Hardfacing material, flux-cored welding wire and hardfacing wear part
By optimizing the composition of the flux-cored welding wire, a mixed matrix of austenite and tempered martensite is formed, increasing the solid solution content of chromium. This solves the problem of wear failure of traditional chromium carbide coatings in corrosive environments, and improves both wear resistance and corrosion resistance.
Patent Information
- Application Number
- CN202611213426.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional chromium carbide coatings are prone to pitting and intergranular corrosion in salt spray, acidic, or chloride-containing corrosive environments, leading to wear resistance failure. Furthermore, it is difficult to increase the solid solubility of Cr in the matrix to improve corrosion resistance.
By optimizing the composition of the flux-cored welding wire, reducing the ratio of carbon to chromium, and increasing the nickel content, a mixed matrix of austenite and tempered martensite is formed, increasing the solid solution content of chromium, and combining the effects of molybdenum and manganese to form a wear-resistant layer to enhance the corrosion resistance and wear resistance of the matrix.
This approach achieves significant improvements in corrosion resistance and hardness of welded wear-resistant parts while ensuring wear resistance, thus extending their service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of welding technology, and in particular to a hardfacing material, flux-cored welding wire, and wear-resistant surfacing components. Background Technology
[0002] Applying a chromium carbide-rich alloy to the surface of a base material through welding or fusion processes creates a chromium carbide overlay (CCO) with a hard and durable surface. This significantly improves the material's wear resistance, impact resistance, corrosion resistance, and heat resistance, making it ideal for high-wear industrial applications. Traditional chromium carbide overlays containing 4.5% carbon and 25% chromium exhibit stable and balanced properties and are widely used in abrasive wear conditions in mining, cement, and power plants, becoming a standard reference sample in the industry. However, the performance of this traditionally formulated chromium carbide overlay still has considerable room for improvement.
[0003] In conventionally formulated chromium carbide coatings, the presence of a large amount of hard, particulate M7C3 primary carbides incorporated into the matrix provides excellent dry wear resistance, thus extending the service life of the chromium carbide coating and the overall material. However, the matrix material of the chromium carbide coating itself is primarily steel, which has relatively low corrosion resistance. This makes the chromium carbide coating susceptible to pitting and intergranular corrosion in corrosive abrasive environments such as salt spray, acid, or chloride ion-containing environments, leading to carbide detachment and wear failure.
[0004] To improve the corrosion resistance of chromium carbide coatings and suppress pitting and intergranular corrosion, it is necessary to increase the solid solubility of chromium in the matrix. However, due to limitations in the filler ratio of flux-cored wire and the cost of chromium-containing raw materials, it is difficult to increase the Cr content in the molten pool to over 40%. Furthermore, Cr is a carbide-forming element with a strong ability to bind carbon; in the presence of carbon, Cr readily precipitates, leading to a decrease in solid solubility. In this situation, to increase the solid solubility of Cr in the matrix, it is necessary to reduce the carbon content in the environment. This results in a reduction in chromium carbide particles, leading to a decrease in the wear resistance and hardness of the chromium carbide coating, making it difficult to meet application requirements. Summary of the Invention
[0005] The purpose of this invention is to provide a hardened material, flux-cored welding wire, and wear-resistant surfacing parts with good wear resistance and corrosion resistance.
[0006] To achieve the above objectives, the present invention provides the following technical solution: A flux-cored welding wire includes an outer sheath and a filler wrapped within the outer sheath. The outer sheath is a low-carbon steel strip. The filler includes Cr, C, and Ni elements. The Cr element has a mass fraction of 55% to 65% in the filler, the C element has a mass fraction of 9% to 12% in the filler, and the Ni element has a mass fraction of 3% to 5% in the filler. The mass percentage of the filler in the flux-cored welding wire is any value between 45% and 55%.
[0007] Optionally, the packing material further includes Mo and Nb elements, wherein the Mo element has any value in the mass fraction of the packing material ranging from 1.5% to 4%, and the Nb element has any value in the mass fraction of the packing material ranging from 1% to 3%.
[0008] Optionally, the packing material further includes Si and Mn elements, wherein the mass fraction of Si in the packing material is any value between 1% and 3%, and the mass fraction of Mn in the packing material is any value between 1% and 3%.
[0009] Optionally, the filler is in powder form and includes high-carbon ferrochrome, metallic chromium, nickel powder, ferromolybdenum, ferroniobium, graphite, ferrosilicon, ferromanganese and arc stabilizer, and the outer diameter of the outer skin is any value from 2.4 mm to 4.0 mm.
[0010] Optionally, when the flux-cored wire is used for welding low-carbon steel, the single-layer dilution rate is controlled to be less than or equal to any value of 35%.
[0011] In a second aspect, the present invention also provides a hard-surface material, comprising a matrix and hard particles dispersed within the matrix; the matrix is a mixture of austenite and tempered martensite; the matrix contains Cr element at a mass fraction greater than or equal to 12%; and the hard particles in the hard-surface material have a volume fraction of any value between 25% and 37%.
[0012] Optionally, the tempered martensite accounts for more than or equal to 30% of the matrix, and the matrix contains Mo element with a mass fraction greater than or equal to 0.5%; the hard particles include M7C3 type carbides, M... 23 C6 type carbides and NbC particles, the M7C3 type carbides and the M 23 The total fraction of C6 type carbide in the hardfacing material is any value between 24% and 35%, and the volume fraction of NbC carbide in the hardfacing material is any value between 0.5% and 1.2%.
[0013] Thirdly, the present invention also provides a weld overlay wear-resistant part, comprising a base material layer and a wear-resistant layer covering the surface of the base material layer, wherein the wear-resistant layer is the aforementioned hard surface material, and the average thickness of the wear-resistant layer is any value greater than or equal to 4 mm, and the base material layer is made of low carbon steel.
[0014] Optionally, the wear-resistant layer has an average hardness of any value between 54 HRC and 60 HRC, a neutral salt spray red rust corrosion resistance time of more than 96 h, and, with a 4.5% C-25% Cr chromium carbide coating as a reference, the relative wear resistance of the hard surface material is any value greater than or equal to 0.8.
[0015] Optionally, the mass fraction of C element in the detection surface of the wear-resistant layer is any value between 2.8% and 3.3%, the mass fraction of Nb element is any value between 0.5% and 1.5%, the mass fraction of Ni element is any value between 1.0% and 2.5%, the mass fraction of Mo element is any value between 1.0% and 2.0%, and the mass fraction of Cr element is any value between 30% and 33%. The detection surface is obtained by removing the oxide layer from the surface of the wear-resistant layer.
[0016] According to a first aspect of the invention, the ratio of carbon to chromium content is reduced to decrease the precipitation of hard chromium carbide particles during the solidification process of the weld pool, thereby increasing the solid solution content of chromium in the weld metal matrix and improving the overall corrosion resistance of the weld metal. By appropriately controlling the hardenability and austenite stability of the matrix with metallic nickel, combined with the role of chromium in stabilizing austenite at a high mass fraction, the matrix of the weld metal is made into a mixture of austenite and martensite. This compensates for the decrease in wear resistance and hardness caused by the reduction in the content of hard chromium carbide particles, thus giving the weld metal both good wear resistance and corrosion resistance, as well as high macroscopic hardness, extending the service life of the weld metal and making it highly practical.
[0017] According to a second aspect of the invention, by constraining the chromium solid solution content and hard particle content in the matrix of the hardfacing material, it is helpful to ensure that the hardfacing material simultaneously possesses good wear resistance and corrosion resistance, resulting in balanced performance and a long service life. The matrix is a mixture of austenite and tempered martensite, giving it the advantages of high hardness and wear resistance of martensite and the advantages of austenite in absorbing impact energy and reducing weld cold cracking, thus providing the hardfacing material with good mechanical properties.
[0018] According to a third aspect of the present invention, by overlaying welding to form a wear-resistant layer covering the surface of the base material and having a certain thickness, it helps to protect the base material and form an overlayed wear-resistant part with good wear and corrosion resistance on the surface.
[0019] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below. Detailed Implementation
[0020] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicating orientation or positional relationships, are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0022] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0023] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0024] To address the aforementioned problems, this invention optimizes the formulation of the flux-cored welding wire used to form the chromium carbide coating, thereby improving the corrosion resistance of the formed chromium carbide coating.
[0025] This application protects a flux-cored welding wire, comprising an outer sheath and filler encased within the sheath. The outer sheath is a low-carbon steel strip. The filler comprises Cr, C, and Ni elements. The Cr element has a mass fraction in the filler of any value between 55% and 65%, for example, any value between 55%, 59%, 63%, and 65%. The C element has a mass fraction in the filler of any value between 9% and 12%, for example, any value between 9%, 10%, 11%, and 12%. The Ni element has a mass fraction in the filler of any value between 3% and 5%, for example, any value between 3%, 4%, and 5%. The mass percentage of the filler in the flux-cored welding wire is any value between 45% and 55%, for example, any value between 45%, 48%, 52%, and 55%.
[0026] By reducing the carbon-to-chromium ratio, the loss of chromium due to carbide precipitation from the matrix is reduced, increasing the solid solution content of chromium in the matrix and thus improving the corrosion resistance of the matrix. During the welding process, the primary phase of the molten pool solidifies as austenite. Due to the high mass fraction of dissolved Cr in the matrix, the martensitic transformation initiation temperature (Ms point) is lowered. However, the precipitation of hard chromium carbide particles causes the Ms point to rise again, making it easier for high-temperature austenite to be retained during cooling to room temperature, resulting in a large amount of retained austenite. For example, in classic chromium carbide capping layers with a composition of 4.5% C and 25% Cr, the matrix is almost entirely austenite in most cases. This application adjusts the composition of the flux-cored wire to ensure that the molten pool contains a suitable amount of Ni. Ni, dissolved in a Fe-dominated matrix, enhances the matrix's hardenability and inhibits diffusion-type phase transformations such as pearlite during cooling. Furthermore, by appropriately controlling the austenite stability and Ms point range, some austenite undergoes martensitic transformation during weld cooling, resulting in a mixed austenite and quenched martensite microstructure. Simultaneously, utilizing the heat dissipation within the weld layer and the thermal cycling of subsequent weld passes, the quenched martensite undergoes self-tempering to tempered martensite, forming a relatively uniformly distributed austenite and tempered martensite dual-phase matrix. Compared to austenite, tempered martensite exhibits higher hardness and wear resistance, compensating for the reduced wear resistance caused by decreased chromium carbide content. This results in a hardened surface material with both good wear resistance and corrosion resistance. Moreover, as an austenite stabilizing element, Ni broadens the displacement dissolution limit of chromium in iron-based solid solutions, increasing the matrix's capacity to accommodate Cr atoms and contributing to higher Cr solid solution content, thereby enhancing the matrix's corrosion resistance.
[0027] It is important to note that although Ni, along with Nb and Mo (mentioned later), are commonly used components in flux-cored welding wires, this application employs content adjustments to alter the roles of each element during the welding process, resulting in unique technical effects. In this application, the proportions of Cr, C, Ni, and Fe (the main component of the matrix) must be coordinated to ensure the hardfacing material simultaneously achieves good corrosion resistance, wear resistance, and high hardness, thereby improving its overall performance. Therefore, the proportions of various elements in this application constitute a complete solution and should not be discussed separately. Furthermore, changes in elemental composition alter the changes and mechanisms of action of each element during the welding process, leading to fundamental differences in the solution. For example, when the Ni content in the wear-resistant layer is below 1.0%, the matrix hardenability is insufficient, and diffusion-type phase transformations such as pearlite are more likely to occur during cooling; when the Ni content is too high, the austenite stability is too high, and the amount of martensite transformation decreases. Even if the corrosion resistance of the matrix is improved by adding Ni, the underlying principle is fundamentally different from the solution in this application. When the Cr content in the wear-resistant layer is low (e.g., less than 30%) or the C content is high (e.g., greater than 3.3%), even if the overall wear resistance is improved with the help of Ni, the Cr to C ratio leads to a large amount of Cr precipitating out with the C in the matrix. The Cr solid solution level is low, resulting in poor corrosion resistance and the material performance not meeting expectations. Furthermore, due to the low Cr solid solution level, the matrix is prone to martensite transformation, and there is no incentive to adjust the martensitic transformation initiation temperature M using Ni. s This leads to fundamental differences in the solutions. Besides the situations mentioned above, changes in the filler content, base material, and dilution rate during welding significantly impact the elemental content and proportions in the weld pool, thus greatly affecting the performance of the wear-resistant layer and resulting in differences in the solutions.
[0028] This application improves the hardenability of the matrix and suppresses diffusion-type phase transformations such as pearlite by controlling the Ni content within an appropriate range. Simultaneously, it avoids excessive austenite stability leading to an excessive amount of residual austenite, thus forming a mixed structure of austenite and martensite in the matrix. This improves the mechanical properties of the matrix, compensating for the loss of wear resistance caused by the decrease in chromium carbide particle content. Furthermore, the increased solid solution content of Cr significantly improves the corrosion resistance of the matrix, compensating for the relatively poor corrosion resistance of martensite compared to austenite. Therefore, the hardface material obtained by weld overlay simultaneously achieves high wear resistance, corrosion resistance, and hardness. This application overcomes the technical bias of improving the wear resistance of hardface materials through chromium carbide particles, and also overcomes the technical bias that austenite is superior to martensite in improving the corrosion resistance of the matrix, making the technical solution in this application highly inventive.
[0029] In some embodiments, the filler also includes Mo and Nb elements, wherein the mass fraction of Mo in the filler is any value from 1.5% to 4%, for example, any value from 1.5%, 1.8%, 2.3%, 3.5%, and 4%. The mass fraction of Nb in the filler is any value from 1% to 3%, for example, any value from 1%, 1.2%, 1.9%, 2.6%, and 3%.
[0030] Mo dissolved in austenite will moderately lower the martensitic transformation initiation temperature. s After quenching, the martensitic matrix retains a large number of supersaturated Mo atoms. On the one hand, Mo strengthens the martensitic matrix through solid solution strengthening, enhancing its strength and hardness. Simultaneously, it inhibits cementite coarsening during tempering, promotes the precipitation of fine alloy carbides, and generates a secondary hardening effect. On the other hand, Mo effectively delays the recovery and dislocation annihilation of the martensitic matrix during tempering, inhibits the formation of continuous carbide films at grain boundaries and lath boundaries, improves grain boundary toughness, and reduces temper brittleness. Furthermore, Mo improves austenite stability and hardenability, ensuring that thick-section components fully acquire martensitic structure. It also mitigates temper embrittlement caused by elements such as Cr and Ni, optimizes the stability of dislocation substructures within lath martensite, and achieves a synergistic improvement in the strength and toughness of the martensitic matrix. In addition, Mo can participate in carbide formation in small quantities and reduce the tendency for chromium carbide precipitation, alleviating chromium depletion at grain boundaries. It can also accumulate in the passivation film, significantly improving resistance to pitting corrosion and chloride ion corrosion. Nb is a carbide-forming element with a stronger ability to bind carbon than Cr. It will preferentially capture free carbon in the system to form fine NbC, reduce the carbon activity in the molten pool, weaken the metallurgical driving force for Cr to combine with C and precipitate chromium carbide, reduce the loss caused by Cr desolvation from the matrix, thereby increasing the solid solution content of Cr in the matrix, giving the matrix excellent corrosion resistance, and inhibiting pitting corrosion and intergranular corrosion problems in hardfacing materials.
[0031] The role of Mo in the system of this application is closely related to the formation of martensite during the cooling process. When the matrix does not contain martensite, even if Mo is added to improve the material's resistance to hydrogen corrosion and creep, it cannot be equivalent to the solution in this application. When the content of carbon and chromium in the system is low (e.g., C content less than 0.5%, Cr content less than 7%), adding a small amount of niobium (e.g., less than 0.3%) can refine the grains, optimize the microstructure, and improve hydrogen resistance. However, this effect is fundamentally different from the effect of inhibiting chromium carbide precipitation in this application. Therefore, this technical means is not the same as the technical means in this application.
[0032] In some embodiments, the filler also includes Si and Mn elements, wherein the mass fraction of Si in the filler is any value from 1% to 3%, for example, any value from 1.3%, 2.1%, and 2.8%. The mass fraction of Mn in the filler is any value from 1% to 3%, for example, any value from 1.3%, 2.1%, and 2.8%.
[0033] Mn is the core deoxidizing and desulfurizing element in the system. In the weld pool, it preferentially combines with oxygen and sulfur to form low-melting-point silicates and sulfides. The slag floats to the surface and is removed, eliminating the risk of porosity and hot cracking, purifying the weld metal matrix, and moderately dissolving into the matrix to assist in solid solution strengthening and stabilize the austenite structure. A small amount of manganese enters the M7C3 type carbide lattice to fine-tune the carbide toughness. Si has the dual functions of strong deoxidation and slag regulation. In the weld pool stage, it combines with MnO and Cr2O3 to form a slag with suitable fluidity, isolating air to reduce the oxidation loss of Cr and C, ensuring the effective utilization rate of Cr and C to maintain the total amount of hard phase. Silicon atoms dissolve in the matrix to slightly increase hardness, while refining the primary and eutectic M7C3 type grains and weakening the negative effect of coarse hard phases cutting the matrix.
[0034] In some embodiments, the filler is in powder form and includes high-carbon ferrochrome, metallic chromium, nickel powder, ferromolybdenum, ferroniobium, graphite, ferrosilicon, ferromanganese and an arc stabilizer, and the outer diameter of the outer skin is any value from 2.4 mm to 4.0 mm, for example, any value from 2.4 mm, 2.8 mm, 3.2 mm and 4.0 mm.
[0035] The filler is a blend of two chromium sources: high-carbon ferrochrome and metallic chromium. High-carbon ferrochrome provides combined carbon to generate a sufficient amount of (Cr,Fe)7C3 hard, wear-resistant phase, while metallic chromium, being carbon-free elemental chromium, increases the total chromium mass fraction without raising carbon activity, reducing chromium desolvation from the matrix to precipitate carbides and increasing the solid-solution chromium mass fraction in the austenitic and tempered martensite dual-phase matrix. Simultaneously, the two sources complement each other in particle size and solubility, stabilizing the deposited metallic chromium zone and improving powder filling uniformity. The arc stabilizer relies on high-temperature ionization of low-potential metal ions to stabilize the arc, improving arc ignition and re-ignition stability, increasing the concentration of charged particles in the arc space, and reducing arc breakage and arc drift. Graphite precisely controls the total carbon mass fraction to ensure hard phase formation and optimize powder forming fluidity. Part of the graphite burns in the arc to generate a protective atmosphere, helping to protect the molten pool from excessive oxidation. The synergistic matching of various raw materials enables the hardfacing material to simultaneously achieve high matrix solid-solution chromium, sufficient wear-resistant carbides, excellent corrosion resistance, and stable welding processability.
[0036] In some embodiments, when flux-cored welding wire is used for welding low-carbon steel, the single-layer dilution rate is controlled to be any value less than or equal to 35%, such as any value among 35%, 30%, and 25%. By controlling the dilution rate, it is helpful to control the content of each element in the molten pool during welding, thereby ensuring that the hardened material has good wear resistance and corrosion resistance.
[0037] Secondly, the present invention also provides a hardening material, comprising a matrix and hard particles dispersed within the matrix. The matrix is a mixture of austenite and tempered martensite. The matrix contains a Cr element dissolved in it at a mass fraction greater than or equal to 12%. The mass fraction of the Cr element dissolved in the matrix can be, for example, any value among 12%, 13%, 14%, and 15%. The volume fraction of the hard particles in the hardening material is any value among 25% to 37%, for example, any value among 25%, 30%, 35%, and 37%.
[0038] By controlling the chromium solid solution content and hard particle content in the matrix of hardfacing materials, it is helpful to ensure that the hardfacing materials have both good wear resistance and corrosion resistance, resulting in balanced performance and a long service life. The matrix is a mixture of austenite and tempered martensite, which combines the advantages of high hardness and wear resistance of martensite with the advantages of austenite in absorbing impact energy and reducing cold cracking in welding, giving the hardfacing materials good mechanical properties.
[0039] In some embodiments, the proportion of tempered martensite in the matrix is greater than or equal to 30%, for example, it can be 30%, 40%, 45%, 50%, and 60%. The matrix contains a Mo element dissolved in it at a mass fraction greater than or equal to 0.5%. The mass fraction of the Mo element dissolved in the matrix can be any value among 0.5%, 0.6%, and 0.8%. The hard particles include M7C3 type carbides, M... 23 C6 type carbides and NbC particles, M7C3 type carbides and M 23 The total fraction of C6 carbides in the hardfacing material is any value between 24% and 35%, for example, any value between 25%, 30%, and 35%. The volume fraction of NbC carbides in the hardfacing material is any value between 0.5% and 1.2%, for example, any value between 0.5%, 0.8%, and 1.2%.
[0040] Thirdly, the present invention also provides a wear-resistant overlay component, comprising a base material layer and a wear-resistant layer covering the surface of the base material layer, wherein the wear-resistant layer is the aforementioned hard surface material, and the average thickness of the wear-resistant layer is any value greater than or equal to 4 mm, for example, any value among 4 mm, 8 mm and 12 mm, and the base material layer is made of low carbon steel.
[0041] By overlaying welding to form a wear-resistant layer with a certain thickness covering the surface of the base material, it helps to protect the base material and form an overlay wear-resistant part with good wear and corrosion resistance.
[0042] In some embodiments, the average hardness of the wear-resistant layer is any value from 54 HRC to 60 HRC, for example, any value from 54 HRC, 56 HRC, 58 HRC, and 60 HRC. The neutral salt spray resistance to red rust corrosion is greater than 96 h, meaning no red rust forms after 96 h of exposure to a neutral salt spray environment. And when using a 4.5% C-25% Cr chromium carbide coating as a benchmark, the relative wear resistance of the hardfacing material is any value greater than or equal to 0.8, for example, any value from 0.8, 0.9, 0.95, and 1.05.
[0043] In some embodiments, the mass fraction of C element on the detection surface of the wear-resistant layer is any value from 2.8% to 3.3%, for example, any value from 2.8%, 3.0%, and 3.3%. The mass fraction of Nb element is any value from 0.5% to 1.5%, for example, any value from 0.5%, 1.0%, and 1.5%. The mass fraction of Ni element is any value from 1.0% to 2.5%, for example, any value from 1.0%, 1.5%, 2.0%, and 2.5%. The mass fraction of Mo element is any value from 1.0% to 2.0%, for example, any value from 1.0%, 1.5%, and 2.0%. And the mass fraction of Cr element is any value from 30% to 33%, for example, any value from 30%, 31%, 32%, and 33%. The detection surface is obtained by removing the oxide layer from the surface of the wear-resistant layer.
[0044] Please refer to the following examples for details.
[0045] Example 1: The flux-cored welding wire shown in a preferred embodiment of this application includes an outer sheath and filler. In this embodiment, the outer sheath is formed from SPCC low-carbon steel strip. The filler includes 60wt% high-carbon ferrochrome FeCr68C8, 17wt% metallic chromium, 4wt% nickel powder, 3wt% ferromolybdenum FeMo60-A, 2wt% ferroniobium FeNb65, 6wt% graphite, 4wt% ferrosilicon FeSi75-A, 3wt% ferromanganese FeMn75C7.0, and 1wt% arc stabilizer. The arc stabilizer is potassium titanate. Each raw material is crushed separately, uniformly sieved to a mesh size of 60-200 mesh, thoroughly dried, uniformly mixed in proportion, and dried and sieved again to obtain the filler. The filler contains 57.8% Cr, 11% C, 4.0% Ni, 1.8% Mo, 1.3% Nb, 3% Si, 2.3% Mn, and 17.8% Fe by mass. The filler is placed inside the outer sheath to form a flux-cored wire with an outer diameter of 2.8 mm, resulting in a filler content of 50%.
[0046] A plate-shaped Q235 low-carbon steel substrate was selected as the base material. Double-layer surfacing was performed using self-shielded flux-cored wire arc welding (FCAW-S) with the aforementioned flux-cored wire to obtain a wear-resistant layer with an average thickness of approximately 7 mm. This wear-resistant layer, together with the remaining base material, constitutes the surfacing wear-resistant component, and the wear-resistant layer is made of a hardfacing material. The surfacing parameters were: current 450 A, voltage 28 V, and welding speed 18 cm·min. -1 .
[0047] The wear-resistant component was longitudinally sectioned, and the cross-section of the wear-resistant layer was observed using optical metallographic microscopy. It can be seen that the hardfacing material consists of a matrix and hard particles dispersed within the matrix, and the matrix is a mixture of austenite and tempered martensite. X-ray diffraction (XRD) analysis shows that the proportion of tempered martensite in the matrix is approximately 43%. The dilution rate for double-layer welding was calculated to be approximately 13%. A portion of the surface wear-resistant layer was taken for compositional analysis. Using constant potential electrolytic extraction combined with inductively coupled plasma optical emission spectrometry (ICP-OES), the iron-based matrix was selectively dissolved, and the total mass of Cr, Ni, Mo, and Fe in the solution was measured. The calculated mass fractions of Cr, Mo, and Ni in the matrix were 13.6%, 0.6%, and 2.7%. Metallographic analysis of the volume fraction of hard particles in the hardfacing layer revealed that the hard particles contained M7C3 type particles plus M... 23 The volume fraction of C6 carbides was 29.4%, and the volume fraction of NbC carbides was 0.9%.
[0048] The wear-resistant layer underwent surface treatment to obtain a smooth test surface. The elemental composition of the test surface was determined using a benchtop spark direct-reading spectroscopy system. The results showed Cr 31.2%, C 3.05%, Ni 1.8%, Mo 1.4%, Nb 0.9%, Si 1.0%, and Mn 0.9%. Hardness testing was then performed using the method specified in GB / T 230.1-2018 "Metallic Materials - Rockwell Hardness Test", yielding a hardness of 56.8 HRC for the wear-resistant layer.
[0049] Using a purchased 4.5% C-25% Cr chromium carbide coating as a control group, the wear resistance was tested according to Procedure A of ASTM G65-2016, "Standard Test Method for Measurement of Abrasion Resistance of Metals and Materials Using Dry Sand / Rubber Wheel Apparatus." The control group showed a weight loss of 0.17g, while the wear-resistant layer in this embodiment showed a weight loss of 0.18g, with a relative wear resistance of 0.94. The wear-resistant layer was tested using the neutral salt spray (NSS) method specified in GB / T 10125-2021, "Artificial Atmosphere Corrosion Test - Salt Spray Test." No red rust was observed after 120 hours. This indicates that the hardface material obtained in this application has good wear resistance and corrosion resistance.
[0050] Example 2: The difference between this embodiment and Embodiment 1 lies only in the adjustment of the filler composition. The filler comprises 65 wt% high-carbon ferrochrome FeCr68C8, 12 wt% metallic chromium, 4.5 wt% nickel powder, 2 wt% ferromolybdenum FeMo60-A, 2.5 wt% ferroniobium FeNb65, 6 wt% graphite, 4 wt% ferrosilicon FeSi75-A, 3 wt% ferromanganese FeMn75C7.0, and 1 wt% arc stabilizer. The arc stabilizer is potassium titanate.
[0051] After surface treatment, the wear-resistant layer in this embodiment was found to have the following elemental composition on the exposed surface: Cr 31.1%, C 3.03%, Ni 1.9%, Mo 1.0%, Nb 1.1%, Si 0.9%, and Mn 0.9%.
[0052] The hardness of the wear-resistant layer in this embodiment was tested to be 55.1 HRC, no red rust was observed after 120 hours of salt spray testing, and the wear loss was 0.19 g. The calculated relative wear resistance was 0.89. It exhibits good wear resistance and corrosion resistance.
[0053] Comparative Example 1: The difference between this comparative example and Example 1 is that the filler includes 66.3 wt% high-carbon ferrochrome FeCr68C8, 12.8 wt% metallic chromium, 2.5 wt% nickel powder, and 5.5 wt% graphite.
[0054] Comparative Example 2: The difference between this comparative example and Example 1 is that the filler includes 53.8 wt% high-carbon ferrochrome FeCr68C8, 21.3 wt% metallic chromium, 5.5 wt% nickel powder, and 6.5 wt% graphite.
[0055] Comparative Example 3: The difference between this comparative example and Example 1 is that the filler includes 69.4 wt% high-carbon ferrochrome FeCr68C8, 10.6 wt% metallic chromium, and 3 wt% graphite.
[0056] Comparative Example 4: The difference between this comparative example and Example 1 is that the filler includes 53.8 wt% high-carbon ferrochrome FeCr68C8, 21.3 wt% metallic chromium, and 8 wt% graphite.
[0057] Comparative Example 5: The only difference between this comparative example and Example 1 is that the filler includes 69.5 wt% high-carbon ferrochrome FeCr68C8 and 7.5 wt% metallic chromium.
[0058] Comparative Example 6: The only difference between this comparative example and Example 1 is that the filler includes 36 wt% high-carbon ferrochrome FeCr68C8 and 41 wt% metallic chromium.
[0059] All comparative examples were based on Example 1, with the filler content of the flux-cored wire remaining at 50%. Except for the elements to be investigated and the high-carbon ferrochrome, metallic chromium, and graphite adjusted to keep the total filler mass at 100 wt% and to keep the theoretical content of the non-investigated elements basically stable, the types and amounts of other raw materials, wire preparation conditions, and welding process parameters were the same as in Example 1.
[0060] The metallographic composition of the wear-resistant layers obtained in each comparative example was observed and analyzed, and the elemental composition of the test surface was detected. Hardness, wear resistance, and corrosion resistance were then tested. The testing methods were consistent with those in the examples, and the test results are summarized in the table below.
[0061] Table 1:
[0062] In the table, A represents austenite and M represents martensite.
[0063] In Comparative Examples 1 and 2, the Ni content was adjusted. Ni can improve the hardenability of the alloy matrix and inhibit diffusion-type transformations such as pearlite during cooling of austenite; at the same time, Ni, as an austenite stabilizing element, lowers the martensite transformation initiation temperature. When Ni is too low, hardenability decreases, but austenite stability also decreases accordingly, and some austenite can transform into martensite; when Ni is too high, martensite... s If the temperature is too low, dropping to near room temperature, although austenite avoids the pearlite transformation, it also lacks sufficient supercooling to transform into martensite. This leads to an increase in retained austenite and a decrease in the amount of martensite transformed, resulting in a decrease in overall hardness and relative wear resistance. Ni variations have a relatively small impact on the overall integral rate of hard carbides. The improved corrosion resistance in Comparative Example 2 is also related to the increase in Cr dissolved in the matrix. The addition of Ni can improve the stability of austenite, thereby increasing the amount of Cr dissolved in the matrix.
[0064] Comparative Examples 3 and 4 primarily adjusted the C content. When C is low, the integral rate of chromium-based carbides decreases, and the overall integral rate of hard particles declines, thus reducing hardness and wear resistance. Simultaneously, the Cr consumed in carbide formation decreases, increasing the Cr dissolved in the matrix and improving corrosion resistance. When C is high, the integral rate of chromium-based carbides increases significantly, improving hardness and wear resistance. However, more Cr precipitates with C to form carbides, leading to a decrease in dissolved Cr in the matrix and the creation of localized Cr-depleted areas, thus reducing corrosion resistance. In Comparative Example 3, the reduced chromium carbide precipitation leads to increased M... sThe recovery is limited, making it difficult to form martensite. The small amount of martensite in Comparative Example 4 may be related to the local depletion of C and Cr around the carbides and the cooling conditions, rather than being directly promoted by the overall increase in C content.
[0065] Comparative Examples 5 and 6 primarily adjusted the Cr content. When Cr is too low, both the integral percentage of chromium carbides and the Cr dissolved in the matrix decrease, leading to reduced hardness, wear resistance, and corrosion resistance. When Cr is too high, the overall integral percentage of chromium carbides and the Cr dissolved in the matrix increase, which is beneficial for improving hardness and corrosion resistance; however, wear resistance also depends on the type, size, distribution of carbides, and the matrix's support capacity. When M... 23 When C6 coarsens, agglomerates, or is continuously distributed along grain boundaries, it may increase the risk of local crack initiation and carbide spalling, thus limiting the improvement in relative wear resistance.
[0066] The beneficial effects of this invention are that it provides a hardfacing material with good wear resistance, corrosion resistance, and hardness, as well as a corresponding flux-cored welding wire and weld overlay wear-resistant parts. While ensuring the hardness and wear resistance of the weld overlay wear-resistant parts, it effectively reduces the risk of pitting and intergranular corrosion in corrosive abrasive environments such as salt spray, acid, or chloride ion-containing environments, thus extending their service life. The hardfacing material in this invention has a relatively balanced wear resistance, corrosion resistance, and mechanical strength, making it highly practical.
[0067] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0068] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A flux-cored welding wire characterized by, The device includes an outer sheath and filler encased within the outer sheath. The outer sheath is a low-carbon steel strip. The filler contains Cr, C, and Ni elements. The Cr element has a mass fraction of 55% to 65% in the filler, the C element has a mass fraction of 9% to 12% in the filler, and the Ni element has a mass fraction of 3% to 5% in the filler. The filler accounts for a mass percentage of 45% to 55% in the flux-cored wire.
2. The flux cored welding wire of claim 1, wherein The packing material also includes Mo and Nb elements, wherein the Mo element has any value in the mass fraction of the packing material ranging from 1.5% to 4%, and the Nb element has any value in the mass fraction of the packing material ranging from 1% to 3%.
3. The flux cored welding wire of claim 2, wherein, The packing material also includes Si and Mn elements, wherein the mass fraction of Si in the packing material is any value between 1% and 3%, and the mass fraction of Mn in the packing material is any value between 1% and 3%.
4. The flux-cored welding wire as described in any one of claims 1 to 3, characterized in that, The filler is in powder form and includes high-carbon ferrochrome, metallic chromium, nickel powder, ferromolybdenum, ferroniobium, graphite, ferrosilicon, ferromanganese and arc stabilizer, and the outer diameter of the outer skin is any value between 2.4 mm and 4.0 mm.
5. The flux cored welding wire of claim 1 wherein, When the flux-cored welding wire is used for welding low-carbon steel, the single-layer dilution rate is controlled to be less than or equal to any value of 35%.
6. A hardfacing material characterized by, The material comprises a matrix and hard particles dispersed within the matrix; the matrix is a mixture of austenite and tempered martensite; the matrix contains Cr element at a mass fraction greater than or equal to 12%; and the hard particles in the hard surface material have a volume fraction of any value between 25% and 37%.
7. The hardfacing material of claim 6 wherein, The proportion of the tempered martensite in the matrix is greater than or equal to 30%, and the matrix is solid-solved with Mo element accounting for greater than or equal to 0.5% of the mass fraction of the matrix; the hard particles include chromium carbide and NbC particles, the chromium carbide includes M7C3 type carbide and / or M 23 C6 type carbide; the M7C3 type carbide and the M 23 C6 type carbide in the hard surface material is any value in 24% to 35%, and the volume fraction of the NbC carbide in the hard surface material is any value in 0.5% to 1.2%.
8. A weld overlay wear part characterized by, It includes a base material layer and a wear-resistant layer covering the surface of the base material layer, wherein the wear-resistant layer is a hard surface material as described in claim 6 or 7, and the average thickness of the wear-resistant layer is any value greater than or equal to 4 mm, and the base material layer is made of low carbon steel.
9. The overlay wear part of claim 8, wherein, The wear-resistant layer has an average hardness of any value between 54 HRC and 60 HRC, a neutral salt spray red rust corrosion resistance time of more than 96 h, and, with a 4.5% C-25% Cr chromium carbide coating as a reference, a relative wear resistance of the hard surface material of any value greater than or equal to 0.
8.
10. The wear-resistant weld overlay part as described in claim 9, characterized in that, The mass fraction of C element in the detection surface of the wear-resistant layer is any value between 2.8% and 3.3%, the mass fraction of Nb element is any value between 0.5% and 1.5%, the mass fraction of Ni element is any value between 1.0% and 2.5%, the mass fraction of Mo element is any value between 1.0% and 2.0%, and the mass fraction of Cr element is any value between 30% and 33%. The detection surface is obtained by removing the oxide layer from the surface of the wear-resistant layer.