Iron-based amorphous flux cored wire for austenitic weld surface and method of making the same
By using arc welding technology with iron-based amorphous flux-cored welding wire on the surface of austenitic welds, a high-hardness and corrosion-resistant amorphous coating is formed, which solves the wear and corrosion problems of austenitic welds in high-temperature environments and achieves efficient strengthening and repair of welds.
Patent Information
- Application Number
- CN202611110613.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-24
- Publication Date
- 2026-11-24
AI Technical Summary
Austenitic welds are prone to failure in boiler piping systems of thermal power units due to high temperature, high pressure and corrosion wear. Traditional crystalline material coatings are difficult to achieve both high hardness and corrosion resistance, and their processing brittleness limits their application.
Using iron-based amorphous flux-cored welding wire, an amorphous structure is formed on the surface of the austenitic weld through arc welding technology. The synergistic effect of elements such as molybdenum, chromium, carbon, boron, and silicon is utilized to form a high-hardness, corrosion-resistant amorphous coating.
It significantly improves the hardness and corrosion resistance of austenitic welds, extends the service life of welds, solves the problems of wear and corrosion failure, and is suitable for efficient on-site reinforcement and repair of boiler pipelines in thermal power units.
Smart Images

Figure CN123149648A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the technical field of metallic materials, and in particular to iron-based amorphous flux-cored welding wire for use on the surface of austenitic welds and its preparation method. Background Technology
[0002] In boiler piping systems of thermal power units, austenitic stainless steel welds are widely used due to their excellent high-temperature performance. However, the operating environment is extremely harsh, with the welded areas subjected to high temperatures, high pressures, and severe erosion and corrosion from flue gas and fly ash over long periods. Under these conditions, traditional austenitic welds have low surface hardness and insufficient wear resistance, making them prone to becoming weak points in the entire piping system. This leads to premature failure of the welded area, threatening not only the safe and stable operation of the unit but also increasing the cost of frequent shutdowns for maintenance.
[0003] Currently, although various surface strengthening technologies can be used to improve weld performance, coatings prepared from traditional crystalline materials often struggle to balance high hardness and excellent corrosion resistance. Furthermore, under thermal cycling, coarse grain boundaries can easily become pathways for corrosion and wear. Iron-based amorphous alloys, due to their long-range disordered atomic structure and the absence of crystalline defects such as grain boundaries, exhibit high strength, high hardness, and excellent corrosion and wear resistance, perfectly addressing these challenges. However, the inherent size limitations and processing brittleness of iron-based amorphous materials restrict their direct application as integral structural components. Arc welding technology offers an ideal solution to this problem. It can efficiently prepare alloys with amorphous forming capabilities as coatings on the surface of austenitic welds, bypassing complex processing difficulties and significantly reducing manufacturing costs. This opens up new technical avenues for preparing high-performance protective coatings for boiler pipes and significantly extending the service life of critical components.
[0004] Therefore, there is an urgent need in this field to develop a solution that can effectively address the problem of erosion failure of austenitic steel welds during long-term high-temperature service. Summary of the Invention
[0005] This application proposes an iron-based amorphous flux-cored welding wire for use on the surface of austenitic welds and a method for preparing the same, in order to overcome the deficiencies of the prior art.
[0006] According to a first aspect of the embodiments of this application, an iron-based amorphous flux-cored welding wire for the surface of austenitic welds is provided, comprising flux powder and a welding sheath encapsulating the flux powder. The powder is composed of the following components in weight percentage: 40.0% to 45.0% molybdenum, 30.0% to 35.0% chromium, 5.0% to 7.0% carbon, 6.0% to 8.0% boron, 1.0% to 2.0% silicon, and the remainder being iron; The sum of the mass percentages of all components is 100%.
[0007] In some embodiments, the purity of the alloy powder composed of each component in the powder is not less than 99.9%.
[0008] In some embodiments, the particle size of each component in the powder is between 100 mesh and 200 mesh.
[0009] In some embodiments, the weld bead is a steel strip with a thickness of 0.4 mm and a width of 7 mm.
[0010] In some embodiments, the filler content of the flux-cored wire, which is composed of flux powder wrapped by the solder sheet, is 20% to 25%.
[0011] According to a second aspect of this application, a method for preparing an iron-based amorphous flux-cored welding wire for austenitic weld surfaces as described above is provided, comprising: The ingredients of the powder are weighed according to the following mass percentages: 40.0% to 45.0% molybdenum, 30.0% to 35.0% chromium, 5.0% to 7.0% carbon, 6.0% to 8.0% boron, 1.0% to 2.0% silicon, and the remainder is iron. The sum of the mass percentages of each ingredient is 100%. The powder is placed in a vacuum furnace and heated to dry it, which is used to remove the water of crystallization from the powder. The heated and dried medicinal powder is mixed in a powder mixer. Alcohol is used to remove grease from the surface of the steel strip, and the mixed powder is wrapped inside the steel strip using a flux-cored wire drawing device, and then the first drawing is performed through a first drawing die. After the first drawing process, the die aperture is gradually reduced until the diameter of the flux-cored wire meets the target value. The flux-cored wire is wound onto a wire spool and sealed in a vacuum packaging bag to generate the iron-based amorphous flux-cored wire for the austenitic weld surface.
[0012] In some embodiments, the step of placing the medicinal powder in a vacuum heating furnace for heating and drying includes: The powder is heated and dried in a vacuum furnace at a temperature of 200°C to 240°C and a holding time of 1 hour to 4 hours.
[0013] In some embodiments, mixing the heated and dried medicinal powder in a powder mixer includes: The heated and dried medicinal powder is mixed in a powder mixer, with a mixing time of 1 to 4 hours.
[0014] In some embodiments, the steel strip is 430 stainless steel, the orifice of the first drawing die is 2.6 mm, and the target value is 1.0 mm to 1.2 mm.
[0015] In some embodiments, the method further includes: Based on the conditions of welding current of 180A to 220A, welding voltage of 15V to 26V, and configuration of shielding gas, the iron-based amorphous flux-cored wire for the surface of austenitic weld is surfacing. The shielding gas consists of argon and helium in a volume ratio of 4:1. The thickness of the surfacing is 1.8 mm to 2 mm, and the overlap rate of the surfacing weld is 20% to 30%.
[0016] The beneficial effects of the iron-based amorphous flux-cored welding wire for austenitic weld surfaces and its preparation method according to the embodiments of this application include at least the following: This application's embodiments, through the synergistic design of key elements such as molybdenum, chromium, boron, and carbon, facilitate the formation of an amorphous structure in the flux-cored welding wire under the rapid cooling conditions of arc welding, laying the foundation for excellent hardness, corrosion resistance, and high-temperature erosion resistance of the weld layer. By employing a flux-cored welding wire structure, the precision alloy components are cleverly encapsulated in powder form within a metal outer sheath, overcoming the difficulties and high costs associated with the preparation of integral amorphous alloys, while ensuring good metallurgical compatibility with austenitic substrates. The weld layer obtained by the amorphous flux-cored welding wire of this application's embodiments exhibits high hardness and good high-temperature erosion resistance, solving the problems of wear and corrosion failure in austenitic steel welds during long-term high-temperature service. Attached Figure Description
[0017] Figure 1 This is a schematic flowchart of a preparation method according to an embodiment of this application; Figure 2 This is a diagram illustrating the macroscopic morphology of the weld overlay obtained by overlaying iron-based amorphous flux-cored wire for austenitic weld surfaces onto an austenitic steel plate, based on Example 2 of this application. Figure 3 This is a diagram illustrating the surface morphology of the weld overlay obtained by overlaying iron-based amorphous flux-cored wire for austenitic weld surfaces prepared in Example 2 onto an austenitic steel plate after a high-temperature erosion test at 610°C (10 min). Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the various embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. However, those skilled in the art will understand that many technical details have been provided in the various embodiments of this disclosure to facilitate a better understanding of the disclosure. However, the technical solutions claimed in this disclosure can be implemented even without these technical details and with various variations and modifications based on the following embodiments. The division of the various embodiments below is for ease of description and should not constitute any limitation on the specific implementation of this disclosure. The various embodiments can be combined with and referenced by each other without contradiction.
[0019] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the claimed embodiments of the present application, but merely to illustrate selected embodiments of the present application. Other embodiments obtained by those skilled in the art based on the embodiments of the present application without inventive effort are all within the scope of protection of the embodiments of the present application.
[0020] This application discloses an iron-based amorphous flux-cored wire for use on the surface of austenitic welds and its preparation method. Preferably, the iron-based amorphous flux-cored wire for use on the surface of austenitic welds is prepared based on this preparation method, with the aim of forming a weld overlay layer on the surface of austenitic stainless steel welds using arc welding technology, effectively solving the problem of erosion and corrosion failure of austenitic steel welds during long-term high-temperature service.
[0021] The iron-based amorphous flux-cored wire for use on the surface of austenitic welds includes flux powder and a coating that encapsulates the flux powder.
[0022] For example, the powder is composed of the following components by mass percentage: 40.0% to 45.0% molybdenum (Mo), 30.0% to 35.0% chromium (Cr), 5.0% to 7.0% carbon (C), 6.0% to 8.0% boron (B), 1.0% to 2.0% silicon (Si), and the remainder iron (Fe); wherein the sum of the mass percentages of each component is 100%.
[0023] In this embodiment, iron, as the matrix element of the amorphous welding wire, constitutes the framework of the weld overlay alloy. Its main function is to provide the substrate for the formation of the amorphous phase, and through the synergistic effect with other alloying elements (especially Mo, Cr, and B), it achieves high glass-forming ability (GFA), thereby suppressing the precipitation of crystalline phases under rapid cooling and obtaining a microstructure dominated by amorphous phases. This is the structural basis for the weld overlay to achieve excellent comprehensive performance. Secondly, molybdenum plays a crucial multiple roles in the system of this embodiment. First, as an important amorphous forming element, its large atomic size effectively increases the viscosity and supercooled liquid phase width of the weld overlay alloy, significantly improving the amorphous forming ability and enhancing its thermal stability. Furthermore, molybdenum dissolved in the amorphous matrix greatly enhances the microhardness and high-temperature strength of the weld overlay, and by forming a molybdenum-rich passivation film, significantly enhances the pitting corrosion resistance of the weld overlay in harsh environments (such as chloride-containing media). Chromium is the core element that imparts excellent corrosion resistance to the weld overlay. Uniformly distributed within the amorphous matrix, it preferentially reacts with oxygen to form a dense, highly adhesive Cr2O3 passivation film on the surface of the weld overlay. This protective film effectively blocks the intrusion of corrosive media, thereby greatly enhancing the weld overlay's resistance to uniform corrosion and pitting corrosion in oxidizing and neutral media. This is crucial for the high-temperature oxidation and flue gas corrosion environments faced by boiler pipes in thermal power units. Carbon is one of the key elements for improving the hardness and wear resistance of the weld overlay. It can form high-hardness carbides with metallic elements such as Cr, Mo, and Fe in the system. These fine carbide particles are dispersed in the amorphous matrix, effectively hindering plastic deformation and material loss during abrasive wear. Simultaneously, the addition of carbon helps to expand the amorphous formation range of the alloy and increase the amorphous content of the weld overlay. Boron is the most critical metalloid element in the amorphous welding wire of this application embodiment, playing a decisive role in the formation of amorphous materials. The significant atomic size difference between its small atomic size and that of large metal atoms such as iron (Fe) effectively hinders the long-range diffusion and ordered arrangement of metal atoms during rapid solidification, thus strongly suppressing crystal nucleation and growth, a necessary condition for obtaining high amorphous content. Simultaneously, the addition of boron significantly improves the hardness and wear resistance of the weld overlay. Silicon primarily functions as an auxiliary metalloid element and process modifier in the system. It works synergistically with boron to further enhance the alloy's amorphous forming ability and thermal stability. Furthermore, silicon effectively deoxidizes during welding, reducing porosity and inclusion defects in the weld overlay, and appropriately lowers the alloy's melting point, improving the fluidity and wettability of the molten metal, thereby obtaining a well-formed, dense weld overlay.
[0024] Preferably, the purity of the alloy powder composed of each component in the powder is not less than 99.9%.
[0025] Preferably, the particle size of each component in the powder is between 100 mesh and 200 mesh.
[0026] Preferably, the weld bead is a steel strip (preferably 430 stainless steel strip), the steel strip has a thickness of 0.4 mm and a width of 7 mm.
[0027] Preferably, the filling rate of the flux-cored wire composed of the flux powder wrapped by the welding skin is 20% to 25%.
[0028] This application's embodiments, through the synergistic design of key elements such as molybdenum, chromium, boron, and carbon, facilitate the formation of an amorphous structure in the flux-cored welding wire under the rapid cooling conditions of arc welding, laying the foundation for excellent hardness, corrosion resistance, and high-temperature erosion resistance of the weld layer. By employing a flux-cored welding wire structure, the precision alloy components are cleverly encapsulated in powder form within a metal outer sheath, overcoming the difficulties and high costs associated with the preparation of integral amorphous alloys, while ensuring good metallurgical compatibility with austenitic substrates. The weld layer obtained by the amorphous flux-cored welding wire of this application's embodiments exhibits high hardness and good high-temperature erosion resistance, solving the problems of wear and corrosion failure in austenitic steel welds during long-term high-temperature service.
[0029] See attached document Figure 1 As shown, a preparation method is illustrated for preparing the above-mentioned iron-based amorphous flux-cored welding wire for austenitic weld surfaces, comprising the following steps 110-160.
[0030] Step 110: Weigh the components of the powder by mass percentage, which include 40.0% to 45.0% molybdenum, 30.0% to 35.0% chromium, 5.0% to 7.0% carbon, 6.0% to 8.0% boron, 1.0% to 2.0% silicon, and the remainder is iron, with the sum of the mass percentages of each component being 100%.
[0031] Step 120: Place the powder in a vacuum furnace and heat it to dry it, in order to remove the water of crystallization from the powder.
[0032] In some embodiments, the powder is placed in a vacuum furnace for heating and drying, including: placing the powder in a vacuum furnace for heating and drying based on a heating temperature of 200°C to 240°C and a holding time of 1 hour to 4 hours.
[0033] Step 130: The heated and dried powder is mixed in a powder mixer.
[0034] In some embodiments, the heating and drying of the drug powder is mixed in a powder mixer, including: mixing the heating and drying of the drug powder in a powder mixer based on a mixing time of 1 hour to 4 hours.
[0035] Step 140: Use alcohol to remove grease from the surface of the steel strip, wrap the mixed powder inside the steel strip using a flux-cored wire drawing device, and perform the first drawing through the first drawing die.
[0036] In some embodiments, the steel strip is made of 430 stainless steel, and the orifice of the first drawing die is 2.6 mm.
[0037] Step 150: After the first drawing, the die aperture is gradually reduced until the diameter of the flux-cored wire meets the target value.
[0038] In some implementations, the target value is 1.0 mm to 1.2 mm.
[0039] Step 160: The flux-cored wire is wound onto a wire spool and sealed in a vacuum packaging bag to generate the iron-based amorphous flux-cored wire for use on the surface of austenitic welds.
[0040] In some embodiments, the method further includes: surfacing the iron-based amorphous flux-cored wire for the austenitic weld surface with a welding current of 180A to 220A, a welding voltage of 15V to 26V, and a shielding gas configuration, wherein the shielding gas consists of argon and helium in a volume ratio of 4:1, the surfacing thickness is 1.8 mm to 2 mm, and the weld overlap rate is 20% to 30%. This method can be understood as a surfacing process for the iron-based amorphous flux-cored wire for the austenitic weld surface.
[0041] Preferably, the welding process involves welding one layer to form the weld overlay.
[0042] This application's embodiments, through optimized welding process parameters and shielding gas combinations, create ideal conditions for rapid solidification of the molten pool and amorphous formation. This preparation method requires only conventional welding equipment and can prepare a high-performance amorphous alloy reinforcement layer on the surface of austenitic stainless steel welds through single-layer cladding. It effectively solves the technical challenge of efficient and high-performance on-site reinforcement and repair of critical components (such as boiler pipes in thermal power units) under high-temperature erosion and corrosion conditions, possessing both excellent engineering applicability and significant technical and economic benefits. The preparation method of this application's embodiments is simple in process. The obtained welding wire has a wide welding process window, suitable for both tungsten inert gas welding (TIG) and metal inert gas welding (MIG), making it easy to implement in engineering sites.
[0043] To further demonstrate the effects of the embodiments of this application, the embodiments of this application are described in detail based on the following embodiments 1 to 6.
[0044] Example 1 includes the following steps S11-S15.
[0045] Step S11: Weigh out Mo as 40.0%, Cr as 30.0%, C as 5.0%, B as 6.0%, Si as 1.0%, and the remainder as Fe according to the mass percentage. The sum of the mass percentages of the above components is 100%.
[0046] Step S12: Place the weighed powder from step 1 into a vacuum heating furnace and heat it at 200°C for 1 hour to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 1 hour. Step S13: Use alcohol to remove the grease from the surface of the 430 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 430 steel strip. The diameter of the first drawing die is 2.6mm. Step S14: After the first drawing process is completed, the die hole diameter is reduced sequentially to finally obtain flux-cored welding wire with a diameter of 1.0~1.2mm.
[0047] Step S15: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.
[0048] In addition, this application embodiment uses an iron-based amorphous flux-cored welding wire prepared for austenitic weld surfaces, as described in Example 1, to perform surface cladding on austenitic steel (TP347H). The cladding method is as follows: the welding current is 180~220A, the welding voltage is 15V, and the shielding gas is 80%Ar+20%He. One layer of cladding is formed, with a thickness controlled at 1.8mm and a weld overlap rate of 20%.
[0049] The welding process and weld overlay properties of an iron-based amorphous flux-cored wire for austenitic weld surfaces described in Example 1 above include at least the following: stable arc and minimal spatter during the welding process; a weld overlay microhardness of 631HV0.3; an amorphous content of 81%; and a weight loss of 0.51g after 10 minutes of high-temperature erosion at 610℃, compared to 1.90g for the base material TP347H after the same process. Therefore, the weld overlay developed based on Example 1 exhibits excellent high-temperature erosion resistance.
[0050] Example 2 includes the following steps S21-S25.
[0051] Step S21: Weigh out Mo as 45.0%, Cr as 35.0%, C as 7.0%, B as 8.0%, Si as 2.0%, and the remainder as Fe according to the mass percentage. The sum of the mass percentages of the above components is 100%.
[0052] Step S22: Place the weighed medicine powder from step 1 into a vacuum heating furnace and heat it at 240°C for 4 hours to remove the water of crystallization from the medicine powder; place the dried medicine powder into a powder mixer for thorough mixing for 4 hours. Step S23: Use alcohol to remove the grease from the surface of the 430 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 430 steel strip. The diameter of the first drawing die is 2.6mm. Step S24: After the first drawing process is completed, the die hole diameter is reduced in sequence to finally obtain flux-cored welding wire with a diameter of 1.0~1.2mm.
[0053] Step S25: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.
[0054] In addition, this application embodiment uses Example 2 to prepare an iron-based amorphous flux-cored welding wire for surfacing austenitic steel (TP347H) surfaces. The surfacing method is as follows: the welding current is 220A, the welding voltage is 26V, and the shielding gas is 80%Ar+20%He. One layer of surfacing is formed, with a thickness controlled at 2.0mm and a weld overlap rate of 30%.
[0055] The welding process and weld overlay properties of an iron-based amorphous flux-cored wire for austenitic weld surfaces described in Example 2 above include at least the following: stable arc and minimal spatter during the welding process; a weld overlay microhardness of 638HV0.3; an amorphous content of 82%; and a weight loss of 0.55g after 10 minutes of high-temperature erosion at 610°C, compared to 1.90g for the base material TP347H after the same process. Therefore, the weld overlay developed based on Example 2 exhibits excellent high-temperature erosion resistance.
[0056] Reference Figure 2 The diagram illustrates the macroscopic morphology of the weld overlay layer obtained by using the iron-based amorphous flux-cored wire prepared in Example 2 for austenitic weld surfaces on an austenitic steel plate, as shown in this embodiment of the application. Figure 2 As can be seen, the weld overlay layer is aesthetically pleasing. (See attached image.) Figure 3 The image shows the surface morphology of an austenitic steel plate after a high-temperature erosion test (10 min) at 610°C, obtained by using an iron-based amorphous flux-cored wire prepared in Example 2 for austenitic weld surface surfacing in an embodiment of this application. Figure 3 As can be seen, after the weld overlay was subjected to high-temperature erosion, the surface erosion morphology was fine and uniform, and no large blocky weld overlay erosion shear morphology was found.
[0057] Example 3 includes the following steps S31-S35.
[0058] Step S31: Weigh out Mo as 43.0%, Cr as 33.0%, C as 6.0%, B as 7.0%, Si as 1.5%, and the remainder as Fe according to the mass percentage. The sum of the mass percentages of the above components is 100%.
[0059] Step S32: Place the weighed powder from step 1 into a vacuum heating furnace and heat it at 220°C for 2.5 hours to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 2.5 hours. Step S33: Use alcohol to remove the grease from the surface of the 430 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 430 steel strip. The diameter of the first drawing die is 2.6mm. Step S34: After the first drawing process is completed, the die hole diameter is reduced in sequence to finally obtain flux-cored welding wire with a diameter of 1.0~1.2mm.
[0060] Step S35: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.
[0061] In addition, this application embodiment uses an iron-based amorphous flux-cored welding wire prepared in Example 3 for surfacing austenitic steel (TP347H). The surfacing method is as follows: the welding current is 200A, the welding voltage is 20V, and the shielding gas is 80%Ar+20%He. One layer of surfacing is formed, with a thickness controlled at 1.9mm and a weld overlap rate of 25%.
[0062] The welding process and weld overlay properties of an iron-based amorphous flux-cored wire for austenitic weld surfaces described in Example 3 above include at least the following: stable arc and minimal spatter during the welding process; a weld overlay microhardness of 629HV0.3; an amorphous content of 81.4%; and a weight loss of 0.50g after 10 minutes of high-temperature erosion at 610℃, compared to 1.90g for the base material TP347H after the same process. Therefore, the weld overlay developed based on Example 3 exhibits excellent high-temperature erosion resistance.
[0063] Example 4 includes the following steps S41-S45.
[0064] Step S41: Weigh out Mo as 41.0%, Cr as 31.0%, C as 5.1%, B as 6.1%, Si as 1.1%, and the remainder as Fe according to the mass percentage. The sum of the mass percentages of the above components is 100%.
[0065] Step S42: Place the weighed powder from step 1 into a vacuum heating furnace and heat it at 210°C for 1.1 hours to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 1.1 hours. Step S43: Use alcohol to remove the grease from the surface of the 430 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 430 steel strip. The diameter of the first drawing die is 2.6mm. Step S44: After the first drawing process is completed, the die hole diameter is reduced in sequence to finally obtain flux-cored welding wire with a diameter of 1.0~1.2mm.
[0066] Step S45: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.
[0067] In addition, this application embodiment uses an iron-based amorphous flux-cored welding wire prepared in Example 4 for surfacing austenitic steel (TP347H). The surfacing method is as follows: the welding current is 181A, the welding voltage is 16V, and the shielding gas is 80%Ar+20%He. One layer of surfacing is formed, with a thickness controlled at 1.81mm and a weld overlap rate of 21%.
[0068] The welding process and weld overlay properties of an iron-based amorphous flux-cored wire for austenitic weld surfaces described in Example 4 above include at least the following: stable arc and minimal spatter during the welding process; a weld overlay microhardness of 627HV0.3; an amorphous content of 83%; and a weight loss of 0.58g after 10 minutes of high-temperature erosion at 610°C, compared to 1.90g for the base material TP347H after the same process. Therefore, the weld overlay developed based on Example 4 exhibits excellent high-temperature erosion resistance.
[0069] Example 5 includes the following steps S51-S55.
[0070] Step S51: Weigh out Mo as 42.0%, Cr as 32.0%, C as 5.2%, B as 6.2%, Si as 1.2%, and the remainder as Fe according to the mass percentage. The sum of the mass percentages of the above components is 100%.
[0071] Step S52: Place the weighed medicine powder from step 1 into a vacuum heating furnace and heat it at 222℃ for 1.4 hours to remove the water of crystallization from the medicine powder; place the dried medicine powder into a powder mixer for thorough mixing for 1.4 hours. Step S53: Use alcohol to remove the grease from the surface of the 430 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 430 steel strip. The diameter of the first drawing die is 2.6mm. Step S54: After the first drawing process is completed, the die hole diameter is reduced sequentially to finally obtain flux-cored welding wire with a diameter of 1.0~1.2mm.
[0072] Step S55: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.
[0073] In addition, this application embodiment uses an iron-based amorphous flux-cored welding wire prepared in Example 5 for surfacing austenitic steel (TP347H). The surfacing method is as follows: the welding current is 195A, the welding voltage is 18V, and the shielding gas is 80%Ar+20%He. One layer of surfacing is formed, with a thickness controlled at 1.85mm and a weld overlap rate of 27%.
[0074] The welding process and weld overlay properties of an iron-based amorphous flux-cored wire for austenitic weld surfaces described in Example 5 above include at least the following: stable arc and minimal spatter during the welding process; a weld overlay microhardness of 639HV0.3; an amorphous content of 86%; and a weight loss of 0.44g after 10 minutes of high-temperature erosion at 610°C, compared to 1.90g for the base material TP347H after the same process. Therefore, the weld overlay developed based on Example 5 exhibits excellent high-temperature erosion resistance.
[0075] Example 6 includes the following steps S61-S65.
[0076] Step S61: Weigh out Mo as 44.0%, Cr as 34.0%, C as 6.9%, B as 7.9%, Si as 1.9%, and the remainder as Fe according to the mass percentage. The sum of the mass percentages of the above components is 100%.
[0077] Step S62: Place the weighed medicine powder from step 1 into a vacuum heating furnace and heat it at 230°C for 3.8 hours to remove the water of crystallization from the medicine powder; place the dried medicine powder into a powder mixer for thorough mixing for 3.8 hours. Step S63: Use alcohol to remove the grease from the surface of the 430 steel strip, and use a flux-cored wire drawing device to wrap the flux powder prepared in step 2 inside the 430 steel strip. The diameter of the first drawing die is 2.6mm. Step S64: After the first drawing process is completed, the die hole diameter is reduced sequentially to finally obtain flux-cored welding wire with a diameter of 1.0~1.2mm.
[0078] Step S65: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.
[0079] In addition, this application embodiment uses an iron-based amorphous flux-cored welding wire prepared for austenitic weld surfaces, as described in Example 6, to perform surface cladding on austenitic steel (TP347H). The cladding method is as follows: the welding current is 219A, the welding voltage is 25V, and the shielding gas is 80%Ar + 20%He. One layer of cladding is formed, with a thickness controlled at 1.99mm and a weld overlap rate of 29%.
[0080] The welding process and weld overlay properties of an iron-based amorphous flux-cored wire for austenitic weld surfaces described in Example 6 above include at least the following: stable arc and minimal spatter during the welding process; a weld overlay microhardness of 633HV0.3; an amorphous content of 83.3%; and a weight loss of 0.515g after 10 minutes of high-temperature erosion at 610°C, compared to 1.90g for the base material TP347H after the same process. Therefore, the weld overlay developed based on Example 6 exhibits excellent high-temperature erosion resistance.
[0081] This application embodiment is based on the Fe-Mo-Cr alloy system, with the addition of B, C, and Si elements, resulting in an amorphous coating with high hardness and good high-temperature wear resistance. The welding wire in this application embodiment forms the amorphous coating through arc welding. Utilizing the high cooling rate during arc welding, the preparation process is simpler and has higher application value compared to amorphous coatings produced by traditional casting methods. Based on a reasonable element ratio (controlling the content of main alloying elements and trace alloying elements), the amorphous content in the amorphous coating reaches over 80%. The welding wire provided in this application embodiment has a simple preparation process. The obtained welding wire has a wide welding process window, suitable for both TIG and MIG welding methods, and is easy to implement in engineering fields.
[0082] It is understood that the above embodiments are merely exemplary implementations used to illustrate the principles of this application, and this application is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and substance of this application, and these modifications and improvements are also considered to represent the scope of protection of this application.
Claims
1. An iron-based amorphous flux cored wire for an austenitic weld surface, characterized by, Includes the powder and the solder coating that encapsulates the powder. The powder is composed of the following components in weight percentage: 40.0% to 45.0% molybdenum, 30.0% to 35.0% chromium, 5.0% to 7.0% carbon, 6.0% to 8.0% boron, 1.0% to 2.0% silicon, and the remainder being iron; The sum of the mass percentages of all components is 100%.
2. The iron-based amorphous core flux for austenitic weld surface according to claim 1, characterized in that, The purity of the alloy powder composed of each component in the powder is not less than 99.9%.
3. The iron-based amorphous core flux for austenitic weld surface according to claim 1, characterized in that, The particle size of each component in the powder is between 100 and 200 mesh.
4. The iron-based amorphous core flux for austenitic weld surface according to claim 1, characterized in that, The weld bead is a steel strip with a thickness of 0.4 mm and a width of 7 mm.
5. The iron-based amorphous core flux solder wire for austenitic weld surface according to claim 1, characterized in that, The flux-cored wire, which is composed of flux powder wrapped by the welding skin, has a flux powder filling rate of 20% to 25%.
6. A production method for producing an iron-based amorphous flux cored wire for an austenitic weld surface as claimed in any one of claims 1 to 5, characterized in that, include: The ingredients of the powder are weighed according to the following mass percentages: 40.0% to 45.0% molybdenum, 30.0% to 35.0% chromium, 5.0% to 7.0% carbon, 6.0% to 8.0% boron, 1.0% to 2.0% silicon, and the remainder is iron. The sum of the mass percentages of each ingredient is 100%. The powder is placed in a vacuum furnace and heated to dry it, which is used to remove the water of crystallization from the powder. The heated and dried medicinal powder is mixed in a powder mixer. Alcohol is used to remove grease from the surface of the steel strip, and the mixed powder is wrapped inside the steel strip using a flux-cored wire drawing device, and then the first drawing is performed through a first drawing die. After the first drawing process, the die aperture is gradually reduced until the diameter of the flux-cored wire meets the target value. The flux-cored wire is wound onto a wire spool and sealed in a vacuum packaging bag to generate the iron-based amorphous flux-cored wire for the austenitic weld surface.
7. A method of manufacture according to claim 6, wherein, The step of placing the medicinal powder in a vacuum heating furnace for heating and drying includes: The powder is heated and dried in a vacuum furnace at a temperature of 200°C to 240°C and a holding time of 1 hour to 4 hours.
8. The preparation method according to claim 6, characterized in that, The step of mixing the heated and dried medicinal powder in a powder mixer includes: The heated and dried medicinal powder is mixed in a powder mixer, with a mixing time of 1 to 4 hours.
9. The preparation method according to claim 6, characterized in that, The steel strip is made of 430 stainless steel, the aperture of the first drawing die is 2.6 mm, and the target value is 1.0 mm to 1.2 mm.
10. The preparation method according to claim 6, characterized in that, The method further includes: Based on the conditions of welding current of 180A to 220A, welding voltage of 15V to 26V, and configuration of shielding gas, the iron-based amorphous flux-cored wire for the surface of austenitic weld is surfacing. The shielding gas consists of argon and helium in a volume ratio of 4:
1. The thickness of the surfacing is 1.8 mm to 2 mm, and the overlap rate of the surfacing weld is 20% to 30%.