A reinforced gas shielded welding wire for high manganese austenitic cryogenic steel

The solid gas-shielded welding wire with Mn-Cr-Ni-Mo-W-RE-N composite reinforcement system solves the problems of unstable flux ratio and post-weld slag inclusion risk in the welding of high-manganese austenitic cryogenic steel, achieving high-efficiency welding performance and stability, and is suitable for on-site construction of LNG storage tanks and cryogenic pipelines.

CN123149652APending Publication Date: 2026-11-24BOXSITE WELDING TECH (JIANGSU) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611652941.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing methods for welding high-manganese austenitic low-temperature steels include unstable flux ratios, poor moisture resistance, high risk of slag inclusions after welding, coarse as-cast weld microstructure, and insufficient impact toughness at -196℃. Conventional gas-shielded welding wire is difficult to use, has a narrow process window, and poor applicability.

Method used

Solid gas-shielded welding wire with Mn-Cr-Ni-Mo-W-RE-N composite reinforcement system is prepared by vacuum smelting, electroslag remelting, hot rolling and cold drawing and electroplating copper treatment to produce austenitic weld metal microstructure, ensuring compositional uniformity and stability, reducing oxidation and hot cracking sensitivity and improving welding performance.

Benefits of technology

The weld metal exhibits significantly improved impact toughness at -196℃, a wide welding process window, minimal spatter, and strength matching that of the base material. It requires no preheating or post-weld heat treatment, making it suitable for LNG storage tank and cryogenic pipeline construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149652A_ABST
    Figure CN123149652A_ABST
Patent Text Reader

Abstract

This invention provides a reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel is a solid gas-shielded welding wire with the following chemical composition by mass percentage: C: 0.2-0.4%, Mn: 21-25%, Si: 0.2-0.5%, Cr: 3-5%, Ni: 2-4%, Mo: 0.4-0.8%, W: 0.3-0.7%, N: 0.04-0.09%, RE: 0.015-0.04%, S≤0.008%, P≤0.012%, with the balance being Fe and unavoidable impurities. The present invention provides an enhanced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel. The present invention adopts a Mn-Cr-Ni-Mo-W-RE-N composite reinforcement system, which stabilizes the austenite in the weld and has significantly better impact toughness at -196℃ than conventional high-manganese gas-shielded welding wire. The low S and low P design and rare earth desulfurization and deoxidation greatly reduce the sensitivity to solidification hot cracking, while reducing Mn oxide porosity, widening the welding process window and reducing spatter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of welding materials technology, and in particular to an enhanced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel. Background Technology

[0002] High-manganese austenitic cryogenic steel is a type of nickel-free / low-nickel cryogenic steel with a Mn content of 22-26wt%. Relying on high manganese to stabilize austenite, the Ms point is reduced to below -196℃. It is widely used to replace 9Ni steel in LNG storage tanks and cryogenic pressure vessels, with significant cost advantages.

[0003] The welding of this steel presents several challenges: high manganese content makes it highly susceptible to oxidation and burn-off; large amounts of Mn vapor and dust result in difficulties in deoxidizing the molten pool, leading to porosity and slag inclusions; the wide solidification range makes high-Mn austenitic welds highly sensitive to hot cracking; conventionally used gas-shielded welding wires produce coarse as-cast weld structures with insufficient impact toughness at -196℃, making joints prone to toughness mismatch; existing solid welding wire alloy systems are limited, relying solely on the Mn-Ni-Cr basic ratio, lacking toughening components that refine the microstructure and purify grain boundaries, resulting in a narrow process window, significant spatter, and hindering efficient gas-shielded welding in the field.

[0004] Most existing high-manganese low-temperature steel welding wires are submerged arc welding wires or ordinary solid welding wires. There are few reinforced welding wires specifically optimized for gas shielded welding conditions. Flux-cored welding wires have defects such as unstable flux ratio, poor moisture resistance, and high risk of slag inclusion after welding.

[0005] Therefore, it is necessary to provide an enhanced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel to solve the above-mentioned technical problems. Summary of the Invention

[0006] This invention provides an enhanced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, which solves the problems of unstable flux powder ratio, poor moisture resistance, and high risk of slag inclusion after welding that exist in flux-cored welding wire.

[0007] To solve the above-mentioned technical problems, the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel provided by the present invention is a solid gas-shielded welding wire with a chemical composition by mass percentage as follows: C: 0.2-0.4%, Mn: 21-25%, Si: 0.2-0.5%, Cr: 3-5%, Ni: 2-4%, Mo: 0.4-0.8%, W: 0.3-0.7%, N: 0.04-0.09%, RE: 0.015-0.04%, S≤0.008%, P≤0.012%, balance Fe and unavoidable impurities.

[0008] Preferably, the chemical composition by mass percentage is: C: 0.3%, Mn: 23.2%, Si: 0.35%, Cr: 4.1%, Ni: 3%, Mo: 0.6%, W: 0.45%, N: 0.065%, RE: 0.025%, S: 0.005%, P: 0.009%, with the balance being Fe.

[0009] Preferably, the diameter of the welding wire is φ1.0mm, φ1.2mm or φ1.6mm.

[0010] Preferably, the microstructure of the weld metal formed by the welding wire is austenite, and the area of ​​austenite in the microstructure is ≥96%, without continuous ferrite network structure.

[0011] Preferably, the mechanical properties of the weld metal formed by the welding wire meet the following requirements: yield strength Rp0.2≥400MPa, tensile strength Rm≥660MPa, elongation after fracture A≥32%, and average value of V-notch impact energy at -196℃≥65J, with a single value ≥50J.

[0012] Preferably, the preparation of the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel requires the use of a preparation method for the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, including the following steps: S1. Raw material selection: High-purity electrolytic iron, electrolytic manganese, metallic chromium, electrolytic nickel plate, ferromolybdenum, ferrotungsten, ferrizirconium, ferrochrome nitride, Ce-La mixed rare earth alloy, and industrial silicon are selected as raw materials. Mn, Zr, and rare earth burn-off compensation are set during the batching process. S2. Dual-stage smelting: First, the metal is smelted in a vacuum induction furnace. After the metal is melted, argon gas is introduced for protection. Ferrochromium nitride, electrolytic manganese, and ferrizirconium are added in sequence. The temperature is lowered to 1450-1470℃ and Ce-La mixed rare earth alloy is added. The metal is then cast to obtain a consumable electrode. Then, an argon-protected electroslag remelting is carried out using a CaF2-Al2O3-CaO ternary low-oxygen slag system. The melting rate is controlled at 4.5-6.0 kg / min. After remelting, a low-segregation steel ingot is obtained. S3. Hot rolling: Steel ingots are heated to 1120-1160℃ and held at that temperature. They are then hot rolled in multiple passes, with a final rolling temperature of 980-1040℃, and rolled into hot-rolled wire rods. S4. Hydrogen-protected solution annealing: After shot blasting to remove oxide scale, wire rod is sent to a bell-type annealing furnace, heated to 1050-1100℃ under hydrogen protection, held for 60-90 minutes, and then slowly cooled to below 300℃ before being taken out of the furnace. S5. Multi-pass cold drawing forming: Cold drawing in multiple passes, and when the cumulative deformation reaches 45%-50%, hydrogen-protected intermediate annealing is performed, and the wire is drawn to the target welding wire diameter. S6. Electroplating thin copper and dehydrogenation: After cleaning and activation, electroplat copper, controlling the copper layer thickness to 0.2-0.5μm; after rinsing, dehydrogenation is carried out at a low temperature of 160-190℃ for 40-60min. S7. Inspection, Packaging and Warehousing: Inspect the appearance and dimensions of the finished products. Qualified finished products are then wrapped in trays, vacuum-sealed for moisture protection, and stored in the warehouse.

[0013] Preferably, the diameter of the hot-rolled wire rod in step S3 is φ6.5mm.

[0014] Preferably, the single-pass cold drawing section shrinkage rate in step S5 is ≤18%.

[0015] Preferably, in step S5, the annealing temperature is 750-800℃, and the holding time is 25-40 minutes.

[0016] Compared with related technologies, the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel provided by the present invention has the following beneficial effects: This invention provides a reinforced gas-shielded welding wire for welding high-manganese austenitic cryogenic steel. The invention employs a Mn-Cr-Ni-Mo-W-RE-N composite reinforcement system, resulting in stable austenitic weld and significantly superior impact toughness at -196℃ compared to conventional high-manganese gas-shielded welding wires. Its low sulfur and phosphorus content design, along with rare earth desulfurization and deoxidation, greatly reduces solidification hot cracking sensitivity and minimizes Mn oxide porosity, resulting in a wider welding process window and less spatter. The strength and plasticity of the deposited metal match the high-manganese austenitic cryogenic steel base material, eliminating strength mismatch and preventing martensitic phase transformation embrittlement of the joint under LNG cryogenic conditions. As a solid welding wire, it has uniform composition and superior stability compared to flux-cored welding wires, offering excellent moisture resistance, smooth wire feeding, and compatibility with robotic automated gas-shielded welding. The accompanying process is simple, requiring no preheating or post-weld heat treatment, making it suitable for on-site construction of LNG storage tanks and cryogenic pipelines. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of a preferred embodiment of the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel provided by the present invention. Detailed Implementation

[0018] The present invention will be further described below with reference to the accompanying drawings and embodiments. Example

[0019] This invention provides a reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, comprising: a solid gas-shielded welding wire with a chemical composition by mass percentage as follows: C: 0.3%, Mn: 23.2%, Si: 0.35%, Cr: 4.1%, Ni: 3%, Mo: 0.6%, W: 0.45%, N: 0.065%, RE: 0.025%, S: 0.005%, P: 0.009%, balance Fe and unavoidable impurities.

[0020] The diameter of the welding wire is φ1.0mm, φ1.2mm or φ1.6mm.

[0021] The weld metal formed by the welding wire has an austenitic microstructure, with the austenitic area accounting for ≥96% and no continuous ferrite network structure.

[0022] The mechanical properties of the weld metal formed by the welding wire meet the following requirements: yield strength Rp0.2≥400MPa, tensile strength Rm≥660MPa, elongation after fracture A≥32%, and average value of V-notch impact energy at -196℃≥65J, with a single value ≥50J.

[0023] The preparation of the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel requires the use of a preparation method for the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, which includes the following steps: S1. Raw material selection: High-purity electrolytic iron, electrolytic manganese, metallic chromium, electrolytic nickel plate, ferromolybdenum, ferrotungsten, ferrizirconium, ferrochrome nitride, Ce-La mixed rare earth alloy, and industrial silicon are selected as raw materials. Mn, Zr, and rare earth burn-off compensation are set during the batching process. S2. Dual-stage smelting: First, the metal is smelted in a vacuum induction furnace. After the metal is melted, argon gas is introduced for protection. Ferrochromium nitride, electrolytic manganese, and ferrizirconia are added in sequence. The temperature is lowered to 1450℃ and Ce-La mixed rare earth alloy is added. The metal is then cast to obtain a consumable electrode. Then, an argon-protected electroslag remelting is carried out using a CaF2-Al2O3-CaO ternary low-oxygen slag system. The melting rate is controlled at 4.5 kg / min. After remelting, a low-segregation steel ingot is obtained. S3. Hot rolling: The steel ingot is heated to 1120℃ and held for a period of time. It is then hot rolled in multiple passes, with a final rolling temperature of 980℃, and rolled into a hot-rolled wire rod with a diameter of φ6.5mm. S4. Hydrogen-protected solution annealing: After shot blasting to remove oxide scale, the wire rod is sent to a bell-type annealing furnace, heated to 1050℃ under hydrogen protection and held for 70 minutes, then slowly cooled to below 300℃ before being taken out of the furnace. S5. Multi-pass cold drawing forming: Cold drawing in multiple passes, with a single pass section shrinkage rate ≤18%. When the cumulative deformation reaches 45%, hydrogen protection intermediate annealing is performed at a temperature of 750℃ for 25 minutes, and then the wire is drawn to the target welding wire diameter. S6. Electroplating thin copper and dehydrogenation: After cleaning and activation, electroplat copper, controlling the copper layer thickness to 0.2μm; after rinsing, dehydrogenation is carried out at 160℃ for 40min. S7. Inspection, Packaging and Warehousing: Inspect the appearance and dimensions of the finished products. Qualified finished products are then wrapped in trays, vacuum-sealed for moisture protection, and stored in the warehouse. Example

[0024] This invention provides a reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, comprising: a solid gas-shielded welding wire with a chemical composition by mass percentage as follows: C: 0.3%, Mn: 23%, Si: 0.3%, Cr: 3%, Ni: 4%, Mo: 0.5%, W: 0.4%, N: 0.06%, RE: 0.02%, S: 0.007%, P: 0.01%, balance Fe and unavoidable impurities.

[0025] The diameter of the welding wire is φ1.0mm, φ1.2mm or φ1.6mm.

[0026] The weld metal formed by the welding wire has an austenitic microstructure, with the austenitic area accounting for ≥96% and no continuous ferrite network structure.

[0027] The mechanical properties of the weld metal formed by the welding wire meet the following requirements: yield strength Rp0.2≥400MPa, tensile strength Rm≥660MPa, elongation after fracture A≥32%, and average value of V-notch impact energy at -196℃≥65J, with a single value ≥50J.

[0028] The preparation of the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel requires the use of a preparation method for the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, which includes the following steps: S1. Raw material selection: High-purity electrolytic iron, electrolytic manganese, metallic chromium, electrolytic nickel plate, ferromolybdenum, ferrotungsten, ferrizirconium, ferrochrome nitride, Ce-La mixed rare earth alloy, and industrial silicon are selected as raw materials. Mn, Zr, and rare earth burn-off compensation are set during the batching process. S2. Dual-stage smelting: First, the metal is smelted in a vacuum induction furnace. After the metal is melted, argon gas is introduced for protection. Ferrochromium nitride, electrolytic manganese, and ferrizirconia are added in sequence. The temperature is lowered to 1450℃ and Ce-La mixed rare earth alloy is added. The metal is then cast to obtain a consumable electrode. Then, an argon-protected electroslag remelting is carried out using a CaF2-Al2O3-CaO ternary low-oxygen slag system. The melting rate is controlled at 4.5 kg / min. After remelting, a low-segregation steel ingot is obtained. S3. Hot rolling: The steel ingot is heated to 1130℃ and held for a period of time. It is then hot rolled in multiple passes, with a final rolling temperature of 1000℃, and rolled into a hot-rolled wire rod with a diameter of φ6.5mm. S4. Hydrogen-protected solution annealing: After shot blasting to remove oxide scale, wire rod is sent to a bell-type annealing furnace, heated to 1070℃ under hydrogen protection and held for 70 minutes, then slowly cooled to below 300℃ before being taken out of the furnace. S5. Multi-pass cold drawing forming: Cold drawing in multiple passes, with a single pass section shrinkage rate ≤18%. When the cumulative deformation reaches 45%, hydrogen protection intermediate annealing is performed at a temperature of 760℃ for 30 minutes, and then the wire is drawn to the target welding wire diameter. S6. Electroplating thin copper and dehydrogenation: After cleaning and activation, electroplat copper, controlling the copper layer thickness to 0.3μm; after rinsing, dehydrogenation is carried out at 170℃ for 45min. S7. Inspection, Packaging and Warehousing: Inspect the appearance and dimensions of the finished products. Qualified finished products are then wrapped in trays, vacuum-sealed for moisture protection, and stored in the warehouse. Example

[0029] This invention provides a reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, comprising: a solid gas-shielded welding wire with a chemical composition by mass percentage as follows: C: 0.3%, Mn: 23%, Si: 0.5%, Cr: 5%, Ni: 3%, Mo: 0.6%, W: 0.5%, N: 0.09%, RE: 0.04%, S: 0.008%, P: 0.006%, balance Fe and unavoidable impurities.

[0030] The diameter of the welding wire is φ1.0mm, φ1.2mm or φ1.6mm.

[0031] The weld metal formed by the welding wire has an austenitic microstructure, with the austenitic area accounting for ≥96% and no continuous ferrite network structure.

[0032] The mechanical properties of the weld metal formed by the welding wire meet the following requirements: yield strength Rp0.2≥400MPa, tensile strength Rm≥660MPa, elongation after fracture A≥32%, and average value of V-notch impact energy at -196℃≥65J, with a single value ≥50J.

[0033] The preparation of the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel requires the use of a preparation method for the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, which includes the following steps: S1. Raw material selection: High-purity electrolytic iron, electrolytic manganese, metallic chromium, electrolytic nickel plate, ferromolybdenum, ferrotungsten, ferrizirconium, ferrochrome nitride, Ce-La mixed rare earth alloy, and industrial silicon are selected as raw materials. Mn, Zr, and rare earth burn-off compensation are set during the batching process. S2. Dual-stage smelting: First, the metallurgical process is carried out in a vacuum induction furnace. After the metallurgical process is cleared, argon gas is introduced for protection. Ferrochromium nitride, electrolytic manganese, and ferrizirconia are added in sequence. The temperature is lowered to 1470℃ and Ce-La mixed rare earth alloy is added. The metallurgical process is then cast to obtain a consumable electrode. Then, an argon-protected electroslag remelting is carried out using a CaF2-Al2O3-CaO ternary low-oxygen slag system. The melting rate is controlled at 5.0 kg / min. After remelting, a low-segregation steel ingot is obtained. S3. Hot rolling: The steel ingot is heated to 1150℃ and held for a period of time. It is then hot rolled in multiple passes, with a final rolling temperature of 980-1040℃, and rolled into a hot-rolled wire rod with a diameter of φ6.5mm. S4. Hydrogen-protected solution annealing: After shot blasting to remove oxide scale, the wire rod is sent to a bell-type annealing furnace, heated to 1100℃ under hydrogen protection and held for 60 minutes, then slowly cooled to below 300℃ before being taken out of the furnace. S5. Multi-pass cold drawing forming: Cold drawing in multiple passes, with a single pass section shrinkage rate ≤18%. When the cumulative deformation reaches 50%, intermediate annealing under hydrogen protection is performed at a temperature of 800℃ and a holding time of 30 minutes. The wire is then drawn to the target welding wire diameter. S6. Electroplating thin copper and dehydrogenation: After cleaning and activation, electroplat copper, controlling the copper layer thickness to 0.3μm; after rinsing, dehydrogenation is carried out at 190℃ for 45min. S7. Inspection, Packaging and Warehousing: Inspect the appearance and dimensions of the finished products. Qualified finished products are then wrapped in trays, vacuum-sealed for moisture protection, and stored in the warehouse. Example

[0034] This invention provides a reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, comprising: a solid gas-shielded welding wire with a chemical composition by mass percentage as follows: C: 0.4%, Mn: 25%, Si: 0.5%, Cr: 5%, Ni: 4%, Mo: 0.8%, W: 0.7%, N: 0.07%, RE: 0.03%, S: 0.005%, P: 0.007%, balance Fe and unavoidable impurities.

[0035] The diameter of the welding wire is φ1.0mm, φ1.2mm or φ1.6mm.

[0036] The weld metal formed by the welding wire has an austenitic microstructure, with the austenitic area accounting for ≥96% and no continuous ferrite network structure.

[0037] The mechanical properties of the weld metal formed by the welding wire meet the following requirements: yield strength Rp0.2≥400MPa, tensile strength Rm≥660MPa, elongation after fracture A≥32%, and average value of V-notch impact energy at -196℃≥65J, with a single value ≥50J.

[0038] The preparation of the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel requires the use of a preparation method for the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, which includes the following steps: S1. Raw material selection: High-purity electrolytic iron, electrolytic manganese, metallic chromium, electrolytic nickel plate, ferromolybdenum, ferrotungsten, ferrizirconium, ferrochrome nitride, Ce-La mixed rare earth alloy, and industrial silicon are selected as raw materials. Mn, Zr, and rare earth burn-off compensation are set during the batching process. S2. Dual-stage smelting: First, the metallurgical process is carried out in a vacuum induction furnace. After the metallurgical process is completed, argon gas is introduced for protection. Ferrochromium nitride, electrolytic manganese, and ferrizirconia are added in sequence. The temperature is lowered to 1470℃ and Ce-La mixed rare earth alloy is added. The metallurgical process is then cast to obtain a consumable electrode. Then, an argon-protected electroslag remelting is carried out using a CaF2-Al2O3-CaO ternary low-oxygen slag system. The melting rate is controlled at 6.0 kg / min. After remelting, a low-segregation steel ingot is obtained. S3. Hot rolling: The steel ingot is heated to 1160℃ and held for a period of time. It is then hot rolled in multiple passes, with a final rolling temperature of 1040℃, and rolled into a hot-rolled wire rod with a diameter of φ6.5mm. S4. Hydrogen-protected solution annealing: After shot blasting to remove oxide scale, the wire rod is sent to a bell-type annealing furnace, heated to 1100℃ under hydrogen protection and held for 90 minutes, then slowly cooled to below 300℃ before being taken out of the furnace. S5. Multi-pass cold drawing forming: Cold drawing in multiple passes, with a single pass section shrinkage rate ≤18%. When the cumulative deformation reaches 50%, hydrogen protection intermediate annealing is performed at a temperature of 800℃ for 35 minutes, and then the wire is drawn to the target welding wire diameter. S6. Electroplating thin copper and dehydrogenation: After cleaning and activation, electroplat copper, controlling the copper layer thickness to 0.5μm; after rinsing, dehydrogenation is carried out at 190℃ for 60min. S7. Inspection, Packaging and Warehousing: Inspect the appearance and dimensions of the finished products. Qualified finished products are then wrapped in trays, vacuum-sealed for moisture protection, and stored in the warehouse.

[0039] Compared with related technologies, the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel provided by the present invention has the following beneficial effects: This invention employs a Mn-Cr-Ni-Mo-W-RE-N composite reinforcement system, resulting in stable austenitic weld and significantly superior impact toughness at -196℃ compared to conventional high-manganese gas-shielded welding wire. The low S and P design, along with rare earth desulfurization and deoxidation, significantly reduces solidification hot cracking sensitivity while minimizing Mn oxidation porosity, widening the welding process window and reducing spatter. The strength and plasticity of the deposited metal match the high-manganese austenitic cryogenic steel base material, eliminating strength mismatch and preventing martensitic phase transformation embrittlement of the joint under LNG cryogenic conditions. The solid welding wire has uniform composition and superior stability compared to flux-cored welding wire, offering excellent moisture resistance, smooth wire feeding, and compatibility with robotic automated gas-shielded welding. The accompanying process is simple, requiring no preheating or post-weld heat treatment, making it suitable for on-site construction of LNG storage tanks and cryogenic pipelines.

[0040] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, characterized in that, This is a solid gas-shielded welding wire with the following chemical composition by mass percentage: C: 0.2-0.4%, Mn: 21-25%, Si: 0.2-0.5%, Cr: 3-5%, Ni: 2-4%, Mo: 0.4-0.8%, W: 0.3-0.7%, N: 0.04-0.09%, RE: 0.015-0.04%, S≤0.008%, P≤0.012%, balance Fe and unavoidable impurities.

2. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, characterized in that, The chemical composition by mass percentage is as follows: C: 0.3%, Mn: 23.2%, Si: 0.35%, Cr: 4.1%, Ni: 3%, Mo: 0.6%, W: 0.45%, N: 0.065%, RE: 0.025%, S: 0.005%, P: 0.009%, balance Fe.

3. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, characterized in that, The diameter of the welding wire is φ1.0mm, φ1.2mm or φ1.6mm.

4. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, characterized in that, The weld metal formed by the welding wire has an austenitic microstructure, with the austenitic area accounting for ≥96% and no continuous ferrite network structure.

5. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, characterized in that, The mechanical properties of the weld metal formed by the welding wire meet the following requirements: yield strength Rp0.2≥400MPa, tensile strength Rm≥660MPa, elongation after fracture A≥32%, and average value of V-notch impact energy at -196℃≥65J, with a single value ≥50J.

6. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, wherein the preparation of the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel requires the use of a preparation method for the reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel, characterized in that... Includes the following steps: S1. Raw material selection: High-purity electrolytic iron, electrolytic manganese, metallic chromium, electrolytic nickel plate, ferromolybdenum, ferrotungsten, ferrizirconium, ferrochrome nitride, Ce-La mixed rare earth alloy, and industrial silicon are selected as raw materials. Mn, Zr, and rare earth burn-off compensation are set during the batching process. S2. Dual-stage smelting: First, the metal is smelted in a vacuum induction furnace. After the metal is melted, argon gas is introduced for protection. Ferrochromium nitride, electrolytic manganese, and ferrizirconium are added in sequence. The temperature is lowered to 1450-1470℃ and Ce-La mixed rare earth alloy is added. The metal is then cast to obtain a consumable electrode. Then, an argon-protected electroslag remelting is carried out using a CaF2-Al2O3-CaO ternary low-oxygen slag system. The melting rate is controlled at 4.5-6.0 kg / min. After remelting, a low-segregation steel ingot is obtained. S3. Hot rolling: Steel ingots are heated to 1120-1160℃ and held at that temperature. They are then hot rolled in multiple passes, with a final rolling temperature of 980-1040℃, and rolled into hot-rolled wire rods. S4. Hydrogen-protected solution annealing: After shot blasting to remove oxide scale, wire rod is sent to a bell-type annealing furnace, heated to 1050-1100℃ under hydrogen protection, held for 60-90 minutes, and then slowly cooled to below 300℃ before being taken out of the furnace. S5. Multi-pass cold drawing forming: Cold drawing in multiple passes, and when the cumulative deformation reaches 45%-50%, hydrogen-protected intermediate annealing is performed, and the wire is drawn to the target welding wire diameter. S6. Electroplating thin copper and dehydrogenation: After cleaning and activation, electroplat copper, controlling the copper layer thickness to 0.2-0.5μm; after rinsing, dehydrogenation is carried out at a low temperature of 160-190℃ for 40-60min. S7. Inspection, Packaging and Warehousing: Inspect the appearance and dimensions of the finished products. Qualified finished products are then wrapped in trays, vacuum-sealed for moisture protection, and stored in the warehouse.

7. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, characterized in that, In step S3, the diameter of the hot-rolled wire rod is φ6.5mm.

8. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, characterized in that, In step S5, the single-pass cold drawing section shrinkage rate is ≤18%.

9. The reinforced gas-shielded welding wire for welding high-manganese austenitic low-temperature steel according to claim 1, characterized in that, In step S5, the annealing temperature is 750-800℃, and the holding time is 25-40 minutes.