A nickel-based alloy welding rod

By combining a specific ratio of electrode coating and nickel-based alloy core, the problems of poor molten pool fluidity and poor welding process performance of nickel-based alloy welding materials are solved, resulting in good weld formation and arc stability, which meets the requirements for nuclear power equipment manufacturing.

CN123149653APending Publication Date: 2026-11-24CHINA NUCLEAR POWER ENGINEERING COMPANY LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611654725.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Nickel-based alloy welding materials have poor molten pool fluidity, poor welding process performance, and poor weld formation, and are prone to defects such as slag inclusions.

Method used

Welding electrodes are prepared by using a specific ratio of electrode coating components, including TiO₂, NaF, CaCO₃, NiNb alloy, etc., in combination with a nickel-based alloy core, through mixing, pressure coating and staged baking processes to form a dense coating, which improves the fluidity of the molten pool and the stability of the arc.

Benefits of technology

Without increasing the welding current, improve the weld formation quality, reduce the tendency of slag inclusions, enhance welding operability and arc stability, and meet the manufacturing standards for nuclear power equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149653A_ABST
    Figure CN123149653A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of welding materials and discloses a nickel-based alloy welding electrode, comprising a nickel-based alloy core and a flux coating covering the surface of the core. The solid components of the flux coating, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities. The nickel-based alloy welding electrode of this invention possesses excellent welding process performance and can improve the fluidity of the molten pool and the quality of the weld formation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of welding materials technology, and specifically relates to a nickel-based alloy welding electrode. Background Technology

[0002] Nickel-based alloy materials are widely used in the manufacture of equipment such as reactor pressure vessels and steam generators in nuclear power plants. Nickel-based alloy welding materials have low thermal conductivity and high surface tension between the liquid metal and slag in the molten state, resulting in relatively insufficient spreadability and fluidity. This can easily lead to defects such as poor weld formation, undercut, porosity, slag inclusions, and impurities in the deposited metal.

[0003] To improve the fluidity of the weld pool, existing technologies often increase the welding current. However, increasing the welding current leads to increased loss of alloying elements, reduced arc stability, accelerated temperature rise of the electrode coating, worsened welding operability, increased spatter, and deteriorated weld formation. Another approach uses alkaline slag systems. These electrodes require short-arc welding to maintain arc stability and weld pool protection, but when the current is too low or the operation is unstable, electrode sticking and arc interruption are likely to occur.

[0004] 690 series nickel-based alloys have a high chromium content and good resistance to high-temperature corrosion, making them widely used in the manufacturing of key equipment for nuclear power plants. In addition to meeting the nuclear power equipment manufacturing standards, the 690 series nickel-based alloy welding materials used in nuclear power plants must also have good welding process performance. Summary of the Invention

[0005] In view of the above problems, this application provides a nickel-based alloy welding electrode that solves at least one of the following problems in existing nickel-based alloy welding materials: poor molten pool fluidity, poor welding process performance, poor weld formation, and slag inclusions.

[0006] On one hand, the present invention provides a welding electrode coating, wherein the solid components of the coating, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities.

[0007] Furthermore, the mass percentage of Ni in the NiNb alloy is 25%–30%, and the mass percentage of Nb is 65%–70%.

[0008] On the other hand, the present invention also provides a nickel-based alloy welding electrode, comprising a nickel-based alloy core and a coating covering the surface of the core.

[0009] Further, the nickel-based alloy welding core composition, by mass percentage, includes: C≤0.015%, Mn: 0.6%~1.0%, Si≤0.10%, Cr: 29.0%~31.0%, Fe: 9.0%~10.0%, Ti: 0.2%~0.3%, Al: 0.08%~0.15%, Nb: 0.7%~1.0%, Ni≥55%, Cu≤0.10%, N≤0.008%, S≤0.002%, P≤0.005%, Mo: 0.3%~0.5%.

[0010] Preferably, the nickel-based alloy core composition, by mass percentage, includes: C: 0.010%–0.014%, Mn: 0.65%–0.88%, Si: 0.018%–0.05%, Cr: 29.93%–30.27%, Fe: 9.67%–9.92%, Ti: 0.22%–0.28%, Al: 0.087%–0.13%, Nb: 0.74%–0.93%, Ni: 57 .65%~58.43%, Cu: 0.0023%~0.0064%, N: 0.0031%~0.0066%, S: 0.0011%~0.0019%, P: 0.0025%~ 0.0039%, Mo: 0.32% to 0.48%, V: 0.0068% to 0.013%, Co: 0.0059% to 0.0069%, Ta: 0.0010% to 0.0025%.

[0011] On the other hand, the present invention also provides a method for preparing nickel-based alloy welding electrodes, comprising the following steps: The raw materials of the solid components of the coating are mixed evenly, and an alkali metal silicate binder is added. After stirring evenly, the mixture is sent to a pressing machine for pressing and coating, so that the coating is wrapped on the surface of the nickel-based alloy welding core. The welding rod is then baked to produce the welding rod.

[0012] The solid components, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities.

[0013] Preferably, the mass of the alkali metal silicate binder is 20% to 25% of the mass of the solid component; and / or the alkali metal silicate binder is potassium sodium water glass; and / or the baking includes two stages: low-temperature baking and high-temperature baking, wherein the low-temperature baking is 60℃ to 100℃ for 4 to 6 hours; and the high-temperature baking is 330℃ to 370℃ for 1.5 to 3 hours.

[0014] Preferably, the stirring time after adding the alkali metal silicate binder is 12 min to 30 min; and / or the pressing pressure of the pressing machine is 100 MPa to 120 MPa.

[0015] Further, the nickel-based alloy welding core composition, by mass percentage, includes: C≤0.015%, Mn: 0.6%~1.0%, Si≤0.10%, Cr: 29.0%~31.0%, Fe: 9.0%~10.0%, Ti: 0.2%~0.3%, Al: 0.08%~0.15%, Nb: 0.7%~1.0%, Ni≥55%, Cu≤0.10%, N≤0.008%, S≤0.002%, P≤0.005%, Mo: 0.3%~0.5%.

[0016] Preferably, the nickel-based alloy core composition, by mass percentage, includes: C: 0.010%–0.014%, Mn: 0.65%–0.88%, Si: 0.018%–0.05%, Cr: 29.93%–30.27%, Fe: 9.67%–9.92%, Ti: 0.22%–0.28%, Al: 0.087%–0.13%, Nb: 0.74%–0.93%, Ni: 57 .65%~58.43%, Cu: 0.0023%~0.0064%, N: 0.0031%~0.0066%, S: 0.0011%~0.0019%, P: 0.0025%~ 0.0039%, Mo: 0.32% to 0.48%, V: 0.0068% to 0.013%, Co: 0.0059% to 0.0069%, Ta: 0.0010% to 0.0025%.

[0017] Compared with the prior art, the present invention has at least one of the following beneficial effects: 1. The electrode coating provided by the present invention, through the synergistic proportion of functional components such as NaF, TiO2, SrCO3 and NiNb alloy in the solid composition, helps to reduce the surface tension of the molten pool, adjust the viscosity and surface tension of the slag, improve the fluidity and spreading of the molten pool during nickel-based alloy welding, and make the electrode have the comprehensive process characteristics of clear molten pool in alkaline slag system and good arc stability in acidic slag system.

[0018] 2. The nickel-based alloy welding electrode provided by the present invention, through the combination of nickel-based alloy welding core and the above-mentioned coating, helps to improve the weld formation quality without increasing the welding current, reduces poor weld formation and slag inclusion tendency caused by insufficient molten pool fluidity, and the slag shell coverage is uniform, slag removal is easy, and it has good adaptability to AC and DC power supplies.

[0019] 3. The nickel-based alloy welding electrode preparation method provided by the present invention, through the mixing, pressing and coating and staged baking process of solid components and alkali metal silicate binder, helps to form a dense and uniform coating on the surface of the welding core, and maintains the stability of the electrode coating strength and welding process performance. Attached Figure Description

[0020] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 This is a diagram showing the slag coverage effect of the welding electrode of Comparative Example 1 of the present invention when flat welding is performed at a welding current of 120A; Figure 2 This is a diagram showing the slag coverage effect of the welding electrode in Embodiment 1 of the present invention when flat-welded at a welding current of 120A; Figure 3 This is a diagram showing the weld formation effect of the welding electrode of Comparative Example 1 of the present invention when flat welding is performed at a welding current of 120A. Figure 4 This is a diagram showing the weld formation effect of the welding electrode in Embodiment 1 of the present invention when flat welding is performed at a welding current of 120A; Figure 5 This is a weld formation diagram of a vertically upward weld using a welding electrode in Embodiment 1 of the present invention, with a welding current of 120A. Detailed Implementation

[0021] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0023] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0024] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0025] On one hand, a specific embodiment of the present invention provides a welding electrode coating, wherein the solid components of the coating, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities.

[0026] Furthermore, the mass percentage of Ni in the NiNb alloy is 25%–30%, and the mass percentage of Nb is 65%–70%.

[0027] In some embodiments, using NiNb alloy instead of single Ni powder or Nb powder can simultaneously achieve the strengthening effect of Nb element and the transitional supplementation effect of Ni element during the welding metallurgy process, which helps to compensate for the oxidation loss of Ni during welding and improve the comprehensive mechanical properties of the deposited metal.

[0028] Preferably, the NiNb alloy contains 30% Ni by mass and 70% Nb by mass.

[0029] In some embodiments, further limiting the mass ratio of Ni to Nb within the above range can provide an appropriate amount of Ni to compensate for welding burn-off while maintaining effective strengthening by Nb, which is beneficial for the stable control of the chemical composition and mechanical properties of the deposited metal.

[0030] Furthermore, the coating is formed using an alkali metal silicate binder.

[0031] Preferably, the alkali metal silicate binder is potassium sodium water glass.

[0032] Using potassium sodium water glass as a binder helps to uniformly wet and bond the solid coating components, enabling the coating to form a dense coating structure after pressure coating and baking, thus ensuring the strength of the electrode coating and the welding process performance.

[0033] Preferably, the potassium-sodium water glass is potassium-sodium water glass with a strength of 38.5-39°Be″ at 20°C.

[0034] In some embodiments, potassium sodium water glass with a viscosity of 38.5°Be″~39°Be″ at 20°C is used. Its viscosity is conducive to the uniform mixing and pressing of solid powder and binder, and helps the coating to form a uniform coating layer on the core surface, reducing eccentricity and surface defects during the pressing process.

[0035] The following details the role and dosage selection of each solid component in the coating of the nickel-based alloy welding electrode used in this invention: TiO2's main functions are to stabilize the electric arc and form slag. It can regulate the melting point, viscosity, surface tension, and fluidity of the slag, improve weld formation, and reduce spatter. In this invention, the addition of TiO2 plays a crucial role in weld formation and arc stability. The TiO2 content in the flux coating is controlled at 16%–22%.

[0036] NaF: Its main functions are slag formation and hydrogen removal. It also helps reduce the surface tension of liquid metal, improve the fluidity of the molten pool, lower the melting temperature of the coating, make the weld bead more aesthetically pleasing, improve weld quality, and reduce porosity. The NaF content in the coating is controlled between 26% and 32%.

[0037] CaCO3's main function is to decompose into CaO and CO2 under the heat of the electric arc. It is a commonly used slag-forming and gas-generating material in welding electrode manufacturing. It can increase the basicity of the slag, stabilize the arc, refine the molten droplets, increase the interfacial tension between the slag and the metal, improve slag removal, and has good desulfurization capabilities. CO2 can reduce the hydrogen partial pressure in the arc atmosphere, reduce the hydrogen content in the weld, and prevent nitrogen from the air from entering the arc. The CaCO3 content in the coating is controlled at 10%–14%.

[0038] Potassium feldspar: Primarily used for slag formation, arc stabilization, and improving re-arc re-ignition performance. Due to its high SiO2 content, it increases arc voltage during welding, refines molten droplets, and improves electrode melting speed. However, it can also cause Si reversion in the weld, and the higher Al2O3 content increases slag viscosity, making slag removal difficult and resulting in inclusions in the weld, affecting its internal quality. Therefore, the potassium feldspar content in the coating should be controlled between 6% and 8%.

[0039] NiNb alloy: Compared to pure Ni and pure Nb, NiNb alloy is an alloy system with Ni as the base material and Nb added for strengthening. Its role in electrode coating is twofold: firstly, to improve the overall performance of the weld metal through the addition of Nb; and secondly, to act as a transition Ni, compensating for the Ni loss due to oxidation during the welding process. Adding NiNb alloy improves the mechanical properties of the weld metal compared to adding pure Nb. The NiNb alloy content in the coating is controlled at 5%–7%.

[0040] Cr: A transition element to compensate for Cr loss due to deoxidation, oxidation, insufficient transition time, and other factors such as splashing and evaporation. The Cr content in the coating is controlled at 3%–5%.

[0041] Mn's main function is as a transition element and deoxidizer. Increasing the Mn content in nickel-based welds refines the weld microstructure and simultaneously improves the material's high-temperature strength, ductility, and crack resistance. Mn also has a strong affinity for S and O, acting as a S-fixing agent and forming MnO. The Mn content in the flux coating is controlled between 8% and 12%.

[0042] Na2CO3: Used as a lubricant in the coating, but often contains small amounts of chlorides, carbonates, and other impurities. It is highly hygroscopic, easily causing the welding electrode to absorb moisture severely and turn yellow. Therefore, the Na2CO3 content in the coating should be controlled between 0.2% and 0.5%.

[0043] Polytetrafluoroethylene (C2F4): Used as a humectant in the flux coating. During the mixing process with water glass, nickel-based alloy welding electrode powder dries rapidly, easily agglomerating and hardening, increasing the difficulty of electrode coating and affecting electrode eccentricity. Excessive PTFE content in the flux coating leads to poor arc stability and increased spatter. Therefore, the PTFE content in the flux coating is controlled between 0.8% and 1%.

[0044] Sodium carboxymethyl cellulose (CMC): Its main function is to increase the plasticity of the coating, which is beneficial for the stability of eccentricity during the electrode coating process. When the CMC content in the coating is too high, it will cause indentations and burrs on the electrode surface, and the coating will become brittle. Therefore, the sodium carboxymethyl cellulose (CMC) content in the coating should be controlled between 0.4% and 0.6%.

[0045] SrCO3: Due to its high decomposition temperature, adding it to the flux coating helps adjust the physical properties of the slag during welding, improves slag removal, and suppresses spatter. The SrCO3 content in the flux coating should be controlled between 7% and 10%.

[0046] On the other hand, a specific embodiment of the present invention also provides a nickel-based alloy welding electrode, comprising a nickel-based alloy welding core and a coating covering the surface of the welding core.

[0047] The welding electrode, through the combination of the core and the coating, can improve the fluidity and spreadability of the molten pool during welding, which helps to obtain a well-formed weld with fewer defects, while taking into account the stability of the welding arc and the performance of the operation process.

[0048] Specifically, the solid components of the coating, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities.

[0049] Further, the nickel-based alloy welding core composition, by mass percentage, includes: C≤0.015%, Mn: 0.6%~1.0%, Si≤0.10%, Cr: 29.0%~31.0%, Fe: 9.0%~10.0%, Ti: 0.2%~0.3%, Al: 0.08%~0.15%, Nb: 0.7%~1.0%, Ni≥55%, Cu≤0.10%, N≤0.008%, S≤0.002%, P≤0.005%, Mo: 0.3%~0.5%.

[0050] The above composition design ensures that the chemical composition of the weld core deposited metal matches that of the CHN690HR1 series alloy base material, which helps to ensure that the high-temperature corrosion resistance and mechanical properties of the weld metal meet the requirements of relevant standards for nuclear power equipment manufacturing.

[0051] Preferably, the nickel-based alloy core composition, by mass percentage, includes: C: 0.010%–0.014%, Mn: 0.65%–0.88%, Si: 0.018%–0.05%, Cr: 29.93%–30.27%, Fe: 9.67%–9.92%, Ti: 0.22%–0.28%, Al: 0.087%–0.13%, Nb: 0.74%–0.93%, Ni: 57 .65%~58.43%, Cu: 0.0023%~0.0064%, N: 0.0031%~0.0066%, S: 0.0011%~0.0019%, P: 0.0025%~ 0.0039%, Mo: 0.32% to 0.48%, V: 0.0068% to 0.013%, Co: 0.0059% to 0.0069%, Ta: 0.0010% to 0.0025%.

[0052] The above-mentioned preferred composition range can further control the fluctuation of the chemical composition of the welding core, reduce the deviation of the deposited metal performance caused by element burn-off and unstable transition during the welding process, and help to obtain a weld with uniform composition and stable performance.

[0053] In some embodiments, the addition of trace elements such as V, Co, and Ta helps to refine the weld microstructure and improve the welding metallurgical properties, which has a positive effect on improving the comprehensive mechanical properties of the deposited metal and the quality of the weld joint.

[0054] On the other hand, a specific embodiment of the present invention also provides a method for preparing a nickel-based alloy welding electrode, comprising the following steps: The solid components of the coating are mixed evenly, an alkali metal silicate binder is added, and after stirring evenly, the mixture is sent to a pressing machine for pressing and coating. The coating is then wrapped around the surface of the nickel-based alloy welding core and baked to produce a welding rod. The solid components of the coating, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities.

[0055] The above preparation method, through the reasonable ratio of solid components and the combination of alkali metal silicate binder, helps the powder to form a uniform and plastic agglomerate. After pressure coating and baking, a dense and firmly adhered coating can be formed on the surface of the welding core, thereby giving the welding electrode good welding process performance and stable arc characteristics.

[0056] Preferably, the Cr and Mn elements in the coating can be added in the form of ferrochrome powder and ferromanganese powder, respectively. Their main functions are to transition alloying elements, deoxidize and refine the weld structure.

[0057] Preferably, the mass of the alkali metal silicate binder is 20% to 25% of the mass of the solid component; and / or the alkali metal silicate binder is potassium sodium water glass; and / or the baking includes two stages: low-temperature baking and high-temperature baking, wherein the low-temperature baking is 60℃ to 100℃ for 4 to 6 hours; and the high-temperature baking is 330℃ to 370℃ for 1.5 to 3 hours.

[0058] In some embodiments, the amount of binder is in the range of 20% to 25%, which helps to give the coating appropriate plasticity and coating properties, and is beneficial to the formation of coating strength after pressure coating and baking. Using potassium sodium water glass as a binder helps to uniformly wet and bond the solid components. Staged baking at low temperature and high temperature is beneficial to the gradual evaporation of moisture and organic matter in the coating, reducing the risk of coating cracking and falling off, and improving the quality of the finished welding electrode.

[0059] Preferably, the stirring time after adding the alkali metal silicate binder is 12 min to 30 min; and / or the pressing pressure of the pressing machine is 100 MPa to 120 MPa.

[0060] In some embodiments, an appropriate stirring time helps to ensure uniform mixing of the solid components and the binder, prevents powder agglomeration, and improves the uniformity of pressure coating; the above-mentioned pressure range is conducive to the formation of a dense and uniform coating layer on the core surface, which helps to reduce electrode eccentricity and surface defects, and improves the bonding strength between the coating and the core.

[0061] Further, the nickel-based alloy welding core composition, by mass percentage, includes: C≤0.015%, Mn: 0.6%~1.0%, Si≤0.10%, Cr: 29.0%~31.0%, Fe: 9.0%~10.0%, Ti: 0.2%~0.3%, Al: 0.08%~0.15%, Nb: 0.7%~1.0%, Ni≥55%, Cu≤0.10%, N≤0.008%, S≤0.002%, P≤0.005%, Mo: 0.3%~0.5%.

[0062] Preferably, the nickel-based alloy core composition, by mass percentage, includes: C: 0.010%–0.014%, Mn: 0.65%–0.88%, Si: 0.018%–0.05%, Cr: 29.93%–30.27%, Fe: 9.67%–9.92%, Ti: 0.22%–0.28%, Al: 0.087%–0.13%, Nb: 0.74%–0.93%, Ni: 57 .65%~58.43%, Cu: 0.0023%~0.0064%, N: 0.0031%~0.0066%, S: 0.0011%~0.0019%, P: 0.0025%~ 0.0039%, Mo: 0.32% to 0.48%, V: 0.0068% to 0.013%, Co: 0.0059% to 0.0069%, Ta: 0.0010% to 0.0025%.

[0063] In summary, the electrode coating provided by this invention, through the synergistic proportioning of functional components such as NaF, TiO2, SrCO3, and NiNb alloy in the solid composition, helps to reduce the surface tension of the molten pool, adjust the viscosity and surface tension of the slag, and improve the molten pool fluidity and spreading properties during nickel-based alloy welding. This allows the electrode to combine the advantages of a clear molten pool in alkaline slag systems and good arc stability in acidic slag systems. The nickel-based alloy welding electrode provided by this invention, through the combination of the nickel-based alloy core and the aforementioned coating, helps to improve weld formation quality without increasing the welding current, reducing poor weld formation and slag inclusion tendency caused by insufficient molten pool fluidity. Furthermore, it provides uniform slag coverage, easy slag removal, and good adaptability to both AC and DC power supplies.

[0064] The nickel-based alloy welding electrode of the present invention will be described below with reference to specific embodiments.

[0065] Example 1 This embodiment provides a nickel-based alloy welding electrode.

[0066] The solid components of the electrode coating in this embodiment, by mass percentage, include: TiO2: 22%, NaF: 30%, CaCO3: 10%, potassium feldspar: 8%, NiNb alloy: 5%, Cr: 4%, Mn: 9%, Na2CO3: 0.4%, polytetrafluoroethylene (C2F4): 1%, sodium carboxymethyl cellulose (CMC): 0.6%, and SrCO3: 10%, as shown in Table 1.

[0067] The chemical composition of the nickel-based alloy core of the welding electrode in this embodiment, by mass percentage, includes: C: 0.012%, Mn: 0.82%, Si: 0.05%, Cr: 29.93%, Fe: 9.83%, Ti: 0.27%, Al: 0.087%, Nb: 0.9%, Ni: 57.65%, Cu: 0.0053%, N: 0.0039%, S: 0.0011%, P: 0.0025%, Mo: 0.42%, V: 0.0068%, Co: 0.0063%, Ta: 0.0021%.

[0068] The preparation process of nickel-based alloy welding electrodes is as follows: After the raw materials of the solid components of the flux coating are mixed evenly, potassium sodium water glass at 38.5°Be″~39°Be″ at 20℃ is added at 22% by mass of the solid components. After stirring for 15 minutes, the mixture is fed into a pressing machine with a pressing pressure of 110MPa to coat the surface of the nickel-based alloy welding core. The welding electrode is then produced by low-temperature baking and high-temperature baking. The low-temperature baking is 60℃~100℃ / 4h~6h; the high-temperature baking is 330℃~370℃ / 1.5h~3h.

[0069] The welding electrode prepared by the above method has excellent appearance quality and the electrode specification is φ4.0mm.

[0070] Weld the above-mentioned welding rods under the following welding conditions: welding current 120A~135A, welding voltage 22V~32V, welding speed 12cm / min~20cm / min.

[0071] The chemical composition of the welded metal was analyzed, and the results were as follows: C: 0.033%, Mn: 2.84%, Si: 0.31%, Cr: 28.76%, Fe: 10.88%, Ti: 0.068%, Al: 0.03%, Nb: 1.45%, Cu: 0.0052%, N: 0.011%, S: 0.0068%, P: 0.0013%, Mo: 0.074%, V: 0.012%, Co: 0.0066%, Ta: 0.0015%, Ni balance.

[0072] The mechanical properties and impact properties of the weld metal are shown in Tables 2 and 3, respectively.

[0073] Example 2 This embodiment provides a nickel-based alloy welding electrode, the solid components of which, by mass percentage, include: TiO2: 16%, NaF: 32%, CaCO3: 14%, potassium feldspar: 6%, NiNb alloy: 7%, Cr: 5%, Mn: 10%, Na2CO3: 0.2%, polytetrafluoroethylene: 0.8%, sodium carboxymethyl cellulose: 0.5%, and SrCO3: 8.5%.

[0074] The chemical composition, preparation process, welding process parameters, and performance testing methods of the welding core are the same as those in Example 1.

[0075] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0076] Example 3 This embodiment provides a nickel-based alloy welding electrode, the solid components of which, by mass percentage, include: TiO2: 20%, NaF: 28%, CaCO3: 12%, potassium feldspar: 8%, NiNb alloy: 6%, Cr: 5%, Mn: 12%, Na2CO3: 0.5%, polytetrafluoroethylene: 1%, sodium carboxymethyl cellulose: 0.5%, and SrCO3: 7%.

[0077] The chemical composition, preparation process, welding process parameters, and performance testing methods of the welding core are the same as those in Example 1.

[0078] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0079] Example 4 This embodiment provides a nickel-based alloy welding electrode, the solid components of which, by mass percentage, include: TiO2: 22%, NaF: 30%, CaCO3: 10%, potassium feldspar: 8%, NiNb alloy: 5%, Cr: 4%, Mn: 9%, Na2CO3: 0.6%, polytetrafluoroethylene: 1%, sodium carboxymethyl cellulose: 0.4%, and SrCO3: 10%.

[0080] The chemical composition, preparation process, welding process parameters, and performance testing methods of the welding core are the same as those in Example 1.

[0081] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0082] Example 5 This embodiment provides a nickel-based alloy welding electrode, the solid components of which, by mass percentage, include: TiO2: 18%, NaF: 32%, CaCO3: 14%, potassium feldspar: 6%, NiNb alloy: 7%, Cr: 5%, Mn: 8%, Na2CO3: 0.2%, polytetrafluoroethylene: 0.8%, sodium carboxymethyl cellulose: 0.5%, and SrCO3: 8.5%.

[0083] The chemical composition, preparation process, welding process parameters, and performance testing methods of the welding core are the same as those in Example 1.

[0084] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0085] Comparative Example 1 The difference from Example 1 is that the solid component of the coating in this comparative example does not contain TiO2. The solid component of the coating, by mass percentage, includes: NaF: 30%, CaCO3: 32%, potassium feldspar: 8%, NiNb alloy: 5%, Cr: 4%, Mn: 9%, Na2CO3: 0.4%, polytetrafluoroethylene (C2F4): 1%, sodium carboxymethyl cellulose (CMC): 0.6%, and SrCO3: 10%.

[0086] The chemical composition, preparation process, and welding process parameters of the welding core are the same as those in Example 1.

[0087] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0088] Comparative Example 2 The difference from Example 2 is that Nb iron is used instead of NiNb alloy in this comparative example, and its coating solid components, by mass percentage, include: TiO2: 16%, NaF: 32%, CaCO3: 14%, potassium feldspar: 6%, Nb iron: 7%, Cr: 5%, Mn: 10%, Na2CO3: 0.2%, polytetrafluoroethylene (C2F4): 0.8%, sodium carboxymethyl cellulose (CMC): 0.5%, and SrCO3: 8.5%.

[0089] The chemical composition, preparation process, and welding process parameters of the welding core are the same as those in Example 1.

[0090] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0091] Comparative Example 3 The difference from Example 3 is that sodium alginate is used instead of polytetrafluoroethylene in this comparative example, and the solid components of its coating, by mass percentage, include: TiO2: 20%, NaF: 28%, CaCO3: 12%, potassium feldspar: 8%, NiNb alloy: 6%, Cr: 5%, Mn: 12%, Na2CO3: 0.5%, sodium alginate: 1%, sodium carboxymethyl cellulose: 0.5%, SrCO3: 7%.

[0092] The chemical composition of the welding core is the same as that in Example 3.

[0093] Because sodium alginate has lower moisturizing properties than polytetrafluoroethylene (PTFE), the powder dries faster after being added to potassium sodium water glass. During stirring, it tends to clump and harden, reducing powder uniformity and making it difficult to apply the coating according to the process parameters of Example 3. Even with shortened stirring time and increased coating pressure, the electrode appearance remains rough, increasing the difficulty of controlling eccentricity. During welding, phenomena such as incomplete melting of the flux coating, flux peeling, and uneven slag coverage occur, resulting in poorer weld pool fluidity and weld formation compared to Example 3.

[0094] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0095] Comparative Example 4 The difference from Example 4 is that this comparative example reduces the NiNb alloy content, and its coating solid components, by mass percentage, include: TiO2: 22%, NaF: 30%, CaCO3: 12%, potassium feldspar: 8%, NiNb alloy: 3%, Cr: 4%, Mn: 9%, Na2CO3: 0.6%, polytetrafluoroethylene (C2F4): 1%, sodium carboxymethyl cellulose (CMC): 0.4%, and SrCO3: 10%.

[0096] The chemical composition, preparation process, and welding process parameters of the welding core are the same as those in Example 1.

[0097] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0098] Comparative Example 5 The difference from Example 5 is that this comparative example increases the NiNb alloy content, and its coating solid components, by mass percentage, include: TiO2: 18%, NaF: 30%, CaCO3: 14%, potassium feldspar: 6%, NiNb alloy: 9%, Cr: 5%, Mn: 8%, Na2CO3: 0.2%, polytetrafluoroethylene (C2F4): 0.8%, sodium carboxymethyl cellulose (CMC): 0.5%, and SrCO3: 8.5%.

[0099] The chemical composition, preparation process, and welding process parameters of the welding core are the same as those in Example 1.

[0100] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0101] Comparative Example 6 The difference from Example 3 is that BaCO3 is used instead of SrCO3 in this comparative example, and the solid components of its coating, by mass percentage, include: TiO2: 20%, NaF: 28%, CaCO3: 12%, potassium feldspar: 8%, NiNb alloy: 6%, Cr: 5%, Mn: 12%, Na2CO3: 0.5%, polytetrafluoroethylene (C2F4): 1%, sodium carboxymethyl cellulose (CMC): 0.5%, and BaCO3: 7%.

[0102] The chemical composition, preparation process, and welding process parameters of the welding core are the same as those in Example 1.

[0103] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0104] Comparative Example 7 The difference from Example 1 is that CaF2 is used instead of NaF in this comparative example, and the solid components of its coating, by mass percentage, include: TiO2: 22%, CaF2: 30%, CaCO3: 10%, potassium feldspar: 8%, NiNb alloy: 5%, Cr: 4%, Mn: 9%, Na2CO3: 0.4%, polytetrafluoroethylene (C2F4): 1%, sodium carboxymethyl cellulose (CMC): 0.6%, and SrCO3: 10%.

[0105] The chemical composition, preparation process, and welding process parameters of the welding core are the same as those in Example 1.

[0106] The mechanical and impact properties of the weld metal are shown in Tables 2 and 3, respectively. The welding process properties and coating properties are shown in Table 4.

[0107] Performance testing: Tensile tests, impact tests, and bending tests were all conducted in accordance with NB / T 20004-2014 "Physical and Chemical Testing Methods for Materials of Nuclear Island Mechanical Equipment in Nuclear Power Plants".

[0108] Table 1. Solid components (wt%) of the drug coating in the examples and comparative examples

[0109] Table 2 Tensile properties of weld metal in the weld state of the examples and comparative electrodes

[0110] Table 3. Room temperature impact performance of the welding electrodes in the examples and comparative examples.

[0111] Table 4 Welding process performance and coating performance of the welding electrodes used in the examples and comparative examples

[0112] Table 5 Comparison of welding electrode production performance between Example 3 and Comparative Example 3

[0113] Note: The calculation method for electrode eccentricity shall be in accordance with GB / T983 and shall be tested using an eccentricity meter.

[0114] The nickel-based alloy welding electrodes prepared in Examples 1-5 exhibited good molten pool fluidity and spreading properties, good molten pool visibility, good arc stability, and good operability in both long and short arc welding when applied by DC reverse polarity welding. The slag shell coverage was uniform, slag removal was easy, the weld bead formation was bright, and welding fumes were relatively minimal. Tables 2 and 3 show that the weld metals of Examples 1-5, under both room temperature and high temperature conditions, maintained relatively stable tensile strength, yield strength, elongation after fracture, and impact absorption energy, meeting the mechanical properties required by relevant standards for nuclear power equipment manufacturing. Intergranular corrosion tests were conducted on the weld metals of Examples 1-5 according to ASTM A262 E method. No cracks or intergranular corrosion tendency were observed after the tests, indicating good resistance to intergranular corrosion.

[0115] As shown in Table 4, compared with Example 1, Comparative Example 1 contains no TiO2 and has a higher CaCO3 content, making arc ignition relatively difficult, arc stability poor, and increasing the tendency for arc breakage and extinguishing. The slag is also more viscous and has poorer fluidity. As shown in Table 2, the room temperature tensile strength and yield strength of the weld metal in Comparative Example 1 are slightly lower than those in Example 1. As shown in Table 3, the room temperature impact absorption energy of Comparative Example 1 is higher than that of Example 1. The absence of TiO2 in the coating of Comparative Example 1 reduces arc stability and the ability to regulate the melting point, viscosity, and surface tension of the slag, resulting in reduced molten pool fluidity during welding, difficulty in arc ignition and stabilization, and increased slag viscosity. The higher CaCO3 content in the coating increases the basicity of the slag, resulting in relatively better desulfurization and dephosphorization effects and a lower content of impurities such as sulfur and phosphorus in the weld metal, which is beneficial for improving impact toughness.

[0116] Depend on Figures 1-4 It can be seen that, under the flat welding condition of 120A welding current, compared with Comparative Example 1, the electrode slag shell of Example 1 is more uniform and complete, the weld formation is bright and smooth, and the fluidity and spreading of the molten pool are relatively better. Figure 5 It can be seen that when the welding electrode in the embodiment is used for vertical welding at a welding current of 120A, the weld formation is good, and the fluidity of the molten pool and the controllability of the operation meet the requirements for vertical welding.

[0117] As shown in Table 4, compared with Example 2, Comparative Example 2, which replaced NiNb alloy with niobium iron, exhibited poorer slag fluidity during welding, relatively rougher weld formation, and decreased slag coverage uniformity. Tables 2 and 3 show that the room temperature tensile strength and yield strength of the weld metal in Comparative Example 2 were lower than those in Example 2, and the room temperature impact absorption energy was also lower. These results indicate that NiNb alloy has certain advantages over niobium iron alone in terms of alloy element transition stability and the overall performance of the weld metal.

[0118] Table 5 shows that, compared with Example 3, Comparative Example 3, which uses sodium alginate instead of polytetrafluoroethylene (PTFE), dries the powder faster after adding the binder. However, it tends to clump and harden during stirring, resulting in decreased powder uniformity, increased pressure during coating, a relatively rougher electrode appearance, and greater difficulty in controlling eccentricity. Table 4 shows that in Comparative Example 3, the flux coating did not completely melt during welding, leading to flux peeling, uneven slag coverage, and poorer weld pool fluidity and weld formation compared to Example 3. These results indicate that PTFE plays a role in delaying powder drying, improving coating performance, and enhancing welding process stability.

[0119] As shown in Table 4, compared with Example 4, Comparative Example 4 reduced the NiNb alloy content, but the welding process performance was not significantly different from that of Example 4. As shown in Table 2, the room temperature tensile strength and yield strength of the weld metal in Comparative Example 4 were lower than those in Example 4. As shown in Table 3, the room temperature impact absorption energy of Comparative Example 4 was higher than that of Example 4. The reduction in NiNb alloy content resulted in a decrease in the amount of Nb transition in the weld metal, leading to insufficient precipitation of the reinforcing phase and a decrease in tensile strength. However, the reduced reinforcing phase content improved impact toughness, hence the higher room temperature impact absorption energy compared to Example 4.

[0120] As shown in Table 4, compared with Example 5, Comparative Example 5, with its increased NiNb alloy content, exhibited relatively larger spatter during welding. Table 2 shows that the room temperature and high temperature tensile strength and yield strength of the weld metal in Comparative Example 5 were higher than those in Example 5, while the elongation after fracture was lower. When the NiNb alloy content is too high, the amount of Nb in the weld metal increases, leading to more strengthening phases, increased strength, and decreased elongation after fracture. This also increases alloy cost, increases welding spatter, reduces the plasticity of the weld metal, adversely affects welding operability, and ultimately reduces overall process performance.

[0121] As shown in Table 4, compared with Example 3, Comparative Example 6, which replaced SrCO3 with BaCO3, resulted in an irregular molten pool, poor slag fluidity, incomplete slag removal, and poor weld formation during welding. These results indicate that SrCO3 plays a positive role in adjusting the physical properties of slag, improving slag removal, and suppressing spatter.

[0122] As shown in Table 4, compared with Example 1, Comparative Example 7, which used CaF2 instead of NaF, resulted in an irregular molten pool, poor slag fluidity, insufficient slag spreading, significant spatter, and poor slag removal and weld formation during welding. These results indicate that NaF has a positive effect on reducing the surface tension of the molten pool, improving its fluidity, and enhancing slag spreading.

[0123] In summary, the electrode coating provided by this invention, through the synergistic proportioning of functional components such as NaF, TiO2, SrCO3, and NiNb alloy in the solid composition, helps to reduce the surface tension of the molten pool, adjust the viscosity and surface tension of the slag, and improve the molten pool fluidity and spreading properties during nickel-based alloy welding. This allows the electrode to combine the advantages of a clear molten pool in alkaline slag systems and good arc stability in acidic slag systems. The nickel-based alloy welding electrode provided by this invention, through the combination of the nickel-based alloy core and the aforementioned coating, helps to improve weld formation quality without increasing the welding current, reducing poor weld formation and slag inclusion tendency caused by insufficient molten pool fluidity. Furthermore, it provides uniform slag coverage, easy slag removal, and good adaptability to both AC and DC power supplies.

[0124] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A nickel-based alloy welding electrode, characterized in that, The coating comprises a nickel-based alloy core and a flux coating covering the surface of the core. The solid components of the flux coating, by mass percentage, are: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities.

2. The welding electrode according to claim 1, characterized in that, The nickel-based alloy core composition, by mass percentage, includes: C≤0.015%, Mn: 0.6%~1.0%, Si≤0.10%, Cr: 29.0%~31.0%, Fe: 9.0%~10.0%, Ti: 0.2%~0.3%, Al: 0.08%~0.15%, Nb: 0.7%~1.0%, Ni≥55%, Cu≤0.10%, N≤0.008%, S≤0.002%, P≤0.005%, Mo: 0.3%~0.5%.

3. The welding electrode according to claim 1 or 2, characterized in that, The nickel-based alloy core composition, by mass percentage, includes: C: 0.010%–0.014%, Mn: 0.65%–0.88%, Si: 0.018%–0.05%, Cr: 29.93%–30.27%, Fe: 9.67%–9.92%, Ti: 0.22%–0.28%, Al: 0.087%–0.13%, Nb: 0.74%–0.93%, Ni: 57.6%. 5%~58.43%, Cu: 0.0023%~0.0064%, N: 0.0031%~0.0066%, S: 0.0011%~0.0019%, P: 0.0025%~0 .0039%, Mo: 0.32%~0.48%, V: 0.0068%~0.013%, Co: 0.0059%~0.0069%, Ta: 0.0010%~0.0025%.

4. A welding electrode coating, characterized in that, The solid components of the coating, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities; The NiNb alloy contains 25%–30% Ni by mass and 65%–70% Nb by mass.

5. A method for preparing a nickel-based alloy welding electrode, characterized in that, Includes the following steps: The raw materials of the solid components of the coating are mixed evenly, and an alkali metal silicate binder is added. After stirring evenly, the mixture is sent to a pressing machine for pressing and coating. The wet coating is pressed onto the surface of the nickel-based alloy welding core and then baked to produce a welding rod.

6. The preparation method according to claim 5, characterized in that, The solid components of the coating, by mass percentage, include: TiO2: 16%–22%, NaF: 26%–32%, CaCO3: 10%–14%, potassium feldspar: 6%–8%, NiNb alloy: 5%–7%, Cr: 3%–5%, Mn: 8%–12%, Na2CO3: 0.2%–0.5%, polytetrafluoroethylene: 0.8%–1%, sodium carboxymethyl cellulose: 0.4%–0.6%, SrCO3: 7%–10%, with the remainder being unavoidable impurities.

7. The preparation method according to claim 5, characterized in that, The nickel-based alloy core composition, by mass percentage, includes: C≤0.015%, Mn: 0.6%~1.0%, Si≤0.10%, Cr: 29.0%~31.0%, Fe: 9.0%~10.0%, Ti: 0.2%~0.3%, Al: 0.08%~0.15%, Nb: 0.7%~1.0%, Ni≥55%, Cu≤0.10%, N≤0.008%, S≤0.002%, P≤0.005%, Mo: 0.3%~0.5%.

8. The preparation method according to claim 5, characterized in that, The mass of the alkali metal silicate binder is 20% to 25% of the mass of the solid component of the drug coating; and / or, the alkali metal silicate binder is potassium sodium water glass; and / or, the baking includes two stages: low-temperature baking and high-temperature baking, wherein the low-temperature baking temperature is 60°C to 100°C and the high-temperature baking temperature is 330°C to 370°C.

9. The preparation method according to claim 5, characterized in that, The stirring time after adding the alkali metal silicate binder is 12 min to 30 min; and / or the pressing pressure of the pressing machine is 100 MPa to 120 MPa.