg=W1 / Tg(1)+W2 / Tg(2)+···+Wn / Tg(n) [1]
[0098] Here, W1, W2, ... Wn refer to the weight fraction (weight %) of each of the monomer components (1), (2), ... (n) constituting the acrylic polymer relative to the total monomer components, and Tg(1), Tg(2), ... Tg(n) represent the glass transition temperatures (in absolute temperature: K) of the homopolymers of monomer components (1), (2), ... (n).
[0099] It should be noted that the "glass transition temperature (Tg) of the homopolymer" (sometimes simply referred to as "the Tg of the homopolymer") in this specification refers to the "glass transition temperature (Tg) of the homopolymer of that monomer," and specifically, values from *Polymer Handbook* (3rd edition, John Wiley & Sons, Inc., 1987) can be cited. It should also be noted that, except for monomers with a polyorganosiloxane backbone, the Tg of homopolymers of monomers not described in the aforementioned literature is, for example, a value obtained by the following determination method (refer to Japanese Patent Application Publication No. 2007-51271). Specifically, 100 parts by mass of monomer, 0.2 parts by mass of 2,2'-azobisisobutyronitrile, and 200 parts by mass of ethyl acetate as the polymerization solvent are added to a reactor equipped with a thermometer, stirrer, nitrogen inlet pipe, and reflux condenser, and stirred for 1 hour while introducing nitrogen. Oxygen in the polymerization system is removed by the above operation, and then the temperature is raised to 63°C and reacted for 10 hours. Next, the mixture was cooled to room temperature to obtain a homopolymer solution with a solid content of 33% by mass. This homopolymer solution was then cast onto a release liner and dried to prepare a test sample (sheet-like homopolymer) approximately 2 mm thick. The test sample was then punched into a disc shape with a diameter of 7.9 mm, clamped with parallel plates, and viscoelasticity was measured using a viscoelasticity testing machine (trade name "ARES", manufactured by Rheometrics) in shear mode while applying a shear strain at a frequency of 1 Hz within a temperature range of -70°C to 150°C at a heating rate of 5°C / min. The peak temperature of tanδ was taken as the Tg of the homopolymer.
[0100] In order to form a crosslinked structure in the above-mentioned acrylic polymers, structural units derived from multifunctional compounds (e.g., multifunctional monomers, multifunctional oligomers) that can copolymerize with monomeric components that form acrylic polymers may be included.
[0101] Examples of multifunctional monomers include multifunctional (meth)acrylates containing two or more olefinic unsaturated double bonds in one molecule. From the viewpoint that cross-linking structures can be easily introduced through photopolymerization (active energy radiation polymerization), multifunctional (meth)acrylates are preferred as multifunctional monomers.
[0102] Examples of polyfunctional (meth)acrylates include difunctional (meth)acrylates, trifunctional (meth)acrylates, and polyfunctional (meth)acrylates with four or more functions.
[0103] Examples of bifunctional (meth)acrylates include: ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, glycerol dimethacrylate, neopentyl glycol dimethacrylate, stearic acid modified pentaerythritol dimethacrylate, dihydrodicyclopentadienyl diacrylate, di(meth)acryloyl isocyanurate, and ethoxylated bisphenol A diacrylate (BPAEODE).
[0104] Examples of trifunctional (meth)acrylates include: trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tri(acryloyloxyethyl) isocyanurate.
[0105] Examples of polyfunctional (meth)acrylates with more than four functions include: di(trimethylolpropane)tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, alkyl-modified dipentaerythritol pentaacrylate, and dipentaerythritol hexa(meth)acrylate.
[0106] The molecular weight of the multifunctional monomer is preferably 5000 or less, more preferably 3000 or less, even more preferably 2000 or less, and particularly preferably 1000 or less. Furthermore, the molecular weight is preferably 200 or more. When the molecular weight is within the above range, it is easier to make the viscoelasticity (e.g., shear storage modulus and dielectric loss tangent) of the base polymer more suitable.
[0107] Examples of multifunctional oligomers include: urethane acrylate oligomers (oligomers having a urethane backbone and two or more acryloyl groups), epoxy acrylate oligomers (oligomers having an epoxy backbone and two or more acryloyl groups), and silicone acrylate oligomers (oligomers having a siloxane backbone and two or more acryloyl groups). Uramate acrylate oligomers are preferred as multifunctional oligomers.
[0108] The weight-average molecular weight (Mw) of the multifunctional oligomer is preferably 20,000 or less, more preferably 15,000 or less, and even more preferably 5,000 or more. This configuration is preferred from the viewpoint of appropriately adjusting the viscoelasticity (e.g., shear storage modulus and dielectric loss tangent) of the base polymer. The weight-average molecular weight is determined by gel permeation chromatography (GPC) and calculated using polystyrene conversion.
[0109] In the polymerization of the aforementioned basic polymers (especially acrylic polymers), depending on the type of polymerization reaction, polymerization initiators such as thermal polymerization initiators and photopolymerization initiators (photoinitiators) can be used, with photopolymerization initiators being preferred. It should be noted that only one polymerization initiator can be used, or two or more can be used.
[0110] There are no particular limitations on the photopolymerization initiators mentioned above. Examples include: benzoin ether photopolymerization initiators, acetophenone photopolymerization initiators, α-keto alcohol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzoyl photopolymerization initiators, benzophenone photopolymerization initiators, ketal photopolymerization initiators, thioxanone photopolymerization initiators, etc. It should be noted that only one photopolymerization initiator can be used, or two or more can be used.
[0111] Examples of photopolymerization initiators for the aforementioned benzoin ethers include: benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-1-one, and anisoimine methyl ether. Examples of photopolymerization initiators for the aforementioned acetophenones include: 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 4-phenoxydichloroacetophenone, and 4-(tert-butyl)dichloroacetophenone. Examples of photopolymerization initiators for the aforementioned α-keto alcohols include: 2-methyl-2-hydroxyphenylacetone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropane-1-one. Examples of photopolymerization initiators for the aforementioned aromatic sulfonyl chlorides include: 2-naphthalenesulfonyl chloride. Examples of photoactive oxime photopolymerization initiators include 1-phenyl-1,1-propanedione-2-(O-ethoxycarbonyl)-oxime. Examples of benzoin-based photopolymerization initiators include benzoin. Examples of benzoinyl-based photopolymerization initiators include benzoinyl. Examples of benzophenone-based photopolymerization initiators include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, poly(vinylbenzophenone), α-hydroxycyclohexylphenyl ketone, etc. Examples of ketal-based photopolymerization initiators include benzoinyl dimethyl ketal. Examples of thioxanthone-based photopolymerization initiators include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, dodecylthioxanthone, etc.
[0112] There is no particular limitation on the amount of the photopolymerization initiator used in the polymerization of the above-mentioned base polymer (especially acrylic polymers). For example, it is preferably 0.001 to 1 part by mass relative to 100 parts by mass of all monomer units (total amount of monomer components constituting the base polymer) of the above-mentioned base polymer (especially acrylic polymers), and more preferably 0.01 to 0.50 parts by mass.
[0113] Furthermore, there are no particular limitations on the aforementioned thermal polymerization initiators, and examples include: azo polymerization initiators, peroxide polymerization initiators (such as benzoyl peroxide, tert-butyl maleate peroxide, etc.), and redox polymerization initiators. Among these, the azo polymerization initiators disclosed in Japanese Patent Application Publication No. 2002-69411 are preferred. Examples of the aforementioned azo polymerization initiators include: 2,2'-azobisisobutyronitrile (hereinafter sometimes referred to as "AIBN"), 2,2'-azobis(2-methylbutyronitrile) (hereinafter sometimes referred to as "AMBN"), dimethyl 2,2'-azobis(2-methylpropionic acid), and 4,4'-azobis(4-cyanopentanoic acid).
[0114] There is no particular limitation on the amount of the thermal polymerization initiator used in the polymerization of the aforementioned base polymer (especially acrylic polymers). For example, in the case of the aforementioned azo polymerization initiator, the amount can be 0.05 to 0.5 parts by mass or 0.1 to 0.3 parts by mass relative to 100 parts by mass of all monomer units (the total amount of monomer components constituting the base polymer) of the base polymer (especially acrylic polymers).
[0115] There are no particular limitations on the adhesive composition described above. Examples include compositions comprising the aforementioned base polymer (especially acrylic polymers); compositions comprising mixtures (sometimes referred to as "monomer mixtures") or portions thereof of the monomer components constituting the aforementioned base polymer. Examples of the former include water-dispersible compositions (emulsion compositions), and examples of the latter include active energy ray-cured compositions. Preferably, the adhesive composition comprises the aforementioned monomer mixture or portions thereof.
[0116] Examples of the aforementioned monomer mixtures include those composed of a single monomer component and those composed of two or more monomer components. Furthermore, the term "partial polymer," sometimes also referred to as "prepolymer," "slurry," etc., refers to a composition in which one or more monomer components in the aforementioned monomer mixture have been partially polymerized.
[0117] In addition to the photopolymerization initiator contained in the base polymer (especially acrylic polymers), the above-described adhesive composition may also contain a photopolymerization initiator. That is, a photopolymerization initiator may be added during the preparation of the above-described adhesive composition. As the photopolymerization initiator other than the photopolymerization initiator contained in the base polymer, photopolymerization initiators exemplified as those used in the base polymer can be used. It should be noted that only one photopolymerization initiator other than the photopolymerization initiator contained in the base polymer may be used, or two or more photopolymerization initiators may be used.
[0118] The content (proportion) of the photopolymerization initiator in the above-described adhesive composition, excluding the photopolymerization initiator contained in the base polymer (especially acrylic polymers), is not particularly limited. It is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, and even more preferably 0.05 parts by mass or more, and can be 0.1 parts by mass or more, relative to 100 parts by mass of the base polymer. Furthermore, the above-described content (proportion) is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, and can be 0.5 parts by mass or less, relative to 100 parts by mass of the base polymer.
[0119] Furthermore, the above-mentioned adhesive composition preferably does not contain or substantially does not contain organic solvents. As for the aforementioned organic solvents, there are no particular limitations on any organic compound that can be used as a solvent, such as: hydrocarbon solvents like cyclohexane, hexane, and heptane; aromatic solvents like toluene and xylene; ester solvents like ethyl acetate and methyl acetate; ketone solvents like acetone and methyl ethyl ketone; and alcohol solvents like methanol, ethanol, butanol, and isopropanol. It should be noted that only one of the above-mentioned organic solvents may be used, or two or more may be used.
[0120] In the above-mentioned adhesive composition, "substantially free of" organic solvents means that, except in cases where organic solvents are unavoidably mixed in, no organic solvents are actively incorporated. Specifically, the content of organic solvents in the adhesive composition is said to be substantially free of organic solvents if the total amount of the adhesive composition (100% by mass) is 1.0% by mass or less (preferably 0.5% by mass or less, more preferably 0.2% by mass or less).
[0121] After the adhesive layer 20 is formed from the above-described adhesive composition, a photopolymerization initiator may be further added thereto. Therefore, the source of the photopolymerization initiator contained in the adhesive layer 20 is not particularly limited, and may be: (i) a photopolymerization initiator contained in the above-described base polymer (especially an acrylic polymer), (ii) a photopolymerization initiator other than (i) added to the above-described adhesive composition, or (iii) a photopolymerization initiator further added after the adhesive layer 20 is formed from the above-described adhesive composition. It should be noted that, as the photopolymerization initiator added in (iii), a photopolymerization initiator exemplified as used in the above-described acrylic polymer may be used. Only one photopolymerization initiator may be used in (iii), or two or more may be used.
[0122] In (iii), the photopolymerization initiator can be added to the adhesive layer 20 by coating a solution of the photopolymerization initiator onto one side of the adhesive layer 20. The solution can be applied to either the first side 20a or the second side 20b of the adhesive layer 20. There are no particular limitations as long as the photopolymerization initiator solution is liquid and can be applied to and penetrate the adhesive layer 20. For example, if the photopolymerization initiator is liquid, it can be applied directly as a solution, or it can be applied as a solution obtained by dissolving the photopolymerization initiator in a solvent. By adding the solution as described above, the photopolymerization initiator in the solution penetrates along the thickness direction within the adhesive layer 20 at the aforementioned one side of the adhesive layer 20. As a result, the photopolymerization initiator is dissolved within the adhesive layer 20.
[0123] Furthermore, during the process of the photopolymerization initiator penetrating into the adhesive layer 20, a concentration gradient can be formed in the thickness direction. That is, the concentration of the photopolymerization initiator on the side coated with the above solution (the aforementioned one side) can be higher than that on the opposite side (the side opposite to the aforementioned one side).
[0124] Then, by drying the adhesive layer 20, the adhesive layer 20 is restored to a state close to that before the solution was applied. Therefore, in the adhesive layer 20, differences in physical properties between the surface and the back side, changes in adhesive strength, etc., can be further suppressed. When the adhesive layer 20 is dry, the penetration of the photopolymerization initiator into the adhesive layer 20 stops, and the concentration gradient of the photopolymerization initiator is fixed.
[0125] In the adhesive layer 20, the cumulative irradiation intensity is 3000 mJ / cm. 2 The difference ΔG(%)[G2-G1] between the gel fraction G1(%) before photocuring and the gel fraction G2(%) after photocuring under the aforementioned conditions can be 1% or more, or 2% or more, 3% or more, or 4% or more. There is no particular upper limit to the aforementioned ΔG(%); for example, the aforementioned ΔG(%) can be 10% or less. Specifically, the photocuring treatment can be performed by the following methods. Furthermore, the gel fraction can be determined by the following methods. In this specification, the adhesive layer with the aforementioned ΔG of 1% or more can be referred to as a "photocurable adhesive layer". The aforementioned gel fractions G1, G2, and the difference ΔG in the gel fraction can be controlled, for example, by adjusting the monomer composition, molecular weight, degree of crosslinking, type and amount of additives such as photopolymerization initiators and multifunctional compounds of the base polymer. Alternatively, it can be controlled by methods such as adding photopolymerization initiators, multifunctional compounds, etc., after the adhesive layer is formed (post-addition); or by not performing a photopolymerization reaction at all when the adhesive layer is formed by photocuring.
[0126] [Photocuring treatment]
[0127] The adhesive sheet (adhesive layer) formed between the release liner is irradiated with ultraviolet light under the following irradiation conditions, with the release liner in between.
[0128] (irradiation conditions)
[0129] Light source: metal halide lamp
[0130] Illuminance: 300mW / cm 2
[0131] Cumulative light exposure: 3000 mJ / cm 2
[0132] [Gel score]
[0133] Approximately 1 g of adhesive sample was collected from the adhesive sheet (adhesive layer), and its mass (W1) was determined. Next, the collected adhesive sample was immersed in 40 g of ethyl acetate in a container for 7 days. Then, the component insoluble in ethyl acetate (insoluble fraction) was completely recovered. Next, the insoluble fraction was dried at 130°C for 2 hours (removal of ethyl acetate). Next, the mass of the insoluble fraction (W2) was determined. Then, the gel fraction was calculated based on the following formula.
[0134] Gel fraction (mass%) = (W2 / W1) × 100
[0135] The adhesive layer 20 is photocurable, thus exhibiting the property of undergoing a photocuring reaction upon exposure to active energy rays such as ultraviolet light, resulting in an increase in gel fraction (high elasticity). Such an adhesive layer 20 is soft before photocuring and becomes highly elastic after photocuring, making it suitable for bonding components (adhesives) together before photocuring, and then ensuring good adhesive reliability through photocuring. Therefore, the adhesive layer 20 is suitable, for example, for display panel applications.
[0136] The adhesive layer 20 may, as needed and without impairing the characteristics of the present invention, contain known additives such as oligomers (preferably acrylic oligomers), silane coupling agents, ultraviolet absorbers, softeners, crosslinking agents, crosslinking accelerators, tackifying resins (rosin derivatives, polyterpene resins, oil-soluble phenolic resins, etc.), anti-aging agents, fillers, colorants (pigments, dyes, etc.), chain transfer agents, plasticizers, solvents, surfactants, antistatic agents, rust inhibitors, and antioxidants. It should be noted that only one such additive may be used, or two or more may be used.
[0137] The haze of the adhesive layer 20 is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. The haze can be measured using a haze meter according to JIS K7136. Examples of haze meters include the "NDH 2000" manufactured by Nippon Denshoku Kogyo Co., Ltd. and the "HM-150" manufactured by Murakami Color Technology Research Institute Co., Ltd.
[0138] From the viewpoint of ensuring the cohesiveness of the adhesive layer 20, the shear storage modulus of the adhesive layer 20 at 25°C is preferably 10 kPa or more, more preferably 15 kPa or more, even more preferably 20 kPa or more, and particularly preferably 25 kPa or more. From the viewpoint of achieving the flexibility required for optical adhesive sheets used in flexible devices in the adhesive layer 20, the above-mentioned shear storage modulus is preferably 500 kPa or less, more preferably 250 kPa or less, even more preferably 100 kPa or less, even more preferably 80 kPa or less, even more preferably 70 kPa or less, even more preferably 60 kPa or less, and particularly preferably 50 kPa or less. Methods for adjusting the shear storage modulus include, for example, the selection of the type of base polymer in the adhesive layer 20, adjustment of the molecular weight, adjustment of the amount of compounding, adjustment of the glass transition temperature, and adjustment of the degree of crosslinking. Methods for adjusting the shear storage modulus also include the selection of components other than the base polymer in the adhesive layer 20 and adjustment of their amounts. The shear storage modulus of the adhesive layer is determined by dynamic viscoelasticity measurement. This measurement can be performed using the Advanced Rheometric Expansion System (ARES) manufactured by RheometricScientific. In this measurement, the measurement mode is set to shear mode, the measurement temperature range is set to -40℃ to 100℃, the heating rate is set to 5℃ / min, and the frequency is set to 1Hz.
[0139] From the viewpoint of ensuring the adhesion of the adhesive layer 20, the thickness of the adhesive layer 20 is preferably 5 μm or more, more preferably 10 μm or more, further preferably 15 μm or more, and particularly preferably 30 μm or more. From the viewpoint of reducing the thickness of the adhesive sheet Y, the above-mentioned thickness is preferably 250 μm or less, more preferably 230 μm or less, further preferably 200 μm or less, and particularly preferably 150 μm or less.
[0140] (Second membrane layer)
[0141] Film layer 30 may be, for example, a release liner, a surface protective film, a functional optical film, or a substrate film (support film). It should be noted that, in this specification, when both film layer 10 and film layer 30 are release liners, the former is sometimes referred to as the first release liner and the latter as the second release liner.
[0142] Materials used as release liner materials include, for example, polyester, polyolefin, and polycarbonate. Specifically, materials exemplified as release liner materials used in the aforementioned film layer 10 can be listed. The film layer 30, serving as the release liner, is in peelable contact with the second surface 20b of the adhesive layer 20. The surface of such film layer 30 (the surface on the adhesive layer 20 side) preferably undergoes a release treatment. Examples of release treatments include, for example, silicone release treatment and fluorine-containing release treatment. From the viewpoint of ensuring the protective function of the adhesive layer 20, the thickness of the film layer 30 serving as the release liner is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. From the viewpoint of reducing the thickness of the adhesive sheet Y, the thickness of the film layer 30 serving as the release liner is preferably 150 μm or less, more preferably 120 μm or less, and even more preferably 100 μm or less.
[0143] When the film layer 30 is a surface protective film, the second side 20b of the adhesive layer 20 is bonded to such a film layer 30. The film layer 30, as a surface protective film, and the adhesive layer 20 form a surface protective film with an adhesive layer.
[0144] Materials used as surface protective films include, for example, polyimide (PI), polyester, polyolefin, and polycarbonate. Examples of polyesters include polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate. Examples of polyolefins include polyethylene, polypropylene, and cyclic olefin polymers (COP). From the viewpoint of ensuring the protective function of the surface protective film, the thickness of the film layer 30 is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. From the viewpoint of reducing the thickness of the surface protective film with the adhesive layer, the thickness of the film layer 30 is preferably 100 μm or less, more preferably 70 μm or less, and even more preferably 50 μm or less.
[0145] Examples of functional optical films include polarizing films and retardation films. Functional optical films can also be other optical films such as panel reinforcement materials. When film layer 30 is a functional optical film, the second surface 20b of adhesive layer 20 is bonded to such film layer 30. Film layer 30, as a functional optical film, and adhesive layer 20 form a functional optical film with an adhesive layer.
[0146] Examples of polarizing films include hydrophilic polymer films that have undergone dyeing treatment using a dichroic substance and subsequent stretching treatment. Examples of dichroic substances include iodine and dichroic dyes. Examples of hydrophilic polymer films include polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified films of ethylene-vinyl acetate copolymers. Polyene-oriented films can also be used as polarizing films. Materials for polyene-oriented films include, for example, dehydration products of PVA and dehydrochlorination products of polyvinyl chloride. The polarizing film may have a protective film bonded by an adhesive on one and / or the other side in the thickness direction. From the viewpoint of ensuring the function, strength, and durability of the polarizing film, the thickness of the polarizing film is preferably 10 μm or more, more preferably 20 μm or more. From the viewpoint of reducing the thickness of the adhesive sheet Y, the thickness of the polarizing film is preferably 500 μm or less, more preferably 300 μm or less.
[0147] Examples of phase retardation films include, for example, λ / 2 wavelength films, λ / 4 wavelength films, and viewing angle compensation films. Examples of materials for phase retardation films include polymer films that have undergone birefringence treatment through stretching. Examples of polymer films include cellulose films and polyester films. Examples of cellulose films include, for example, triacetylcellulose films. Examples of polyester films include, for example, polyethylene terephthalate films, polyethylene naphthalate films, and polybutylene terephthalate films. Also examples of phase retardation films include films having a substrate such as a cellulose film and an alignment layer on that substrate. The alignment layer is formed of a liquid crystal compound such as a liquid crystal polymer. From the viewpoint of ensuring the function and strength of the phase retardation film, the thickness of the phase retardation film is preferably 1 μm or more, more preferably 2 μm or more. From the viewpoint of reducing the thickness of the adhesive sheet Y, the thickness of the phase retardation film is preferably 100 μm or less, more preferably 80 μm or less.
[0148] Materials used as the substrate film include, for example, materials used as release liner materials. When film layer 30 is the substrate film, the second side 20b of adhesive layer 20 is bonded to such film layer 30. Film layer 30, as the substrate film, and adhesive layer 20 form a single-sided adhesive sheet. From the viewpoint of ensuring the strength of the substrate, the thickness of the substrate film is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. From the viewpoint of reducing the thickness of the adhesive sheet Y, the thickness of the substrate film is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less.
[0149] The adhesive sheet X can be manufactured, for example, by the following operation. First, the adhesive composition described above is applied to film layer 30 to form a coating film. Next, film layer 10 is bonded to the coating film on film layer 30. Then, it can be manufactured by drying and curing the coating film, or by irradiating the coating film with active energy rays to cure it. Alternatively, it can be further dried by heating if necessary. Thus, an adhesive layer 20 is formed between film layer 10 and film layer 30. The drying temperature of the coating film can be, for example, 50°C to 200°C. The drying time can be, for example, 5 seconds to 20 minutes. In addition, if necessary, film layer 10 and / or film layer 30 can be peeled off from the adhesive layer 20 formed by the above operation to expose the adhesive surface, and a solution of photopolymerization initiator can be applied to the adhesive surface (the additional addition in (iii) above). The exposed adhesive surface is preferably protected by laminating a new film layer 10' and / or film layer 30' before the shaping process described later, thereby producing an adhesive sheet X' having a laminated structure of [film layer 10 / adhesive layer 20 / film layer 30'], [film layer 10' / adhesive layer 20 / film layer 30], or [film layer 10' / adhesive layer 20 / film layer 30'].
[0150] It should be noted that the above-mentioned adhesive composition can be coated using known coating methods. For example, gravure roller coating machines, reverse roller coating machines, licking roller coating machines, dip roller coating machines, bar coating machines, doctor blade coating machines, spray coating machines, comma doctor blade coating machines, direct coating machines, and other coating machines can be used.
[0151] <Exterior machining process>
[0152] The shaping process includes a low-energy process S2 and a high-energy process S3. In the low-energy process S2, a laser is irradiated from the adhesive sheet X side of the workpiece film W (specifically, the film layer 30 side) in a manner consistent with the curing target area of the adhesive layer 20. Specifically, as... Figure 2 As shown in (b), a scanning laser L is irradiated and scanned from the film layer 30 side of the workpiece film W. This causes light absorption or multiphoton absorption in the laser-irradiated area (i.e., the curing target area) of the adhesive layer 20, resulting in a curing reaction. Next, in the high-energy process S3, a laser is irradiated from the adhesive sheet X side of the workpiece film W (specifically, the film layer 30 side) in a manner consistent with the cutting target area of the adhesive layer 20. In this embodiment, the curing target area and the cutting target area are the same, and the same area is irradiated with laser in both the low-energy process S2 and the high-energy process S3. This results in a full cut of the film layer 30 and the adhesive layer 20 along the cutting target area (curing target area), and further, a groove Ga is formed in the film layer 10 along the area directly below the cutting target area (curing target area). Figure 4 This creates a semi-cut groove G in the adhesive sheet X, which, when viewed from above, is a rounded rectangle. Figure 3 ).
[0153] In the manufacturing method of the present invention, at least a portion of the solidified target area (i.e., the laser irradiation area in the low-energy process S2) overlaps (repeates) with the cutting target area (i.e., the laser irradiation area in the high-energy process S3), or the entire solidified target area overlaps with the cutting target area. It should be noted that, in this specification, "at least a portion of the solidified target area overlaps with the cutting target area" means that the cutting target area includes a portion of the solidified target area in the form of a line (i.e., the laser irradiation path in the low-energy process overlaps with the laser irradiation path in the high-energy process by a certain length), and does not include the method where the cutting target area includes a portion of the solidified target area in the form of a point (i.e., the laser irradiation path in the low-energy process and the laser irradiation path in the high-energy process only intersect at a point). For example, the cutting target area A2 preferably includes more than 50% of the solidified target area A1, more preferably more than 80% of the solidified target area A1, and even more preferably more than 90% of the solidified target area A1. Furthermore, the cutting target area A2 can be the same as the solidified target area A1. It should be noted that the starting and ending points of the laser irradiation path in the high-energy process S3 can be set arbitrarily, and can be the same as or different from the starting and ending points of the laser irradiation path in the low-energy process S2.
[0154] In the shaping process of this embodiment, a small (piece-sized) adhesive layer 21 and a surrounding portion 22 are formed in the adhesive layer 20. Additionally, in the film layer 30, a film layer 31 is formed on the adhesive layer 21 and a surrounding portion 32 is formed around the film layer 31. A groove Ga, which is part of a semi-cut groove G, is formed in the film layer 10. Figure 3 This is a top view schematically representing an example of the area in the workpiece film W after the shape processing steps. Figure 3 In the diagram, the half-cut groove G is indicated by a shaded line. Figure 2 The partial sectional view shown in (b) is equivalent to Figure 3 The partial cross-sectional view of the workpiece film W along line II is shown.
[0155] The adhesive layer 20 is photocurable; therefore, when laser is irradiated from the film layer 30 side, the curing reaction competes with the cutting of the adhesive layer 20, or the curing reaction occurs before the cutting of the adhesive layer 20. Therefore, in the shaping process, if the laser irradiation step is only performed once, during the curing of the adhesive layer 20, the laser light passing through the adhesive layer 20 acts on the film layer 10, causing the film layer 10 to decompose and vaporize, sometimes creating voids in the film layer 10. It is presumed that even if the cutting of the adhesive layer 20 is insufficient, the cutting of the film layer 10 will still occur, resulting in grooves Ga( Figure 4The laser irradiation energy will deepen to a level beyond the expected degree. Therefore, in the manufacturing method of the present invention, when the laser irradiation energy in the low-energy step S2 is set to E1 (μJ / mm) and the laser irradiation energy in the high-energy step S3 is set to E2 (μJ / mm), the irradiation energy of each step is adjusted such that the relationship E1 < E2 holds. Thus, firstly, in the low-energy step S2, the load on the film layer 10 is suppressed by irradiating the laser with a lower irradiation energy, and the laser irradiated area of the adhesive layer 20 is cured. Therefore, in the high-energy step S3, due to the attenuation of the photocurability of the adhesive layer 20, the cutting process is more dominant than the curing reaction. It is presumably as a result that over-cutting of the film layer 10 can be suppressed, and the film layer 30 and the adhesive layer 20 can be cut well.
[0156] In addition to the low-energy step S2 and the high-energy step S3, the shaping process may also include an additional irradiation step, in which a portion or all of the cured target area is further irradiated with laser from the X side of the adhesive sheet (specifically, the film layer 30 side) once or twice. This additional irradiation step can be performed at any time after the low-energy step S2; specifically, it can be performed after the high-energy step S3 or between the low-energy step S2 and the high-energy step S3. However, when the additional irradiation step is performed between the low-energy step S2 and the high-energy step S3, the irradiation energy of the laser in this additional irradiation step is the same as or lower than the irradiation energy (E1) of the laser in the low-energy step S2.
[0157] In addition, the shaping process may include one or more processes that irradiate an area different from the laser irradiation area (curing target area) of the low-energy process S2 (other irradiation processes). The aforementioned other irradiation processes may be performed at any time during each process in the shaping process.
[0158] In the manufacturing method of the present invention, there are no particular limitations on the process of fully cutting the film layer 30 and the adhesive layer 20. For example, the film layer 30 can be fully cut in the low-energy process S2 or in the high-energy process S3, and if the above-mentioned additional irradiation process is included, the full cutting can be performed in the additional irradiation process. Similarly, the adhesive layer 20 can be fully cut in the low-energy process S2 or in the high-energy process S3, and if the above-mentioned additional irradiation process is included, the full cutting can be performed in the additional irradiation process.
[0159] (Low-energy process)
[0160] In the manufacturing method of the present invention, the oscillation mode of the laser in the low-energy step S2 is not particularly limited. Examples of such oscillation modes include pulsed oscillation and continuous oscillation. Therefore, the laser can be either a pulsed laser or a continuously oscillating laser. From the viewpoint of suppressing thermal deformation of the laser irradiation area, the laser oscillation mode is preferably a pulsed oscillation mode. That is, the laser is preferably a pulsed laser. If a pulsed laser is used, it is easier to perform ablation processing (non-thermal processing) based on multiphoton absorption in the irradiation area, thus facilitating cutting processing with excellent processing quality. It should be noted that, unless otherwise specified, "laser" is used in this specification as a general term encompassing pulsed lasers, continuously oscillating lasers, etc., without limiting the oscillation mode.
[0161] Types of lasers used in laser processing include gas lasers, solid-state lasers, and semiconductor lasers. Examples of gas lasers include F2 lasers (wavelength 157nm). Examples of solid-state lasers include: Ti:sapphire lasers (wavelength 800nm), Yb:YAG lasers (wavelength 1030nm), the second harmonic of Yb:YAG lasers (wavelength 515nm), Nd:YAG lasers (wavelength 1064nm), the second harmonic of Nd:YAG lasers (wavelength 532nm), the third harmonic of Nd:YAG lasers (wavelength 355nm), and the fourth harmonic of Nd:YAG lasers (wavelength 266nm). These are used in shaping processes... Figure 2 (b) The laser L is preferably selected from the group consisting of Yb:YAG laser (wavelength 1030nm), second harmonic of Yb:YAG laser (wavelength 515nm), Nd:YAG laser (wavelength 1064nm), and second harmonic of Nd:YAG laser (wavelength 532nm) from the perspective of suppressing the deviation of light absorption of each layer in the workpiece film W and from the perspective of using a high-output-power oscillator to increase cutting speed and ensure productivity.
[0162] From the perspective of balancing manufacturing efficiency and processing quality, the diameter of the laser irradiation spot is preferably 20 μm or more, more preferably 25 μm or more, and can be 30 μm or more, or 35 μm or more, 40 μm or more, or 50 μm or more. Furthermore, the diameter of the irradiation spot is preferably 90 μm or less, more preferably 80 μm or less.
[0163] From a manufacturing efficiency perspective, the laser scanning speed in the low-energy process S2 is preferably 50 mm / s or more, more preferably 80 mm / s or more, even more preferably 100 mm / s or more, even more preferably 120 mm / s or more, and particularly preferably 150 mm / s or more. Alternatively, the scanning speed can be 180 mm / s or more, or 200 mm / s or more. From the viewpoint of ensuring good processing quality, the scanning speed is preferably 6000 mm / s or less, more preferably 4000 mm / s or less, and even more preferably 3000 mm / s or less.
[0164] The average output power of the laser is preferably 1W or more, more preferably 5W or more, and even more preferably 10W or more. The average output power may be, for example, 1000W or less, or 500W or less, 100W or less, or 50W or less.
[0165] As an embodiment of the present invention, from the viewpoint of suppressing thermal deformation of the laser-irradiated area and appropriately photocuring in the adhesive layer 20, the laser is preferably an ultraviolet laser. Specifically, the wavelength of the laser is preferably 100 nm or more, more preferably 200 nm or more, and even more preferably 248 nm or more. Furthermore, the wavelength is preferably 2500 nm or less, more preferably 1800 nm or less, even more preferably 1200 nm or less, even more preferably 1000 nm or less, even more preferably 800 nm or less, even more preferably 500 nm or less, and particularly preferably 300 nm or less.
[0166] Furthermore, in one embodiment of the present invention, when the laser is a pulsed laser, from the viewpoint of suppressing thermal deformation of the laser-irradiated area and appropriately causing multiphoton absorption in the film layer 30 and the adhesive layer 20, the wavelength of the pulsed laser is preferably 100 nm or more, more preferably 200 nm or more, and even more preferably 248 nm or more. It can also be 500 nm or more, 800 nm or more, or 1000 nm or more. Additionally, the wavelength is preferably 2500 nm or less, more preferably 1800 nm or less, and even more preferably 1200 nm or less.
[0167] There is no particular limitation on the pulse width of the aforementioned pulsed laser. For example, based on the pulse width, examples include femtosecond pulsed lasers, picosecond pulsed lasers, nanosecond pulsed lasers, and microsecond pulsed lasers. From the viewpoint of ensuring appropriate multiphoton absorption in the film layer 30 and the adhesive layer 20, the aforementioned pulsed laser is preferably a short-pulse laser (picosecond pulsed laser or femtosecond pulsed laser), and from the viewpoint of suppressing thermal deformation of the laser-irradiated region, a femtosecond pulsed laser is more preferred.
[0168] In this embodiment, the laser used in the low-energy process S2 is particularly preferably one or more of the following conditions (1) or (2). By satisfying these conditions, light absorption or multiphoton absorption easily occurs in the laser-irradiated area of the adhesive layer 20, enabling the laser-irradiated area to be moderately cured.
[0169] (1) The laser is an ultraviolet laser.
[0170] (2) The laser is a short-pulse laser.
[0171] From the viewpoint that multiphoton absorption can occur appropriately in the film layer 30 and the adhesive layer 20, the pulse width of the aforementioned pulsed laser is preferably 100 × 10⁻⁶. -15 s (100 femtoseconds) or more, preferably 150 × 10 -15 s or higher, further preferably 200×10 -15 The pulse width is above s. Furthermore, the preferred pulse width is 60 × 10⁻⁶. -12 Less than 60 picoseconds, more preferably 20 × 10 -12 Below s, further preferably 10×10 -12 Below s.
[0172] From the viewpoint that multiphoton absorption can be appropriately achieved in the film layer 30 and the adhesive layer 20, the repetition frequency of the pulses of the aforementioned pulsed laser is preferably 50 kHz or more, more preferably 80 kHz or more, and even more preferably 100 kHz or more. Furthermore, the aforementioned frequency is preferably 5000 kHz or less, more preferably 4000 kHz or less, and even more preferably 3000 kHz or less.
[0173] From the viewpoint of ensuring appropriate multiphoton absorption in the film layer 30 and the adhesive layer 20, the pulse energy of the aforementioned pulsed laser is preferably 10 μJ or more, more preferably 20 μJ or more, even more preferably 30 μJ or more, and particularly preferably 50 μJ or more. From the viewpoint of suppressing thermal deformation in the film layer 10 during the shaping process, the aforementioned pulse energy is preferably 300 μJ or less, more preferably 150 μJ or less, and even more preferably 100 μJ or less. It should be noted that the pulse energy [J] can be calculated by dividing the average output power [W] by the frequency [Hz].
[0174] From the viewpoint that multiphoton absorption can occur appropriately in the film layer 30 and the adhesive layer 20, the peak output power of the aforementioned pulsed laser is preferably 0.1 × 10⁻⁶. 7 W or more, preferably 0.5 × 10 7 W or more, further preferably 1×10 7 W or more. The aforementioned peak output power could, for example, be 800 × 10⁻⁶. 7 For values below W, it can also be 500×10.7 Below W, 100×10 7 Below W, or 10×10 7 Below W. It should be noted that the peak output power [W] can be calculated from the pulse energy [J] / pulse width [s].
[0175] From the viewpoint of suppressing the load on the film layer 10 and moderately curing the adhesive layer 20, the irradiation energy (E1) per unit irradiation length in the low-energy process S2 is preferably 0.1 × 10⁻⁶. 4 μJ / mm or higher, more preferably 0.5×10 μJ / mm. 4 μJ / mm or higher, more preferably 1×10 4 μJ / mm or higher. The irradiation energy (E1) per unit irradiation length can be, for example, 50 × 10⁻⁶. 4 Below μJ / mm, it can also be 30×10 4 Below μJ / mm, 20×10 4 Below μJ / mm, or 10×10 4 Below μJ / mm. It should be noted that the irradiation energy [J / mm] is calculated by dividing the average output power [W] by the scan rate [mm / s].
[0176] (High-energy process)
[0177] The oscillation mode, laser, and laser type of the laser in the high-energy process S3 can be exemplified and explained by those examples used in the low-energy process S2. Furthermore, the preferred methods for the oscillation mode, laser, and laser type of the laser in the high-energy process S3 are the same as those for the low-energy process S2.
[0178] The preferred method for the irradiation spot diameter of the laser described above is the same as the preferred method for the irradiation spot diameter of the laser in the low-energy step S2. Furthermore, the preferred method for the average output power of the laser described above is the same as the preferred method for the average output power of the laser in the low-energy step S2. Additionally, the preferred method for the wavelength of the laser described above is the same as the preferred method for the wavelength of the laser in the low-energy step S2.
[0179] Furthermore, the pulsed laser used in the high-energy process S3 can be exemplified and described as the pulsed laser used in the low-energy process S2. The preferred method for the pulsed laser in the high-energy process S3 is the same as that for the pulsed laser in the low-energy process S2. The preferred method for the wavelength of the pulsed laser is the same as that for the pulsed laser in the low-energy process S2. The preferred method for the pulse width of the pulsed laser is the same as that for the pulse width of the pulsed laser in the low-energy process S2. The preferred method for the pulse repetition frequency of the pulsed laser is the same as that for the pulse repetition frequency of the pulsed laser in the low-energy process S2. The preferred method for the pulse energy of the pulsed laser is the same as that for the pulse energy of the pulsed laser in the low-energy process S2. The preferred method for the peak output power of the pulsed laser is the same as that for the peak output power of the pulsed laser in the low-energy process S2.
[0180] From a manufacturing efficiency perspective, the laser scanning speed in the high-energy process S3 is preferably 20 mm / s or more, more preferably 30 mm / s or more, and even more preferably 50 mm / s or more. Alternatively, the scanning speed can be 80 mm / s or more, 90 mm / s or more, or 100 mm / s or more. From the viewpoint of ensuring good processing quality, the scanning speed is preferably 6000 mm / s or less, more preferably 4000 mm / s or less, and even more preferably 3000 mm / s or less.
[0181] From the viewpoint of adequately cutting the film layer 30 and the adhesive layer 20, the irradiation energy (E2) per unit irradiation length in the high-energy process S3 is preferably 0.1 × 10⁻⁶. 5 μJ / mm or higher, more preferably 0.3×10 μJ / mm. 5 μJ / mm or higher, more preferably 0.5×10 μJ / mm 5 μJ / mm or higher. The irradiation energy (E2) per unit irradiation length can be, for example, 50 × 10⁻⁶. 5 Below μJ / mm, it can also be 30×10 5 Below μJ / mm, 20×10 5 Below μJ / mm, 10×10 5 Below μJ / mm, or 5×10 5 Below μJ / mm.
[0182] The ratio of E2 to E1 [E2 / E1] is greater than 1.0, preferably 1.1 or more, more preferably 1.3 or more, and even more preferably 1.5 or more. Alternatively, the ratio can be 1.6 or more, or 1.8 or more, 2.0 or more, 2.3 or more, or 2.5 or more. For example, the ratio can be 20 or less, or 10 or less, or 5.0 or less. The ratio can be adjusted by appropriately changing the scanning speed, average output power, frequency, pulse energy, wavelength, pulse width, etc., of the low-energy process S2 and the high-energy process S3. Furthermore, in the manufacturing method of the present invention, when the shape processing process includes one or more additional irradiation processes, it is preferable that the laser irradiation energy E1 in the low-energy process S2 is minimized.
[0183] The ratio [R1:R2] of the laser scanning speed R1 in the low-energy process S2 to the laser scanning speed R2 in the high-energy process S3 is preferably 1.5:1 to 50:1, more preferably 3:1 to 45:1, further preferably 10:1 to 45:1, and particularly preferably 15:1 to 45:1. Furthermore, in the manufacturing method of the present invention, when the shape processing step includes one or more additional irradiation steps, the laser scanning speed in the low-energy process S2 is preferably the fastest.
[0184] <Removal Process>
[0185] In the removal process S4, such as Figure 2 As shown in (c), the surrounding portions 22 and 32 are removed from the film layer 10. Figure 2 (b)). In the manufacturing method of the present invention, the film layer 30 and the adhesive layer 20 can be cut well without excessive cutting of the film layer 10, so that the surrounding portions 22 and 32 can be removed smoothly.
[0186] <Cutting Process>
[0187] In cutting process S5, such as Figure 2 As shown in (d), the long film layer 10 is cut into single-sheet film layers 11, thereby forming smaller film layers 11 in the film layer 10. Examples of cutting methods include cutting by laser irradiation and cutting by stamping (cutting) using a die.
[0188] Through the above operations, an adhesive sheet Y in which film layer 11, adhesive layer 21, and film layer 31 are stacked in this order along the thickness direction H can be manufactured. For example... Figure 4As shown, the adhesive layer 21 has an end face 21a formed in the above-described shaping process. The film layer 31 has an end face 31a formed in the shaping process. The end face 31a is flush with the end face 21a. The film layer 11 has a groove Ga formed along the end face 21a. The end faces 21a and 31a are, for example, inclined surfaces that extend outward toward the carrier film C in the thickness direction H. The angle α (inclination angle of the end face 21a) formed between the end face 21a and the surface of the adhesive layer 21 on the film layer 10 side can be, for example, 60° to 88°. The angle β (inclination angle of the end face 31a) formed between the end face 31a and the surface of the film layer 31 on the adhesive layer 20 side can be, for example, 60° to 88°.
[0189] The film layer 11 has a protruding end 11A. The protruding end 11A is in the plane direction D (orthogonal to the thickness direction H). Figure 4 The film layer 11 extends further outward than the end face 21a of the adhesive layer 21. That is, the film layer 11 has an outer end 11e in the planar direction D, located further outward than the outer end 21e of the adhesive layer 21. From the viewpoint of suppressing end adhesion when multiple adhesive sheets Y are overlapped in the thickness direction H, the protrusion length d1 of the protruding end 11A in the planar direction D (the direction orthogonal to the end face 21a when viewed from above), measured from the outer end 21e, is preferably 70 μm or more, more preferably 90 μm or more, and even more preferably 100 μm or more. From the viewpoint of efficiently manufacturing the adhesive sheet Y, the protrusion length d1 is preferably 200 μm or less, more preferably 170 μm or less, and even more preferably 150 μm or less. The protrusion length d1 is the length in the planar direction D from the outer end 21e of the adhesive layer 21 to the outer end 11e of the film layer 11, and is the maximum length of the protruding end 11A.
[0190] The distance between the inner end 31e of the end face 31a of the film layer 31 and the outer end Ge of the groove Ga on the surface direction D (orthogonal to the end face 21a when viewed from above) is defined as the edge width d2. The edge width d2 is preferably 100 μm or less, more preferably 80 μm or less. The edge width d2 is, for example, 10 μm or more or 20 μm or more. The area of the edge width d2 is part of the edge area that can be used as an alignment mark (edge alignment mark) for end detection of the manufactured adhesive sheet Y. When the edge width d2 is 100 μm or less (preferably 80 μm or less), false detection of the edge alignment mark by the detection camera can be suppressed (false detection occurs when the edge alignment mark is too large).
[0191] In the aforementioned shaping process, the end face 21a of the adhesive layer 21 formed by laser irradiation cutting preferably does not have photocurability. The non-photocurable end face 21a can be formed as follows: by irradiating with a laser in a low-energy step S2, preferably light absorption or multiphoton absorption occurs, thereby carrying out a curing reaction, which reduces photocurability and forms a non-photocurable end face 21a. Such an end face 21a cures as the curing reaction proceeds, becoming harder than before the shaping process, and is therefore suitable for suppressing adhesion.
[0192] The hardness of end face 21a is not particularly limited. End face 21a may have, for example, a hardness H1, which is the surface hardness at 25°C as measured by nanoindentation. Additionally, a portion located 20 μm inward from end face 21a toward the surface of adhesive sheet Y may have a hardness H2, which is the surface hardness at 25°C as measured by nanoindentation. From the viewpoint of suppressing accidental deformation of the end face, the ratio of H1 to H2 [H1 / H2] is preferably 1.15 or more, more preferably 1.50 or more, further preferably 2.00 or more, more preferably 2.50 or more, and particularly preferably 2.70 or more. From the viewpoint of suppressing cracks in the end face, the above ratio is preferably 10.0 or less, more preferably 7.00 or less, further preferably 5.00 or less, and particularly preferably 3.50 or less. Furthermore, when the portion located 200 μm away from the end face 21a in the direction inward toward the surface of the adhesive sheet Y has a hardness H3, which is the surface hardness at 25°C as measured by nanoindentation, the ratio of H1 to H3 [H1 / H3] is preferably within the range described above.
[0193] Nanoindentation is a technique for determining various physical properties of a sample at the nanoscale. In this embodiment, nanoindentation is performed according to ISO 14577. In nanoindentation, the process of pressing an indenter into a sample placed on a stage (load application process) and then removing the indenter from the sample (load removal process) is performed. During this series of processes, the load acting between the indenter and the sample and the relative displacement of the indenter relative to the sample are measured (load-displacement measurement). This yields a load-displacement curve. Based on this load-displacement curve, various physical properties (hardness and elastic modulus, etc.) determined at the nanoscale can be calculated for the surface of the sample. For example, a nanoindenter (trade name "Triboindenter," manufactured by Hysitron Corporation) can be used for load-displacement measurements using nanoindentation. In this measurement, the measurement mode was set to single indentation measurement, the measurement temperature was set to 25℃, and a Berkovich (triangular pyramidal) diamond indenter (20μm in diameter) was used. The maximum indentation depth (maximum displacement hmax) of the indenter relative to the test sample during load application was set to 4μm, the indentation speed of the indenter was set to 1000nm / s, and the withdrawal speed of the indenter from the test sample during load removal was set to 1000nm / s. The obtained measurement data were then processed using the dedicated analysis software (Ver. 9.4.0.1) of the "TI 950 Triboindenter". Specifically, based on the obtained load (F)-displacement (h) curve, the maximum load F was calculated. max (at the maximum displacement h) max The load acting on the indenter), the contact projection area Ap (the projected area of the contact area between the indenter and the specimen at maximum load), and the surface hardness of the specimen (=F) are measured. max / Ap).
[0194] The external machining process in this manufacturing method ( Figure 2 In (b)), as described above, the adhesive sheet Y (a single sheet of adhesive with an adhesive layer) is obtained by laser processing. Laser processing is suitable for continuously processing the shape while the workpiece film W flows continuously. Therefore, the manufacturing method of the present invention is suitable for efficiently manufacturing the adhesive sheet Y.
[0195] The adhesive sheet of the present invention can be a double-sided adhesive sheet with adhesive layer surfaces on both sides, or a single-sided adhesive sheet with adhesive layer surfaces on only one side. It should be noted that, in this specification, the term "adhesive sheet" also includes strip-shaped objects, i.e., "adhesive tape." Furthermore, in this specification, the adhesive layer surface is sometimes referred to as the "adhesive surface."
[0196] The aforementioned adhesive sheet can be a so-called "substrate-free" adhesive sheet (hereinafter, sometimes referred to as "substrate-free adhesive sheet") that does not have a substrate (substrate layer), or it can be an adhesive sheet with a substrate (hereinafter, sometimes referred to as "adhesive sheet with substrate"). Examples of the aforementioned substrate-free adhesive sheets include, for instance, double-sided adhesive sheets containing only the adhesive layer of the present invention, and double-sided adhesive sheets containing the adhesive layer of the present invention and an adhesive layer other than the adhesive layer of the present invention (sometimes referred to as "other adhesive layers"). On the other hand, examples of adhesive sheets with a substrate include adhesive sheets having the adhesive layer of the present invention on at least one side of the substrate. The adhesive layers on both sides of the aforementioned double-sided adhesive sheet with a substrate can both be the adhesive layer of the present invention, or one can be the adhesive layer of the present invention and the other can be another adhesive layer. It should be noted that the aforementioned "substrate (substrate layer)" does not include the release liner that is peeled off when using (adhering) the adhesive sheet.
[0197] The manufacturing method of the present invention may also include steps other than the preparation steps S1 to the cutting steps S5. Examples of these other steps include a film layer bonding and replacement step S6. When the manufacturing method of the present invention includes a film layer bonding and replacement step S6, the film layer bonding and replacement step S6 can be performed before the preparation step S1, at any time during each of the preparation steps S1 to the cutting steps S5, and at any stage after the cutting step S5. Furthermore, the manufacturing method of the present invention may include one film layer bonding and replacement step S6, or it may include two or more steps. It should be noted that the manufacturing method of the present invention may omit some of the steps from the preparation steps S1 to the film layer bonding and replacement steps S6 (e.g., steps other than the low-energy step S2 and the high-energy step S3).
[0198] In the film layer bonding and replacement step S6, any optional film layer is peeled off from the adhesive layer, and then other films are bonded to the exposed adhesive surface of the adhesive layer 20. For example, in the manufacturing method of the present invention, in the removal step S4 ( Figure 2 (c) and cutting process S5 Figure 2 In the case of a film layer bonding and replacement step S6 between (d) and (d), after peeling film layer 31 from adhesive layer 21, another film layer is bonded to the adhesive surface of the exposed second side of adhesive layer 21. Here, the other film layer may be a film layer with a surface area larger than the adhesive surface of adhesive layer 20. When using such another film layer, in the cutting step S5, by cutting the area where the other film layer and film layer 11 are present but adhesive layer 21 is absent, a protruding end that extends further outward than the end face 21a of adhesive layer 21 can be formed in the other film layer. When the other film layer has a protruding end, it can be easily peeled off during use, thus providing excellent convenience.
[0199] As described above, the manufacturing method according to the present invention can suppress thermal deformation and vaporization of the film layer 10, and can effectively cut the film layer 30 and the adhesive layer 20, thus enabling the efficient manufacturing of adhesive sheets with semi-cut grooves of appropriate depth with excellent processing quality.
[0200] The embodiments described above are for the purpose of making the present invention easier to understand, and are not intended to limit the present invention.
[0201] Example
[0202] The following examples illustrate the invention in more detail, but the invention is not limited to these examples.
[0203] Example 1
[0204] [Production process of adhesive sheet]
[0205] (Preparation of acrylic oligomers)
[0206] First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet, a mixture containing 60 parts by mass of tetrahydrodicyclopentadienyl methacrylate (DCPMA), 40 parts by mass of methyl methacrylate (MMA), 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added to the mixture, thereby preparing a reaction solution. The reaction was carried out at 70°C for 2 hours under a nitrogen atmosphere, followed by a reaction at 80°C for 2 hours (polymerization reaction). Then, the reaction solution was heated at 130°C to volatilize and remove the toluene, chain transfer agent, and unreacted monomers. This yielded an acrylic oligomer (solid). The weight-average molecular weight of this acrylic oligomer was 5100.
[0207] (Preparation of the prepolymer composition)
[0208] In a flask, 0.031 parts by weight of photopolymerization initiator (trade name "Omnirad 184", 1-hydroxycyclohexylphenyl ketone, manufactured by BASF) and 0.031 parts by weight of photopolymerization initiator (trade name "Omnirad 651", 2,2-dimethoxy-1,2-diphenylethane-1-one, manufactured by BASF) were added to a monomer mixture comprising 71 parts by weight of n-butyl acrylate (BA), 13 parts by weight of N-vinyl-2-pyrrolidone (NVP), 13 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 3 parts by weight of acryloylmorpholine (ACMO). The mixture was then irradiated with ultraviolet light under a nitrogen atmosphere, thereby polymerizing a portion of the monomer components in the mixture to obtain a prepolymer composition. UV irradiation continued until the viscosity of the composition reached approximately 20 Pa·s. This viscosity was measured using a Type B viscometer under the conditions of rotor No. 5, rotor speed of 10 rpm, and temperature of 30°C. The resulting prepolymer composition contains a photopolymer (photopolymer P1a) and monomer components that have not undergone polymerization (residual monomers).
[0209] (Preparation of the adhesive composition)
[0210] Next, 100 parts by weight of the prepolymer composition, 3 parts by weight of the above-mentioned acrylic oligomer, 0.6 parts by weight of the urethane acrylate oligomer (trade name "UN-350", manufactured by Negami Kogyo Co., Ltd.), 0.4 parts by weight of the photopolymerization initiator (trade name "Omnirad 819", phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, manufactured by BASF), 0.5 parts by weight of the antioxidant (trade name "Irganox 1010", manufactured by BASF), 0.2 parts by weight of the rust inhibitor (trade name "BT-120", manufactured by Jōhoku Chemical Industry Co., Ltd.), and 0.3 parts by weight of the silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Industry Co., Ltd.) were mixed to obtain the adhesive composition.
[0211] (Making the basic adhesive sheet)
[0212] Next, an adhesive composition is applied to the release-treated surface of a first release liner (trade name "Diafoil MRF", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with a release-treated surface on one side to form a coating film. Then, the release-treated surface of a second release liner (trade name "Diafoil MRE", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with a release-treated surface on one side is bonded to the coating film on the first release liner. Next, ultraviolet light is irradiated onto the coating film between the release liners from the second release liner side to photocur the coating film, thereby forming an adhesive layer with a thickness of 100 μm (UV irradiation process). During UV irradiation, a black light lamp (wavelength 320 nm–400 nm, manufactured by Toshiba Corporation) is used as the light source, and the illuminance is set to 6.5 mW / cm². 2 The cumulative irradiation intensity was set to 1500 mJ / cm. 2 In the UV irradiation process, a photopolymerization reaction is carried out in the coating film in a system containing the aforementioned residual monomer and a multifunctional compound (urethane acrylate oligomer) to form a photopolymer P1b with a photocrosslinked structure. Furthermore, this photopolymerization reaction occurs around the photopolymer P1a, thus the photopolymer P1b is formed around the photopolymer P1a. The adhesive layer formed in this process contains both the photopolymer P1a and the photopolymer P1b as a base polymer P1. A double-sided base adhesive sheet with release liner [first release liner / base adhesive sheet (100 μm thickness) / second release liner] is produced through the above operation.
[0213] (Preparation of the solution with added components)
[0214] First, 4.0 parts by weight of a multifunctional acrylate monomer (trade name "Viscoat#295", trimethylolpropane triacrylate (TMPTA), manufactured by Osaka Organic Chemicals Co., Ltd.), 0.3 parts by weight of a photopolymerization initiator (trade name "Omnirad819", manufactured by BASF), 7.0 parts by weight of a UV absorber (trade name "Tinosorb S", manufactured by BASF), and 88.7 parts by weight of ethyl acetate as a solvent were mixed to prepare a post-added component solution (the components in the solution other than the solvent are post-added components).
[0215] (Fabrication of curable optical adhesive sheets)
[0216] Next, the second release liner is peeled off from the aforementioned double-sided base adhesive sheet with release liner, and then a coating of the additive solution (coating treatment) is applied to the exposed surface of the base adhesive sheet to a thickness of 20 μm. Coating is performed using an RDS No.10 bar coater manufactured by RDSPECIALTIES. Following this, a drying process is carried out in a desiccator at 110°C for 60 seconds. Through the coating treatment and drying process, the additive components (polyfunctional acrylate monomers, photopolymerization initiator, and UV absorber) penetrate into the base adhesive sheet, and the solvent is vaporized. The base adhesive sheet is transformed into a photocurable adhesive sheet through the penetration of the additive components (photocurable adhesive sheet). Next, the release-treated surface of a third release liner (trade name "Diafoil MRE", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) with a single-sided release-treated surface is bonded to the adhesive sheet on the first release liner. Furthermore, when the above-mentioned photocurable adhesive sheet is subjected to the above-mentioned photocuring treatment, the difference ΔG(%)[G2-G1] between the gel fraction G1(%) before photocuring treatment and the gel fraction G2(%) after photocuring treatment is 5%.
[0217] The above operations were used to create an optical double-sided adhesive sheet with a release liner before shape processing [first release liner / adhesive layer / third release liner].
[0218] [External machining process]
[0219] (Low-energy process)
[0220] Next, pulsed laser light was applied along the predetermined cutting line of the aforementioned optical adhesive sheet, from the third release liner side (top side) in the thickness direction. In this process, the following laser processing apparatus was used: a Yb:YAG laser was used as the laser source (laser medium), the laser wavelength (λ) was set to 1030 nm, the pulse width was set to 2540 fs (femtoseconds), the irradiation spot diameter was set to 64 μm, the average output power P1 was set to 12 W, the pulse repetition frequency F1 was set to 150 kHz, and the scanning speed R1 was set to 170 mm / s. In this process, the pulse energy PE1 of the irradiating laser was 80 μJ, and the irradiation energy E1 was 7.06 × 10⁻⁶. 4 μJ / mm. It should be noted that the pulse energy [J] is calculated by dividing the average output power [W] by the frequency [Hz], and the irradiation energy [J / mm] is calculated by dividing the average output power [W] by the scanning speed [mm / s]. The scanning speed refers to the scanning speed of the irradiation point of the laser L relative to the workpiece film W.
[0221] (High-energy process)
[0222] Next, along the predetermined cutting line of the aforementioned optical adhesive sheet, a pulsed laser was again irradiated from the third release liner side in the thickness direction. The processing conditions in this step were set to the same as in the low-energy step, except that the scanning speed R2 was changed to 105 mm / s. That is, the pulse energy PE2 of the irradiated laser was 80 μJ, and the irradiation energy E2 was 1.14 × 10⁻⁶. 5 μJ / mm.
[0223] The optical adhesive sheet that has undergone the above process has an adhesive layer that is a rounded rectangle when viewed from above and a first peripheral portion therearound. In the third release liner, a second peripheral portion is formed on the first peripheral portion, and a groove is formed on the first release liner along the outer periphery of the first peripheral portion.
[0224] The above operations were used to shape the optical double-sided adhesive sheet with release liner [first release liner / adhesive layer / third release liner].
[0225] Example 2
[0226] Except for setting the processing conditions as described in Table 1, the same procedure as in Example 1 was followed to obtain a double-sided optical adhesive sheet with a release liner.
[0227] Comparative Examples 1 to 2
[0228] The processing conditions for the low-energy process were set as described in Table 1, and the high-energy process was not performed. Otherwise, the process was carried out in the same manner as in Example 1, and a double-sided optical adhesive sheet with a release liner was obtained.
[0229] Comparative Examples 3 to 4
[0230] Except for setting the processing conditions as described in Table 1, the same procedure as in Example 1 was followed to obtain a double-sided optical adhesive sheet with a release liner.
[0231] [evaluate]
[0232] The double-sided optical adhesive sheets with release liner produced in the examples and comparative examples were evaluated as follows, and the results are recorded in Table 1.
[0233] (1) Can the adhesive layer be cut?
[0234] In the double-sided optical adhesive sheets with release liner in the embodiments and comparative examples, the operability of removing the first and second peripheral portions from the first release liner was evaluated according to the following evaluation criteria.
[0235] <Evaluation Criteria>
[0236] ○(Good): The adhesive layer is completely cut to separate the rounded rectangular adhesive layer from its surrounding first periphery, thus enabling good removal of the first and second periphery from the first release liner.
[0237] × (Defect): The adhesive layer was not completely cut. The rounded rectangular adhesive layer was partially adhered to the first surrounding portion around it. Therefore, when the first and second surrounding portions were removed from the first release liner, the adhesive layer was stretched by the first surrounding portion, resulting in deformation and defects.
[0238] (2) Depth of the groove for the first peeling gasket
[0239] The depth of the groove formed on the first release liner in the embodiments and comparative examples was measured at a total of 10 measurement points using a shape analysis laser microscope (trade name "VK-X 1000", manufactured by KEYENCE). The measurement points were arbitrarily selected as adjacent measurement points that were approximately equally spaced in a rectangular annular groove when viewed from above. The average value of the measured groove depths was taken as the groove depth (μm) of the first release liner and evaluated according to the following evaluation criteria.
[0240] <Evaluation Criteria>
[0241] ○ (Good): The depth of the groove is less than 25μm.
[0242] × (Defective): The depth of the groove is greater than 25μm.
[0243] Table 1
[0244] According to the manufacturing method of the double-sided optical adhesive sheet with release liner according to the embodiment, the adhesive layer is fully cut, and the depth of the groove formed on the first release liner is less than 25 μm. Therefore, the adhesive layer can be cut well, and the depth of the half-cut groove is formed to an appropriate depth, resulting in excellent processing quality of the adhesive sheet after half-cutting. This is presumably because, during the low-energy process, when the laser is irradiated along the predetermined cutting line, a photocuring reaction occurs due to the multiphoton absorption of the pulsed laser, accompanied by the consumption of photopolymerization initiator and multifunctional compound. Thus, the energy of the laser irradiated in the subsequent high-energy process is efficiently used for cutting the adhesive layer. In contrast, the manufacturing method of the double-sided optical adhesive sheet with release liner according to the comparative example makes it difficult to simultaneously achieve good cutting of the adhesive layer and appropriate formation of the half-cut groove, resulting in poor processing quality of the adhesive sheet using laser. Specifically, the results were as follows: When the pulsed laser irradiation process was performed only once, as in Comparative Example 1, when the irradiation energy was too low, the depth of the semi-cut groove was appropriate, but the cutting of the adhesive layer became insufficient. As in Comparative Example 2, when the irradiation energy was too high, although the adhesive layer could be cut, the depth of the semi-cut groove was too deep. Furthermore, even when two pulsed laser irradiation processes were performed, in Comparative Examples 3 to 4, where the relationship E1 < E2 was not satisfied, neither good cutting of the adhesive layer nor proper formation of the semi-cut groove could be achieved.
[0245] The following describes various embodiments of the invention involved in this disclosure.
[0246] [Appendix 1] A method for manufacturing an adhesive sheet, wherein the method for manufacturing an adhesive sheet is a method for manufacturing a partially cut adhesive sheet, the adhesive sheet having a laminated structure in which a photocurable adhesive layer and a film layer are stacked in the thickness direction, the method for manufacturing an adhesive sheet comprising: a low-energy step, wherein a laser is irradiated from the adhesive layer side onto a curing target area of the adhesive layer to cure the curing target area; and a high-energy step, wherein a laser is irradiated from the adhesive layer side onto a cutting target area of the adhesive layer to cut the adhesive layer along the cutting target area, thereby partially cutting the adhesive sheet, wherein a portion or all of the curing target area overlaps with the cutting target area, wherein when the irradiation energy of the laser in the low-energy step is set to E1 (μJ / mm) and the irradiation energy of the laser in the high-energy step is set to E2 (μJ / mm), E1 < E2.
[0247] [Note 2] According to the manufacturing method of the adhesive sheet described in Note 1, the adhesive layer is cut by the high-energy process, and the end face of the resulting adhesive layer does not have photocurability.
[0248] [Note 3] In the method for manufacturing the adhesive sheet according to Note 1 or 2, when the scanning speed of the laser in the low-energy process is set to R1 (mm / s) and the scanning speed of the laser in the high-energy process is set to R2 (mm / s), R2 < R1.
[0249] [Appendix 4] In the method for manufacturing the adhesive sheet according to any one of Appendices 1 to 3, the ratio of the scanning speed R1 of the laser in the low-energy process to the scanning speed R2 of the laser in the high-energy process is R1:R2 = 1.5:1 to 50:1.
[0250] [Appendix 5] In the method for manufacturing the adhesive sheet according to any one of Appendices 1 to 4, the laser irradiated in the low-energy process satisfies one or more of the following: (1) or (2): (1) The laser is an ultraviolet laser; (2) The laser is a short-pulse laser.
Claims
1. A method for manufacturing an adhesive sheet, wherein the method for manufacturing the adhesive sheet is a method for manufacturing an adhesive sheet that has been partially cut. The adhesive sheet has a laminated structure in which a photocurable adhesive layer and a film layer are stacked in the thickness direction. The method for manufacturing the adhesive sheet includes: a low energy procedure, wherein A laser is irradiated onto the target area of the adhesive layer from the adhesive layer side to cure the target area. and In a high-energy process, a laser is irradiated onto a target cutting area of the adhesive layer from the adhesive layer side, cutting the adhesive layer along the target cutting area, thereby partially cutting the adhesive sheet. The solidified target area may overlap with part or all of the cut target area. When the laser irradiation energy in the low-energy process is set to E1 (μJ / mm) and the laser irradiation energy in the high-energy process is set to E2 (μJ / mm), E1 < E2.
2. The method for manufacturing the adhesive sheet according to claim 1, wherein, The adhesive layer is cut by the high-energy process, and the resulting adhesive layer has end faces that do not have photocurability.
3. The method for manufacturing the adhesive sheet according to claim 1 or 2, wherein, When the scanning speed of the laser in the low-energy process is set to R1 (mm / s) and the scanning speed of the laser in the high-energy process is set to R2 (mm / s), R2 < R1.
4. The method for manufacturing the adhesive sheet according to claim 3, wherein, The ratio of the laser scanning speed R1 in the low-energy process to the laser scanning speed R2 in the high-energy process is R1:R2 = 1.5:1 to 50:
1.
5. The method for manufacturing the adhesive sheet according to claim 1 or 2, wherein, The laser irradiated in the low-energy process satisfies one or more of the following conditions (1) or (2): (1) The laser is an ultraviolet laser; (2) The laser is a short-pulse laser.
Citation Information
Patent Citations
Acrylic adhesives and its production method
JP2002069411A
Adhesive composition, pressure sensitive adhesive double coated tape, adhesion method and portable electronic device
JP2007051271A
Manufacturing method of laminate film having adhesive layer
JP2024051400A
Method for manufacturing laminate film having adhesive layer
JP2024143048A