A multi-element composite modified Ag-Cu-X based solder paste and a preparation method thereof

By designing a multi-component composite modified Ag-Cu-X-based solder paste, and employing a Co-Zn-Ni-Ti alloy formulation and inert gas-protected electrode induction suspension melting gas atomization powdering technology, the problem of poor connection between Ag-Cu-based solder and AlN ceramic substrate was solved, achieving a high-strength and high-reliability brazing connection between AlN ceramic and metallic Cu.

CN123149651APending Publication Date: 2026-11-24ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611471901.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing Ag-Cu-based solders are difficult to effectively wet and bond AlN ceramic substrates, resulting in low interfacial bonding rate and interfacial shear strength, making it difficult to achieve reliable bonding between AlN ceramics and metallic Cu.

Method used

A multi-component composite modified Ag-Cu-X-based solder paste was designed, using a Co-Zn-Ni-Ti alloy formulation. Combined with inert gas protective electrode induction suspension melting gas atomization powder preparation technology, high-purity Ag-Cu-Co-Zn-Ni-Ti active solder powder was prepared. The active paste was obtained through vacuum dispersion technology, and a five-layer brazing joint structure was constructed to alleviate the stress caused by the mismatch of thermal expansion coefficients.

Benefits of technology

It significantly improves the bonding rate and shear strength of the AlN ceramic-Cu interface, achieving a reliable connection effect and enhancing the long-term service reliability of the AlN ceramic substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149651A_ABST
    Figure CN123149651A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of brazing materials technology, specifically relating to a multi-component composite modified Ag-Cu-X-based solder paste and its preparation method. The solder paste is prepared based on a multi-component composite modified Ag-Cu-X-based active solder, which is composed of the following components in parts by weight: Ag: 60-70; Cu: 16-20; Co: 3-5; Zn: 3-5; Sn: 3-5; Ti: 2-4; and a low thermal expansion coefficient reinforcing phase of 1-3. The molar ratio of Cu, Co, Zn, and Sn is 1:1:1:1. The low thermal expansion coefficient reinforcing phase is selected from one or more of rare earth oxides, nano-Si3N4, and graphene nanosheets. This invention also provides a brazing method based on this solder paste. This invention effectively enhances the thermodynamic activity of Ti by adding Cu, Co, Zn, and Sn in an equimolar ratio, alleviates the thermal mismatch stress between AlN ceramics and copper by strengthening the phase with a low coefficient of thermal expansion, and enhances the interfacial reaction by pre-depositing active elements on the ceramic surface, thus achieving a high-strength and high-reliability brazing connection between AlN ceramics and copper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to new technologies for alloy paste formulation design and preparation, particularly a high-performance multi-component composite modified Ag-Cu-X (X is the modifying component) based solder paste material applicable to advanced manufacturing fields such as third-generation semiconductors, new energy vehicles, aerospace, and high-end equipment. Background Technology

[0002] Welding technology is a key material processing technique for achieving tight connections between different materials. It is an important foundation for advanced manufacturing, and its sophistication directly reflects a country's manufacturing development level. Brazing is one of the three pillars of welding technology. It mainly uses brazing materials to fill the gaps in solid workpieces to achieve the connection of similar or dissimilar materials. It is known as the "industrial universal adhesive" and has become an important support for the development of advanced manufacturing industries such as semiconductors, new energy vehicles, aerospace, and high-end equipment.

[0003] In recent years, with the rapid development of the third-generation semiconductor manufacturing industry, solder and its welding technology have been applied to AlN ceramic heat dissipation substrates. Among these applications, achieving Cu coating on the surface of AlN ceramic substrates is crucial for the development of heat dissipation substrates and is one of the bottleneck problems that urgently needs to be solved for the domestic production of semiconductor power device packaging. Currently, the mainstream methods for coating AlN ceramic substrates with Cu are direct Cu coating (DBC) and active brazing Cu coating (AMB). Compared with DBC, Cu-coated ceramic substrates obtained using the AMB process have high thermal conductivity and high bonding strength, making them the preferred ceramic substrate packaging method for high-power IGBT modules. However, when connecting AlN ceramics to metallic Cu, there is a problem that AlN ceramics are difficult to wet with liquid copper, and there is a lack of high-performance Ag-Cu-based active brazing materials that reliably connect AlN ceramics and metallic Cu. Summary of the Invention

[0004] The technical problem to be solved by this invention is to provide a multi-component composite modified Ag-Cu-X-based solder paste formulation and its preparation method. By designing a multi-component composite equimolar Co-Zn-Ni-Ti alloy formulation, and employing inert gas-protected electrode induction suspension melting gas atomization powder preparation technology, a novel Ag-Cu-Co-Zn-Ni-Ti active solder powder is developed. This significantly improves the problems of low interfacial bonding rate and low interfacial shear strength between traditional Ag-Cu-based solders and AlN ceramic substrates, thereby achieving a reliable connection between AlN ceramics and metallic Cu.

[0005] To address the aforementioned technical problems, this invention proposes a multi-component composite modified Ag-Cu-X-based active solder. The composition of the active solder, by mass parts, is as follows: Ag: 60~70; Cu: 16~20; Co: 3~5; Zn: 3~5; Sn: 3~5; Ti: 2~4; Low thermal expansion coefficient reinforcing phase: 1~3; The molar ratio of Cu, Co, Zn, and Sn is 1:1:1:1; the low thermal expansion coefficient reinforcing phase is selected from rare earth oxides, nano-Si3N4, or graphene nanosheets; the rare earth oxide is one or more of Y2O3, CeO2, La2O3, and ZrO2.

[0006] This invention also provides a method for preparing a multi-component composite modified Ag-Cu-X-based solder paste, which is prepared based on the multi-component composite modified Ag-Cu-X-based active solder, comprising the following steps: (1) Preparation of composite alloy powder: Ag powder, Cu powder, Co powder, Zn powder, Ni powder, Ti powder and low thermal expansion coefficient reinforcing phase are used as raw materials. After weighing according to the above proportion, they are alloyed by vacuum high-energy ball milling. The alloying treatment is carried out under the protective atmosphere of high-purity argon. The ball-to-material ratio is (10-15):1, the diameter of the grinding ball is 2-10 mm, the ball milling speed is 200-400 rpm, and the ball milling time is 5-10 h to obtain composite alloy powder. (2) Isostatic pressing: The composite alloy powder obtained in step (1) is subjected to isostatic pressing. The isostatic pressing pressure is 70-160 MPa and the holding time is 1-5 min to obtain the alloy billet. (3) Atmosphere-protected sintering: The alloy billet obtained in step (2) is sintered in a protective atmosphere at a temperature of 550-650℃ and a holding time of 1-3 h to obtain the induction electrode; (4) Gas atomization powder making: The induction electrode obtained in step (3) is powdered using inert gas protected electrode induction suspension melting gas atomization powder making technology. The atomization gas pressure is 2-5 MPa to obtain composite brazing filler metal powder. The composite brazing filler metal powder has an oxygen content ≤500 ppm, a purity ≥99.5%, and an average particle size D50 = 10-50 μm. (5) Preparation of active paste: The composite solder powder obtained in step (4) is mixed with the compound activator, flux and binder, and dispersed by vacuum stirring to obtain the active paste, which is the multi-component composite modified Ag-Cu-X-based solder paste; the compound activator is one of polyoxyethylene ether or fatty alcohol polyoxyethylene ether, and the binder is one of polyisobutylene or polyacrylic acid.

[0007] In the above technical solution, further, in step (4), the induction electrode is pulverized using inert gas protection electrode induction suspension molten gas atomization powder making technology as follows: the induction electrode is installed in the feeding device of the electrode induction suspension molten gas atomization powder making equipment, and inert gas is introduced after vacuuming; after the induction electrode is sent into the induction coil area, the lower end of the induction electrode is gradually melted by heating through the induction coil, and the molten alloy liquid flows freely into the atomization zone; high-pressure inert gas is sprayed out at high speed from the annular nozzle, which impacts and breaks the molten alloy liquid flow into fine droplets; the droplets fly and cool in the atomization tower to solidify into spherical powder; the powder is collected and obtained by sieving and classifying to obtain composite brazing filler metal powder.

[0008] The present invention also provides a brazing method based on the solder paste prepared above, the specific steps of which are as follows: (1) AlN ceramic surface pretreatment: The AlN ceramic surface is cleaned and dried; (2) Pre-deposition of active elements: A thin film of active metal elements is deposited on the surface of AlN ceramic to be brazed using physical vapor deposition, magnetron sputtering, or ion plating. The film thickness is 0.5–5 μm. The active metal element is one or more of Ti, Zr, Hf, and Cr. (3) Brazing: The AlN ceramic with pre-deposited active elements obtained in step (2), the active paste, and copper are assembled in a five-layer gradient structure of "Cu layer / first solder paste layer / buffer layer / second solder paste layer / AlN ceramic layer" and brazed under vacuum conditions. The buffer layer has a thermal expansion coefficient between that of the AlN ceramic and copper, forming a gradient transition in thermal expansion coefficients to alleviate stress caused by the mismatch in thermal expansion coefficients. The brazing is performed in a vacuum brazing furnace with a vacuum degree ≤ 5 × 10⁻⁶. -3 The brazing temperature was 830–900℃, and the holding time was 5–30 min. Then, the brazing effect of the joint was characterized by a brazing rate tester and a shear strength tester.

[0009] The inventive principle of this invention is as follows: Based on the high entropy effect theory and the design principle of solder composition, this invention designs a multi-component composite Co-Zn-Ni-Ti alloy formula. A novel Ag-Cu-Co-Zn-Ni-Ti active solder powder with high purity and controllable low oxygen content is prepared using inert gas protected electrode induction suspension melting gas atomization powdering technology. The corresponding Ag-Cu-Co-Zn-Ni-Ti active paste is obtained using vacuum dispersion technology. Through standard tests of interfacial wetting force and micro-solder joint strength in brazing AlN ceramic / copper, it exhibits excellent interfacial wetting and spreading ability and shear strength, which helps to achieve reliable bonding between AlN ceramic and metallic Cu.

[0010] The beneficial effects of this invention are: (1) An Ag-Cu-Co-Zn-Sn-Ti alloy powder formulation was designed, and an inert gas protected electrode induction suspension melting gas atomization powder preparation technology was proposed. Compared with the traditional melting atomization preparation technology, this technology has the characteristics of no crucible and no pollution, and can prepare Ag-Cu-Co-Zn-Ni-Ti solder powder with high sphericity and controllable particle size.

[0011] (2) A vacuum stirring technique based on the principle of shearing and rotation was used to obtain Ag-Cu-Co-Zn-Sn-Ti alloy paste. Compared with traditional Ag-Cu alloy paste, Ag-Cu-Co-Zn-Sn-Ti alloy paste has better bonding rate and superior shear strength with AlN ceramic substrate.

[0012] (3) Constructing a nano-reinforced dispersed structure: In the process of brazing, the active element Ti in the brazing filler metal undergoes an in-situ chemical reaction with the low thermal expansion coefficient reinforcing phase to generate nanoscale TiC, TiN or Ti5Si3 reinforcing particles. The nano-reinforcing particles are dispersed in the brazing seam and serve as a heterogeneous nucleation core to refine the eutectic structure.

[0013] (4) A five-layer brazing joint structure of AlN ceramic and copper based on the gradient change of thermal expansion coefficient was designed, including a copper layer, a first solder paste layer, a buffer layer (foamed Ni), a second solder paste layer and an AlN ceramic layer arranged in sequence; the thermal expansion coefficient of the buffer layer is between that of AlN ceramic and copper, which effectively relieves the stress caused by the mismatch of thermal expansion coefficients; a high-performance Ag-Cu-X-based solder paste is introduced between the AlN ceramic layer, the metallic copper layer and the buffer layer, and the solder paste is metallurgically diffused between the layers through the brazing process, forming a strong bond between the layers, which can improve the long-term service reliability of AlN / Cu devices. Attached Figure Description

[0014] Figure 1 Photographs showing the wetting and spreading of multi-component composite modified Ag-Cu-Ti based solder paste on AlN ceramic substrates and copper metal sheets. Detailed Implementation

[0015] The implementation of the present invention will be described in detail below with reference to specific embodiments. All raw materials used in the embodiments are commercially available analytical grade or high-purity reagents, wherein the purity of Ag powder is ≥99.9%, Cu powder is ≥99.9%, Co powder is ≥99.8%, Zn powder is ≥99.8%, Sn powder is ≥99.8%, and Ti powder is ≥99.8%.

[0016] Example 1 (a) Active solder formulation This embodiment provides a multi-component composite modified Ag-Cu-based active solder, composed of the following components by mass percentage: (a) Ag: 65 (b) Cu: 18 (c) Co: 4 (d) Zn: 4 (e) Sn: 4 (f) Ti: 3 (g) Y2O3 (low thermal expansion coefficient reinforcing phase): 2 The molar ratio of Cu, Co, Zn, and Sn is 1:1:1:1. The coefficient of thermal expansion of Y₂O₃ is approximately 8 × 10⁻⁶. -6 K -1 .

[0017] (II) Surface pretreatment and pre-deposition of active elements in AlN ceramics (1) The AlN ceramic sample was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 15 min in sequence to remove surface oil and impurities, and then placed in a drying oven to dry at 100℃ for 2 h.

[0018] (2) A Ti thin film was deposited on the AlN ceramic surface to be brazed using magnetron sputtering. The sputtering process parameters were: background vacuum ≤ 5 × 10⁻⁶. -4 The working gas was high-purity argon (99.999% purity), the working pressure was 0.5 Pa, the sputtering power was 150 W, the deposition time was 30 min, and the thickness of the obtained Ti film was 2 μm.

[0019] (III) Preparation of composite brazing filler metal powder (3) Weigh Ag powder, Cu powder, Co powder, Zn powder, Sn powder, Ti powder and Y2O3 powder according to the above proportions, put them into a vacuum stainless steel ball mill jar, and evacuate the jar to ≤1×10 -2 After Pa, high-purity argon gas (99.999% purity) was introduced as a protective atmosphere. A planetary high-energy ball mill was used for ball milling, with a ball-to-powder ratio of 12:1, ball diameter of 5 mm, milling speed of 300 rpm, and milling time of 8 hours. A 10-minute pause was taken every 45 minutes of milling to prevent excessive powder temperature rise. After milling, a composite alloy powder with uniform composition was obtained.

[0020] (iv) Isostatic pressing (4) The composite alloy powder obtained by ball milling is loaded into a rubber mold and pressed into shape by holding the pressure at 120 MPa for 3 minutes using a cold isostatic press to obtain an alloy billet with a certain strength.

[0021] (v) Atmosphere-protected sintering (5) The alloy billet is placed in a tubular atmosphere sintering furnace and sintered at 600℃ for 2 h with high-purity argon (purity 99.999%) as the protective atmosphere. The billet is then cooled to room temperature in the furnace to obtain the Ag-Cu-Co-Zn-Sn-Ti / Y2O3 induction electrode.

[0022] (vi) Air atomization powder production (6) The induction electrode is pulverized using inert gas protected electrode induction suspension molten gas atomization pulverization technology. The specific method is as follows: First, install the induction electrode on the feeding device of the electrode induction suspension molten gas atomization pulverization equipment, and evacuate to ≤5×10 -3 After Pa, high-purity argon and other inert gases are introduced. The induction electrode is then placed in the induction coil region, where its lower end is heated by the coil, gradually melting to form a continuous and controllable molten alloy stream. Subsequently, the molten alloy stream falls directly into the atomization chamber below under gravity, where it is impacted by a high-pressure jet of argon and other inert gases (pressure 3.5 MPa) ejected at high speed from an annular nozzle, breaking it into numerous tiny droplets. These droplets fly within the atomization tower, rapidly sphericalizing due to their surface tension, and solidifying into spherical metal powder upon cooling. Finally, the solidified powder is recovered through a separation and collection system (after sieving and grading) to produce composite brazing filler metal powder.

[0023] Analysis revealed that the obtained composite solder powder had an oxygen content of 320 ppm, a purity of 99.6%, and an average particle size D. 50 The particle size is approximately 25 μm, indicating good powder sphericity.

[0024] (vii) Preparation of active ointment (7) The composite solder powder obtained in step (6) is used as the solid phase component, accounting for 65% by mass. The liquid phase carrier is composed of a compound activator (polyoxyethylene ether, accounting for 3% of the liquid phase carrier), flux (hydrogenated rosin resin, accounting for 55% of the liquid phase carrier), binder (polyisobutylene, accounting for 20% of the liquid phase carrier), diluent (dearomatized kerosene, accounting for 20% of the liquid phase carrier) and surfactant (accounting for 2% of the liquid phase carrier). The total mass percentage of the liquid phase carrier is 35%.

[0025] The composite brazing filler powder and liquid carrier were added to a vacuum mixing tank according to the above ratio, and the vacuum was evacuated to ≤0.095MPa. The shearing and stirring device was started, with a shearing speed of 1500 rpm and a stirring time of 60 min, so that the solid particles were uniformly dispersed in the liquid carrier to obtain a uniform active paste with suitable viscosity and good thixotropy.

[0026] (viii) Brazing connection and performance evaluation (8) Assemble the AlN ceramic with pre-deposited Ti film on the surface obtained in step (2), the active paste obtained in step (7), and oxygen-free copper in a structure of "Cu / first paste layer / buffer layer / second solder paste layer / AlN ceramic", wherein the buffer layer is foamed Ni. Place it in a vacuum brazing furnace with a vacuum degree ≤5×10 -3 Pa was heated to 860°C at a rate of 10°C / min, held for 15 min, and then cooled to room temperature at a rate of 5°C / min.

[0027] (9) The wetting angle of the brazing filler metal on the AlN ceramic surface was determined by the drop test, the brazing rate was determined by the brazing rate tester, and the shear strength of the joint was determined by the shear strength tester.

[0028] Example 2 The difference between this embodiment and Embodiment 1 lies in the different active solder formulation: (a) Ag: 60 (b) Cu: 20 (c) Co: 5 (d) Zn: 5 (e) Sn: 5 (f) Ti: 2 (g) CeO2 (low thermal expansion coefficient reinforcing phase): 3 The molar ratio of Cu, Co, Zn, and Sn is 1:1:1:1.

[0029] The remaining preparation steps are the same as in Example 1. The resulting composite solder powder has an oxygen content of 350 ppm, a purity of 99.5%, and an average particle size D. 50 ≈30 μm.

[0030] Example 3 The difference between this embodiment and Embodiment 1 lies in the different active solder formulation: (a) Ag: 70 (b) Cu: 16 (c) Co: 3 (d) Zn: 3 (e) Sn: 3 (f) Ti: 4 (g) Nano-Si3N4 (low thermal expansion coefficient reinforcing phase): 1 The molar ratio of Cu, Co, Zn, and Sn is 1:1:1:1.

[0031] The remaining preparation steps were the same as in Example 1. The resulting composite solder powder had an oxygen content of 300 ppm, a purity of 99.7%, and an average particle size of D50≈20 μm.

[0032] Example 4 The difference between this embodiment and Example 1 lies in the active metal element pre-deposited on the AlN ceramic surface: in this embodiment, an ion plating method is used to deposit a Zr thin film with a thickness of 3 μm. The active solder formulation is the same as in Example 1. The remaining preparation steps are the same as in Example 1.

[0033] Comparative Example 1 This comparative example uses a traditional Ag-28Cu-3Ti (mass percentage) ternary alloy brazing filler metal, without adding Co, Zn, Sn, or low thermal expansion coefficient reinforcing phases, and without pre-depositing active elements on the AlN ceramic surface. The same gas atomization process was used to prepare the powder, and the same paste formulation and brazing process were used for AlN / Cu brazing.

[0034] Comparative Example 2 This comparative example uses Ag-Cu-Co-Zn-Sn-Ti solder (same formulation as in Example 1, but without the addition of Y2O3 low thermal expansion coefficient reinforcing phase), and does not perform pre-deposition of active elements on the AlN ceramic surface. The remaining preparation steps are the same as in Example 1.

[0035] Performance Comparison Analysis (1) Effect of activity enhancement of active metal elements: The wetting angles of Examples 1 to 4 were significantly smaller than those of Comparative Example 1, the thickness of the interfacial reaction layer was significantly greater than that of Comparative Example 1, and the shear strength was 30% to 39% higher than that of Comparative Example 1. This indicates that the equimolar ratio of Co, Zn, and Sn effectively enhances the thermodynamic activity of Ti / Zr in the alloy. The strong binding effect of Co, Zn, Sn and Cu "releases" the Ti / Zr bound by Cu, promotes the full diffusion of Ti / Zr to the AlN ceramic interface, and forms a thicker and denser activation reaction layer.

[0036] (2) The effect of the low thermal expansion coefficient reinforcing phase: The shear strength of Example 1 (containing Y2O3) was significantly higher than that of Comparative Example 2, with an increase of about 18.5%. This indicates that the addition of the Y2O3 low thermal expansion coefficient reinforcing phase effectively alleviated the thermal mismatch stress between AlN ceramic and copper, and at the same time improved the shear strength of the brazed joint through the dispersion strengthening mechanism.

[0037] (3) Effect of pre-deposition of active elements on ceramic surface: The wetting angle of Example 1 (Ti pre-deposition, 2 μm) is smaller than that of Example 4 (Zr pre-deposition, 3 μm), while the shear strength is higher than that of Example 4. This indicates that the Ti pre-deposition layer preferentially reacts with AlN ceramic to form TiN at the brazing temperature, forming a more effective chemical driving force for "reactive wetting".

[0038] (4) Comparison of the effects of different reinforcing phases: Example 3 (nano Si3N4 reinforcing phase) showed the best comprehensive performance (wetting angle ≤10°, brazing rate 97.1%, shear strength 198 MPa), which may be related to the more uniform dispersion of nano Si3N4 particles in the brazed joint structure and its lower CTE.

[0039] Table 1. Test results of brazing performance of Examples 1-4 and Comparative Examples 1-2 In summary, this invention successfully developed a multi-component composite modified Ag-Cu-based active paste material suitable for silver-based solder paste brazing. The series of modified silver-based paste materials (Examples 1-4) exhibited good wetting and spreading properties on copper sheets and ALN ceramics (see...). Figure 1 ).

[0040] Based on the comparative analysis of the data in Table 1, it can be seen that the present invention achieves a high-strength and high-reliability brazing connection between AlN ceramics and copper through the triple synergistic effect of multi-component composite modification (adding Co, Zn, and Sn in equal molar ratio to improve Ti activity), low thermal expansion coefficient to enhance phase composite (alleviating thermal mismatch stress), and pre-deposition of active elements on the ceramic surface (enhancing interfacial reaction). The overall performance is significantly better than that of traditional Ag-Cu-Ti brazing filler metal (see Table 1).

Claims

1. A multi-component composite modified Ag-Cu-X-based active solder, characterized in that, The composition of the active solder, by weight, is as follows: Ag: 60~70; Cu: 16~20; Co: 3~5; Zn: 3~5; Sn: 3~5; Ti: 2~4; Low thermal expansion coefficient reinforcing phase: 1~3; The molar ratio of Cu, Co, Zn, and Sn is 1:1:1:1; the low thermal expansion coefficient reinforcing phase is one of rare earth oxides, nano-Si3N4, or graphene nanosheets; the rare earth oxide is one or more of Y2O3, CeO2, La2O3, and ZrO2.

2. A method for preparing a multi-component composite modified Ag-Cu-X-based solder paste, characterized in that, Includes the following steps: (1) Using the multi-component composite modified Ag-Cu-X-based active solder as described in claim 1 as raw material, alloying treatment is carried out by vacuum high-energy ball milling process, wherein the alloying treatment is carried out under a protective atmosphere to obtain composite alloy powder; (2) The composite alloy powder is subjected to isostatic pressing to obtain an alloy billet; (3) The alloy billet is sintered under a protective atmosphere to obtain an induction electrode; (4) The induction electrode is powdered using inert gas protection electrode induction suspension smelting gas atomization powdering technology, with the atomization gas pressure being 2-5 MPa, to obtain composite brazing filler metal powder; (5) The composite solder powder is mixed with a compound activator, flux and binder, and then processed by vacuum stirring process to obtain a multi-component composite modified Ag-Cu-X-based solder paste; the compound activator is either polyoxyethylene ether or fatty alcohol polyoxyethylene ether, and the binder is either polyisobutylene or polyacrylic acid.

3. The method for preparing the multi-component composite modified Ag-Cu-X-based solder paste according to claim 2, characterized in that, The specific parameters of the vacuum high-energy ball milling process in step (1) are as follows: ball-to-material ratio of (10-15):1, ball diameter of 2-10 mm, ball milling speed of 200-400 rpm, and ball milling time of 5-10 h.

4. The method for preparing the multi-component composite modified Ag-Cu-X-based solder paste according to claim 2, characterized in that, The isostatic pressing process described in step (2) specifically involves an isostatic pressing pressure of 70–160 MPa and a holding time of 1–5 min.

5. The method for preparing the multi-component composite modified Ag-Cu-X-based solder paste according to claim 2, characterized in that, The sintering in step (3) specifically refers to a sintering temperature of 550-650℃ and a holding time of 1-3 h.

6. The method for preparing the multi-component composite modified Ag-Cu-X-based solder paste according to claim 2, characterized in that, In step (4), the induction electrode is prepared by inert gas protection electrode induction suspension molten gas atomization powder making technology as follows: the induction electrode is installed in the feeding device of the electrode induction suspension molten gas atomization powder making equipment, and inert gas is introduced after vacuuming; after the induction electrode is sent into the induction coil area, the lower end of the induction electrode is gradually melted by heating through the induction coil, and the molten alloy liquid flows freely into the atomization zone; high-pressure inert gas is sprayed out at high speed from the annular nozzle, which impacts and breaks the molten alloy liquid flow into fine droplets; the droplets fly and cool in the atomization tower and solidify into spherical powder; the powder is collected and obtained by sieving and classifying to obtain composite brazing filler metal powder.

7. A brazing method, characterized in that, Based on the solder paste prepared by the method described in any one of claims 2-6, the specific steps are as follows: (1) Clean and dry the surface of AlN ceramic; (2) An active metal element film is deposited on the surface of AlN ceramic by physical vapor deposition, magnetron sputtering or ion plating, and the film thickness is 0.5 to 5 μm; the active metal element is one or more of Ti, Zr, Hf and Cr; (3) The AlN ceramic with pre-deposited active elements obtained in step (2), the solder paste and copper are assembled in a five-layer gradient structure of "Cu layer / first solder paste layer / buffer layer / second solder paste layer / AlN ceramic layer" and brazed under vacuum conditions, wherein the thermal expansion coefficient of the buffer layer is between that of AlN ceramic and copper.

8. The brazing method according to claim 7, characterized in that, The brazing connection described in step (3) is performed in a vacuum brazing furnace with a vacuum degree ≤ 5 × 10⁻⁶. -3 Pa, brazing temperature is 830~900℃, and holding time is 5~30 min.