Tantalum and zirconium dissimilar metal pipe fitting plug welding joint and electron beam fusion brazing method thereof

By employing electron beam brazing, utilizing a plug-in mating structure and preheating treatment, the welding difficulties of tantalum-zirconium dissimilar metal connections were solved, achieving a metallurgical bond free of porosity and cracks, thus meeting the sealing and load-bearing requirements of the nuclear industry and aerospace fields.

CN123149647APending Publication Date: 2026-11-24BEIJING ATOMIC ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611362864.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The joining of dissimilar metals tantalum and zirconium is difficult due to their large difference in melting point, active chemical properties, and poor wettability of molten zirconium to solid tantalum. Existing joining methods are insufficient to meet the sealing performance and load-bearing capacity requirements of the nuclear industry and aerospace.

Method used

Electron beam brazing is employed, using a plug-in mating structure and preheating treatment. The electron beam is biased towards the low-melting-point base material to locally melt it, forming a metallurgical bond. This avoids large heat input, increases the bonding area, reduces residual stress, and achieves a connection without pores or cracks.

Benefits of technology

It achieves an increased metallurgical bonding area for tantalum-zirconium dissimilar metal connections, excellent joint sealing performance, reduced joint stress concentration, meets the requirements of nuclear industry and aerospace fields, and requires no brazing filler metal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149647A_ABST
    Figure CN123149647A_ABST
Patent Text Reader

Abstract

This invention discloses a plug-in welded joint for tantalum and zirconium dissimilar metal pipes and its electron beam brazing method, belonging to the field of dissimilar refractory metal joining technology. The joint includes a tantalum tube and a zirconium tube. The welding end of the tantalum tube is inserted into the welding end of the zirconium tube to form a plug-in mating area. The insertion depth is 6–10 mm, and the radial mating clearance is 0.01–0.05 mm. The plug-in mating area is then brazed with an electron beam to form a metallurgical bond. The method includes: after joint preparation and pre-welding cleaning, the workpiece is coaxially clamped in a vacuum chamber. The welding area of ​​the tantalum tube is preheated to 600–800°C using a defocused electron beam. Then, the center of the electron beam spot is offset 0.2–0.5 mm relative to the mating interface towards the zirconium tube side for brazing, causing the zirconium side to partially melt while the tantalum side remains solid. The molten zirconium wets, spreads, and forms a metallurgical bond on the solid tantalum surface. This invention eliminates the need for solder, and preheating before soldering improves the wettability of molten zirconium to tantalum and reduces residual stress at the joint. No stable intermetallic compounds are formed in the tantalum-zirconium system, resulting in a joint free of porosity and cracks. Helium mass spectrometry leak detection yields a rate better than 5 × 10⁻⁶. ‑10 Pa·m 3 / s, suitable for connecting tantalum-zirconium dissimilar metal pipe fittings in the nuclear industry and aerospace field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of dissimilar refractory metal joining technology, specifically relating to a tantalum and zirconium dissimilar metal pipe fitting plug-in welding joint and its electron beam fusion brazing method, which is applicable to the metallurgical connection between tantalum and tantalum alloys and zirconium and zirconium alloy pipe fittings in the nuclear industry, aerospace and other fields. Background Technology

[0002] Tantalum (Ta) has a high melting point of 3017℃ and possesses excellent high-temperature strength, superior corrosion resistance (especially against inorganic acids and liquid metal corrosion), and good plasticity and processing properties, making it a key refractory metal material in aerospace, chemical, and high-temperature equipment. Zirconium (Zr) has a melting point of 1852℃, a small thermal neutron absorption cross section, excellent resistance to high temperature and pressure, and excellent water corrosion resistance, making it a key structural material for nuclear reactors. In the nuclear industry and aerospace equipment, it is often necessary to connect tantalum or tantalum alloy tubing with zirconium or zirconium alloy tubing, such as the connection between tantalum alloy components and zirconium alloy piping and cladding in space nuclear power sources, as well as dissimilar metal transition joints outside the reactor core.

[0003] However, tantalum and zirconium have melting points that differ by about 1165°C. The large heat input required for tantalum to fully melt during direct fusion welding can lead to severe overheating, grain coarsening, or even evaporation and burn-off on the zirconium side. Conversely, reducing the heat input can result in incomplete fusion on the tantalum side. Both tantalum and zirconium are highly reactive metals that readily react with oxygen, nitrogen, and hydrogen at high temperatures, causing them to become embrittled. This places extremely high demands on the welding protection environment. Molten zirconium has poor wettability on the surface of solid tantalum at room temperature, and the two metals also have different thermophysical properties. During the welding heating and cooling process, the joint experiences a large temperature gradient and high residual stress, making it prone to cracking.

[0004] In existing connection methods: brazing joints require the introduction of dissimilar filler metals, and the temperature resistance, compatibility with the base material, and radiation resistance of the filler metals are difficult to simultaneously meet the application requirements; diffusion welding joints require overall heating and pressurization of the welded parts, which is difficult to implement for closed structures such as pipe fittings. Regarding joint structure, simple butt joints exhibit abrupt changes in cross-section when the wall thicknesses of the two pipe fittings differ, resulting in high stress concentration at the joint; furthermore, the metallurgical bonding area of ​​the butt joint is limited to the annular cross-section of the pipe wall, resulting in a small bonding area and limiting the sealing length and load-bearing capacity of the joint.

[0005] Electron beam brazing utilizes the high energy density and precise controllable beam position and energy of electron beams. The electron beam is deflected towards the low-melting-point base material, causing localized melting. The molten metal then wets, spreads, and diffuses on the surface of the high-melting-point base material, forming a metallurgical bond. In essence, the low-melting-point side is fusion welded, and the high-melting-point side is brazed. This method is an effective way to join dissimilar metals with significant differences in physicochemical properties. Furthermore, the tantalum-zirconium binary phase diagram shows that tantalum and zirconium form a continuous solid solution at high temperatures, with no stable intermetallic compounds forming. Their good metallurgical compatibility provides a favorable metallurgical basis for tantalum-zirconium brazing. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the present invention aims to provide a plug-in welded joint for tantalum and zirconium dissimilar metal pipe fittings and its electron beam brazing method. This method increases the metallurgical bonding area and sealing length of the tantalum-zirconium dissimilar metal pipe fittings, reduces stress concentration at the joint, and solves the welding difficulties caused by the large difference in melting points between tantalum and zirconium, their active chemical properties, and the poor wettability of molten zirconium to solid tantalum. It can obtain a tantalum-zirconium dissimilar metal joint with excellent sealing performance without the need for brazing filler metal, and is free of porosity and cracks.

[0007] On one hand, this invention provides a plug-in welded joint for tantalum and zirconium dissimilar metal tubing, comprising a tantalum tube and a zirconium tube. The welded end of the tantalum tube is inserted into the welded end of the zirconium tube to form a plug-in mating area. The insertion depth of the tantalum tube is 6–10 mm, and the radial mating clearance of the plug-in mating area is 0.01–0.05 mm. The tantalum tube and the zirconium tube are metallurgically bonded at the plug-in mating area by electron beam brazing. Further, the inner hole of the welded end of the zirconium tube is enlarged to form a plug hole, and the welded end of the tantalum tube is directly inserted into the plug hole. The outer diameter of the tantalum tube is 5–10 mm, and the wall thickness is 0.5–2 mm. The outer diameter of the zirconium tube is 6–12 mm, and the wall thickness is 1–2 mm. The inner diameters of the tantalum tube and the zirconium tube are equal. An annular brazing weld is formed on the outer side of the plug-in mating area.

[0008] On the other hand, the present invention provides an electron beam brazing method for the above-mentioned plug-in welded joint, comprising the following steps: (1) Joint preparation: the welding ends of tantalum tube and zirconium tube are processed into plug-in joints, and the inner hole of the welding end of zirconium tube is enlarged to form a plug hole; (2) Pre-welding cleaning: the mating surfaces are degreased, pickled, cleaned and dried; (3) Assembly and positioning: the welding end of tantalum tube is inserted into the plug hole and coaxially clamped on the rotary table in the vacuum chamber; (4) Electron beam preheating: the vacuum chamber is evacuated to the working vacuum level, and the welding area of ​​tantalum tube is preheated by a defocused electron beam at a preheating temperature of 600-800℃; (5) Electron beam brazing: the electron beam is incident radially from the outside of the plug-in mating area, and the beam spot center is offset by 0.2-0.5mm relative to the mating interface to the zirconium tube side. The accelerating voltage, welding beam current and workpiece rotation speed are controlled so that the zirconium tube side is partially melted while the tantalum side remains solid. The molten zirconium wets and spreads on the solid tantalum surface and forms a metallurgical bond with tantalum. The workpiece rotates once to complete the circumferential weld.

[0009] The working principle of this invention is as follows: the melting point of zirconium (1852℃) is about 1165℃ lower than that of tantalum (3017℃). Before welding, the welding area of ​​the tantalum tube is preheated to 600-800℃ using a defocused electron beam. On the one hand, the increased temperature significantly reduces the contact angle between molten zirconium and solid tantalum, improving the wetting and spreading ability of molten zirconium on the tantalum surface. On the other hand, preheating reduces the temperature gradient of the joint during the welding heating and cooling process, reducing residual stress and preventing crack formation. Preheating also degassing and purifying the tantalum surface. During welding, the center of the electron beam spot is shifted 0.2-0.5mm towards the zirconium tube side. The electron beam energy mainly acts on the zirconium side, causing local melting of the zirconium to form a molten pool. Driven by interfacial tension and capillary action, the molten zirconium wets and spreads on the mating surface of the solid tantalum. Zirconium atoms and tantalum atoms diffuse into each other at the interface, forming a metallurgical bond. Since the tantalum side does not melt, the large heat input required for melting high-melting-point tantalum and the resulting overheating and evaporation problems on the zirconium side are avoided; at the same time, the tantalum-zirconium system does not generate stable intermetallic compounds, and a solid solution bonding layer is formed at the interface, resulting in good joint ductility and toughness.

[0010] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The plug-in mating structure expands the tantalum-zirconium mating surface from the annular cross section of the tube wall to the cylindrical mating surface of the insert section, which significantly increases the metallurgical mating area. The insertion depth of 6-10 mm ensures the sealing length and load-bearing capacity of the joint; (2) The radial mating gap of 0.01-0.05 mm is conducive to the capillary filling of molten zirconium between the mating surfaces, forming a continuous and dense mating layer. The joint is free of pores and cracks, and the leak detection rate by helium mass spectrometry is better than 5×10. - 10 Pa·m 3 / s; (3) Tantalum tube and zirconium tube are straight tubes with equal inner diameters, and the flow channel inside the joint is smooth and continuous without abrupt changes in cross section, and no additional flow resistance is introduced; and the joint structure is simple, easy to process and assemble, and the coaxiality of the insertion is easy to ensure; (4) Electron beam preheating of tantalum before welding significantly improves the wettability of molten zirconium to solid tantalum and reduces the joint temperature gradient and residual stress; (5) Preheating and welding are completed continuously in the same vacuum chamber by the same electron beam equipment, the process is compact and efficient, and the vacuum environment avoids the pollution of active metals by oxygen, nitrogen and hydrogen; (6) No heterogeneous brazing filler is required, no stable intermetallic compounds are generated in the tantalum-zirconium system, the joint interface is not easy to become brittle, and it can meet the usage requirements of pipe connection in the nuclear industry and aerospace field. Attached Figure Description

[0011] Figure 1 This is a schematic diagram of the structure of the plug-in welding joint for tantalum and zirconium dissimilar metal pipe fittings of the present invention; Figure 2 This is an X-ray (RT) photograph of the tantalum-zirconium plug-in welded joint of Embodiment 1 of the present invention. In the figure: 1 is the tantalum tube, 2 is the zirconium tube, and 3 is the annular brazing weld (electron beam welding position). Detailed Implementation

[0012] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the following embodiments are only for illustrating the present invention and not for limiting the scope of protection of the present invention. Equivalent substitutions and improvements made by those skilled in the art under the concept of the present invention should all fall within the scope of protection of the present invention.

[0013] Example 1: As Figure 1 As shown, the tantalum and zirconium dissimilar metal tubular plug-in weld joint in this embodiment includes a pure tantalum tube and a pure zirconium tube. The tantalum tube has an outer diameter of 8mm and an inner diameter of 6mm (wall thickness of 1mm), while the zirconium tube has an outer diameter of 10mm and an inner diameter of 6mm (wall thickness of 2mm). The inner diameters of the two tubes are equal. The inner hole of the zirconium tube welding end is enlarged to 8.04mm to form a plug hole. The welding end of the tantalum tube is directly inserted into the plug hole of the zirconium tube to a depth of 10mm, and the radial fit clearance of the plug-in mating area is 0.02mm.

[0014] The fabrication process of the joint in this embodiment is as follows: the mating surfaces are sequentially degreased with acetone using ultrasonication, then pickled with a mixed hydrofluoric acid-nitric acid pickling solution (by volume fraction: 45% nitric acid, 4% hydrofluoric acid, and the remainder being water), rinsed with deionized water, dehydrated with anhydrous ethanol, and dried; after assembly, the two tubes are coaxial and clamped on the rotary table of the vacuum chamber. The vacuum chamber is evacuated to 4×10⁻⁶. -3 Pa; First, the tantalum tube welding area is preheated with a defocused electron beam at a preheating current of 6mA to preheat the tantalum side to 700℃; then welding is performed: accelerating voltage 60kV, welding beam current 10mA, electron beam surface focusing, beam spot center offset 0.3mm relative to the mating interface towards the zirconium tube side, workpiece rotation speed 10r / min, complete the circumferential weld in one rotation, and set beam current slow rise and slow fall control at the start and end lap joint of the weld.

[0015] The welded joint surface has a continuous and uniform shape; X-ray (RT) inspection of the welded joint yielded the following results: Figure 2 As shown, there are no pores, cracks, or lack of fusion defects inside the weld; helium mass spectrometry leak detection shows that the joint leakage rate is better than 5×10⁻⁶. -10 Pa·m 3 / s, the sealing performance meets the usage requirements.

[0016] Table 1. Joint structure and welding process parameters for Example 1

[0017] Process parameters Value Tantalum tube / Zirconium tube specifications Pure tantalum Φ8mm×Φ6mm / Pure zirconium Φ10mm×Φ6mm Insertion hole size (enlarged hole at the welding end of the zirconium tube) Φ8.04mm Insertion depth / radial clearance 10mm / 0.02mm Preheating method / Preheating temperature Defocused electron beam, 6mA / 700℃ Accelerating voltage / welding beam current 60kV / 10mA Workpiece rotation speed 10r / min Beam spot offset (biased towards the zircon side) 0.3mm Focusing Method Surface Focusing Working vacuum <![CDATA[4×10 -3 Well]]> Helium mass spectrometry leak detection rate <![CDATA[better than 5×10 -10 Pa·m 3 / s]]>

[0018] Example 2: As Figure 1As shown, the tantalum and zirconium dissimilar metal tubular plug-in weld joint in this embodiment includes a Ta-W alloy tube and a Zr-Nb alloy tube. The tantalum alloy tube has an outer diameter of 6 mm and an inner diameter of 4 mm (wall thickness of 1 mm), while the zirconium alloy tube has an outer diameter of 8 mm and an inner diameter of 4 mm (wall thickness of 2 mm). The inner diameters of the two tubes are equal. The inner hole of the welding end of the zirconium alloy tube is enlarged to 6.02 mm to form a plug hole. The welding end of the tantalum alloy tube is directly inserted into the plug hole of the zirconium alloy tube to a depth of 8 mm, and the radial fit clearance of the plug-in mating area is 0.01 mm.

[0019] The fabrication process of the connector in this embodiment is basically the same as that in Embodiment 1, except that the working vacuum degree of the vacuum chamber is 5×10⁻⁶. -3 Pa; tantalum side preheating temperature 600℃; welding beam current 6mA, beam spot center offset 0.2mm towards the zirconium alloy tube side. Post-weld joint formation was good; X-ray inspection showed no defects such as porosity or cracks; metallographic observation showed continuous bonding between the zirconium side molten pool and the tantalum side interface, forming a metallurgical bonding layer at the interface without the formation of brittle intermetallic compounds; helium mass spectrometry leak detection showed a joint leak rate better than 5×10⁻⁶. -10 Pa·m 3 / s.

[0020] Table 2 Joint structure and welding process parameters for Example 2

[0021] Process parameters Value Tantalum tube / Zirconium tube specifications Ta-W Φ6mm×Φ4mmZr-Nb Φ8mm×Φ4mm Insertion hole size (enlarged hole at the welding end of the zirconium tube) Φ6.02mm Insertion depth / radial clearance 8mm / 0.01mm Preheating method / Preheating temperature Defocused electron beam / 600℃ Accelerating voltage / welding beam current 60kV / 6mA Workpiece rotation speed 10r / min Beam spot offset (biased towards the zircon side) 0.2mm Focusing Method Surface Focusing Working vacuum <![CDATA[5×10 -3 Well]]> Helium mass spectrometry leak detection rate <![CDATA[better than 5×10 -10 Pa·m 3 / s]]>

[0022] Example 3: The plug-in welded joint in this example includes a pure tantalum tube and a pure zirconium tube. The tantalum tube has an outer diameter of 10 mm and an inner diameter of 8 mm (wall thickness of 1 mm), while the zirconium tube has an outer diameter of 12 mm and an inner diameter of 8 mm (wall thickness of 2 mm). The inner diameters of the two tubes are equal. The inner hole of the zirconium tube welding end is enlarged to 10.08 mm to form a plug hole. The welding end of the tantalum tube is inserted into the plug hole to a depth of 10 mm, with a radial fit clearance of 0.04 mm. The preparation process is basically the same as in Example 1, except that: the preheating temperature on the tantalum side is 800℃; the welding beam current is 12 mA, the workpiece rotation speed is 8 r / min, and the beam spot center is offset by 0.5 mm towards the zirconium tube side; during the welding process, a circular scan of the electron beam is applied with a scanning frequency of 500 Hz and a scanning amplitude of 0.5 mm to improve the wetting and spreading of molten zirconium on the tantalum mating surface; after welding, the workpiece is heated to 800℃ in a vacuum furnace and held for 30 min, followed by furnace cooling to eliminate residual stress in the joint. The residual stress of the weld joint was significantly reduced after welding, and the leak rate of the joint was better than 5×10⁻⁶ after helium mass spectrometry leak detection. -10 Pa·m 3 / s.

[0023] Table 3 Joint structure and welding process parameters for Example 3

[0024] Process parameters Value Tantalum tube / Zirconium tube specifications Pure tantalum Φ10mm×Φ8mm / Pure zirconium Φ12mm×Φ8mm Insertion hole size (enlarged hole at the welding end of the zirconium tube) Φ10.08mm Insertion depth / radial clearance 10mm / 0.04mm Preheating method / Preheating temperature Defocused electron beam / 800℃ Accelerating voltage / welding beam current 60kV / 12mA Workpiece rotation speed 8r / min Beam spot offset (biased towards the zircon side) 0.5mm Electron beam scanning Circular, 500Hz, amplitude 0.5mm Post-weld heat treatment Vacuum at 800℃ for 30 minutes, followed by furnace cooling. Helium mass spectrometry leak detection rate <![CDATA[better than 5×10 -10 Pa·m 3 / s]]>

Claims

1. A plug-in welded joint for tantalum and zirconium dissimilar metal pipe fittings, characterized in that: The device includes a tantalum tube (1) and a zirconium tube (2). The welding end of the tantalum tube is inserted into the welding end of the zirconium tube to form a mating area. The insertion depth of the tantalum tube is 6 to 10 mm, and the radial mating gap of the mating area is 0.01 to 0.05 mm. The tantalum tube and the zirconium tube are metallurgically bonded at the mating area by electron beam brazing.

2. The tantalum and zirconium dissimilar metal pipe fitting plug-in welding joint according to claim 1, characterized in that: The inner hole of the welded end of the zirconium tube is enlarged to form an insertion hole, and the welded end of the tantalum tube is inserted into the insertion hole.

3. The tantalum and zirconium dissimilar metal pipe fitting plug-in welding joint according to claim 1, characterized in that: The tantalum tube has an outer diameter of 5–10 mm and a wall thickness of 0.5–2 mm; the zirconium tube has an outer diameter of 6–12 mm and a wall thickness of 1–2 mm.

4. The tantalum and zirconium dissimilar metal pipe fitting plug-in welding joint according to claim 1, characterized in that: The inner diameters of the tantalum tube and the zirconium tube are equal; an annular brazing weld (3) is formed on the outer side of the insertion mating area.

5. The tantalum and zirconium dissimilar metal pipe fitting plug-in welding joint according to claim 1, characterized in that: The tantalum tube is a pure tantalum tube or a tantalum alloy tube, and the tantalum alloy is a Ta-W alloy; the zirconium tube is a pure zirconium tube or a zirconium alloy tube, and the zirconium alloy is a Zr-2 alloy, a Zr-4 alloy, or a Zr-Nb alloy.

6. An electron beam brazing method for the plug-in welded joint of tantalum and zirconium dissimilar metal pipe fittings as described in any one of claims 1 to 5, characterized in that, The process includes the following steps: (1) Joint preparation: The welding ends of the tantalum tube and the zirconium tube are processed into plug-in joints, and the inner hole of the welding end of the zirconium tube is enlarged to form a plug hole; (2) Pre-welding cleaning: The mating surfaces of the tantalum tube and the zirconium tube are degreased, pickled, cleaned and dried; (3) Assembly and positioning: The welding end of the tantalum tube is inserted into the plug hole and coaxially clamped on the rotary table in the vacuum chamber; (4) Electron beam preheating: The vacuum chamber is evacuated to the working vacuum level, and a defocused electron beam is used to preheat the tantalum tube. The welding area is preheated at a temperature of 600-800℃; (5) Electron beam brazing: The electron beam is incident radially from the outside of the insertion mating area. The center of the electron beam spot is offset by 0.2-0.5mm relative to the mating interface of the insertion mating area to one side of the zirconium tube. The accelerating voltage, welding beam current and workpiece rotation speed are controlled so that one side of the zirconium tube is partially melted while the other side of the tantalum tube remains solid. The molten zirconium wets and spreads on the surface of the solid tantalum and forms a metallurgical bond with the tantalum. The workpiece completes the welding of the annular weld by rotating the rotary table once.

7. The electron beam brazing method according to claim 6, characterized in that, The pickling in step (2) uses a mixed pickling solution of hydrofluoric acid and nitric acid. The pickling solution is composed of 40% to 50% nitric acid, 3% to 5% hydrofluoric acid, and the remainder is water by volume. After pickling, the solution is rinsed with deionized water, then dehydrated with anhydrous ethanol and dried.

8. The electron beam brazing method according to claim 6, characterized in that, The working vacuum degree mentioned in step (4) is better than 5×10 -3 Pa; the preheating adopts a defocused electron beam or a scanning electron beam, the preheating beam current is 5-10mA, and the preheating time is 10-60s.

9. The electron beam brazing method according to claim 6, characterized in that, The accelerating voltage in step (5) is 60-150kV, the welding beam current is 8-15mA, the workpiece rotation speed is 5-15r / min, and the electron beam is surface focused.

10. The electron beam brazing method according to claim 6, characterized in that, In step (5), the electron beam is scanned during the welding process. The scanning waveform is a circular waveform or a straight waveform. The scanning frequency is 50 to 500 Hz and the scanning amplitude is 0.3 to 1.0 mm.

11. The electron beam brazing method according to claim 6, characterized in that, It also includes step (6) post-weld heat treatment: the welded workpiece is heated to 650-850℃ under vacuum conditions and held for 20-60 minutes, and then cooled with the furnace to eliminate residual stress in the joint.