A method for manufacturing an x-ray tube microfocus anode
By quantitatively controlling the diffusion layer thickness and casting parameters at the tungsten-copper interface, the problems of interfacial thermal resistance and bonding strength of the anode in microfocus X-ray tubes were solved, achieving high-resolution and stable microfocus X-ray tube imaging and improving product consistency and reliability.
Patent Information
- Application Number
- CN202611348695.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-24
AI Technical Summary
In the preparation of microfocus X-ray tube anodes, the thickness of the diffusion layer is uncontrollable, resulting in high interfacial thermal resistance, difficulty in heat dissipation, significant focus thermal drift, insufficient bonding strength, and difficulty in ensuring product consistency and reliability. Furthermore, the focus size and thermal drift rate are not correlated with the final performance indicators.
Pretreatment processes such as vibration polishing and ultrasonic cleaning are employed, combined with vacuum brazing and precision machining. By combining the thermal conduction equation and the atomic diffusion kinetics equation, the diffusion layer thickness and casting parameters of the tungsten-copper interface are quantitatively controlled to ensure that the interface bonding strength and thermal conductivity match the power loading conditions of the X-ray tube.
It achieves precise control over the diffusion layer thickness, keeps the focal thermal drift rate within 5%, improves product consistency and imaging resolution, reduces the cost of scrapping the entire tube due to anode failure, and adapts to the needs of small-batch multi-variety and large-batch single-variety production.
Smart Images

Figure CN123149708A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of X-ray tube manufacturing technology, specifically to a method for preparing a microfocal anode for an X-ray tube. Background Technology
[0002] The microfocus anode is the core functional component of a microfocus X-ray tube. Its main functions are to receive high-speed electron beams to generate X-rays, rapidly conduct away the large amount of heat generated by the bombardment, and absorb secondary electrons and scattered rays to ensure the stable operation of the X-ray tube. With the continuous improvement of medical diagnostics' demand for high-resolution imaging and semiconductor detection's ability to identify nanoscale defects, the focal size of microfocus X-ray tubes has shrunk from the hundreds of micrometers to several micrometers or even submicrometers. The smaller the focal size, the higher the imaging resolution, but the requirements for anode performance increase exponentially.
[0003] When the focal size shrinks to the micrometer level, the power density of the electron beam energy on the target surface increases dramatically, reaching 10-10. 6 ~10 7 W / cm 2 On a massive scale, under these extreme conditions, if the thermal conductivity of the tungsten-copper interface is insufficient, heat will rapidly accumulate on the surface of the tungsten target, causing a sharp rise in target temperature. The thermal expansion of the target surface will directly alter the size and shape of the focal spot, causing thermal drift and resulting in blurred imaging and reduced resolution. In severe cases, interfacial thermal fatigue can lead to the tungsten target detaching or cracking, causing the X-ray tube to fail completely.
[0004] Currently, the mainstream fabrication process for microfocus fixed anodes is the back casting and melting process using a tungsten sheet and an oxygen-free copper rod. The basic procedure involves placing a tungsten sheet in a graphite mold, allowing molten copper to diffuse into the surface of the tungsten sheet at high temperature, forming a metallurgical bond through atomic diffusion, then brazing the cast target blank to an extended copper rod, and finally machining the final shape. However, existing technologies have the following prominent problems: (i) The thickness of the diffusion layer is uncontrollable, and the selection of temperature and holding time relies entirely on the operator's experience or simple trial and error. No quantitative relationship has been established between process parameters and the microstructure of the bonding layer (diffusion layer). However, a thicker diffusion layer is not necessarily better: an excessively thin diffusion layer (<5μm) cannot form sufficient metallurgical bonding, resulting in high interfacial thermal resistance, difficulty in heat dissipation, and significant focal thermal drift; an excessively thick diffusion layer (>30μm) will lead to an increase in interfacial micropores due to the Kirkendall effect caused by tungsten-copper interdiffusion, which weakens the bonding strength and increases interfacial thermal resistance. Due to the lack of quantitative control methods, the diffusion layer thickness of the same batch of products can fluctuate by more than ±15μm, making it difficult to guarantee product consistency and reliability.
[0005] (ii) The interface bonding quality cannot be correlated with the final performance indicators of the microfocus X-ray tube, and the design logic of the existing process is completely disconnected from the final performance of the microfocus X-ray tube. Core performance indicators such as focal size and focal thermal drift rate are not used as input boundary conditions for process design.
[0006] In summary, establishing a quantitative correlation between the microfocus anode fabrication process and the focal performance of the X-ray tube, and achieving precise control over the diffusion layer thickness, thereby ensuring the imaging accuracy and long-term reliability of the microfocus X-ray tube at high power density, is a problem that needs to be solved. Summary of the Invention
[0007] To address the aforementioned problems, this invention provides a method for preparing a microfocus anode for an X-ray tube.
[0008] The technical solution of this invention is: A method for preparing a microfocus anode for an X-ray tube includes the following steps: S1. Parts preparation: S1-1. Tungsten sheet pretreatment: The tungsten sheet blank is cut into blanks, then polished, then cleaned, and finally heat-treated for purification to obtain pretreated tungsten sheets. S1-2 Preparation of cast copper rods: The blank of cast copper rods is processed and then cleaned to obtain cast copper rods; S1-3. Preparation of the extended copper rod: The blank of the extended copper rod is processed and then cleaned to obtain the extended copper rod; S2, Back Casting Blank: S2-1. The pretreated tungsten sheet and cast copper rod are assembled in a graphite mold and cast in a graphite casting furnace to allow copper to penetrate the surface of the tungsten sheet and form a tungsten-copper bonding surface through atomic diffusion to obtain a casting target blank. S2-2. Roughly machine the cast target blank to obtain the cast target blank in the welding preparation state; S3. Vacuum brazing: Take silver-copper brazing sheet and clean the cast target blank obtained in S2-2 and the extended copper rod obtained in S1-3 before welding. The pre-welding cleaning includes degreasing and deoxidation treatment in sequence. Then, the cast target blank, silver-copper brazing sheet and extended copper rod are assembled and fixed in sequence. The assembled workpiece is placed into a vacuum brazing furnace for vacuum brazing. After welding is completed, a semi-finished welded product is obtained. S4. Finished product machining: The welded semi-finished product obtained in S3 is machined to the finished product size using a precision lathe.
[0009] Further, in S1-1, the polishing is performed using a vibratory polishing machine filled with green resin abrasive stones at a frequency of 30-40 Hz and an amplitude of 2-3 mm for 1-2 hours; the cleaning is performed using ultrasonic cleaning at a frequency of 25-40 Hz for 15-20 minutes; the heat treatment purification temperature is 800-1200℃, the holding time is 30-120 minutes, and the heat treatment is carried out under vacuum or a protective atmosphere.
[0010] Explanation: Pretreatment processes such as vibration polishing and ultrasonic cleaning effectively remove oil, oxide layer and processing stress from the surface of tungsten sheets, resulting in a clean and flat tungsten sheet surface. This provides an excellent surface condition for the uniform wetting and full diffusion of liquid copper during the subsequent casting process, ensuring that the tungsten-copper interface is free of impurities.
[0011] Furthermore, in S1-2 and S1-3, both the cast copper rod blank and the extended copper rod blank are oxygen-free copper rods. The processing is turning. After processing, the size of the cast copper rod is Φ20~30 and the size of the extended copper rod is Φ15-20. The cleaning is ultrasonic cleaning at 25~40Hz for 15~20 minutes.
[0012] Note: Oxygen-free copper rods ensure the assembly accuracy of the cast copper rod and the graphite mold, extend the dimensional consistency of the copper rod, and reduce interface defects caused by impurities or dimensional deviations in the copper rod itself.
[0013] Furthermore, in step S2-1, the absolute temperature T of the melting and casting and the holding time t satisfy formula (1): In the formula, T is the absolute temperature of melting and casting, in K, t is the holding time, in s, and D0 is the diffusion constant, in μm. 2 / s, Q is the activation energy of tungsten-copper interdiffusion, in J / mol; R is the ideal gas constant, taken as 8.314 J / (mol·K); β is the dimensionless comprehensive conversion factor, ranging from 80 to 160; ε is the maximum allowable focal thermal drift rate of the microfocal anode in the X-ray tube, in % F 0 α is the target nominal focal size of the microfocal anode in the X-ray tube, in μm; W Let be the average linear thermal expansion coefficient of the tungsten sheet over the range of room temperature to operating temperature, taken as 4.5 × 10⁻⁶. -6 K -1 L represents the thermal diffusion depth of the electron beam in the tungsten sheet, in μm; λ W-Cu denoted as , where is the equivalent thermal conductivity of the tungsten-copper interface, in W / (m·K); and A is the effective heat dissipation area of the tungsten-copper interface, in m². 2P is the X-ray tube power, in W, and P = U·I; where U is the tube voltage, in kV, and I is the tube current, in mA. The holding time t is calculated by first fixing the absolute temperature T of the melting and casting process; Alternatively, the absolute temperature T of the melting and casting can be calculated by first fixing the holding time t; When the absolute temperature T of the melting and casting is fixed, the absolute temperature T ranges from 1100 to 1350℃. When the heat preservation time t is fixed first, the value of heat preservation time t is in the range of 10~60min; Formula (1) is derived by combining formulas (2) to (5), where the maximum allowable temperature rise ΔT at the tungsten-copper interface is first determined. max As shown in formula (2): In the formula, ΔT max ε is the maximum permissible temperature rise at the tungsten-copper interface, in K; ε is the maximum permissible focal thermal drift rate of the X-ray tube microfocus anode, in %; Φ0 is the target nominal focal size of the X-ray tube microfocus anode, in μm; α W Let be the average linear thermal expansion coefficient of the tungsten sheet over the range of room temperature to operating temperature, taken as 4.5 × 10⁻⁶. -6 K -1 L represents the thermal diffusion depth of the electron beam in the tungsten sheet, in μm. Secondly, the target diffusion layer thickness x at the tungsten-copper interface is determined as shown in formula (3): In the formula, x is the target diffusion layer thickness at the tungsten-copper interface, in μm; λ W-Cu denoted as , where is the equivalent thermal conductivity of the tungsten-copper interface, in W / (m·K); and A is the effective heat dissipation area of the tungsten-copper interface, in m². 2 P is the X-ray tube power, in W, and P = U·I, where U is the tube voltage in kV and I is the tube current in mA. Meanwhile, the target diffusion layer thickness x at the tungsten-copper interface satisfies formula (4): In the formula, β is a dimensionless comprehensive conversion factor, ranging from 80 to 160; D is the interdiffusion coefficient of the tungsten-copper system, in μm. 2 / s, expressed by formula (5): In the formula, D0 is the diffusion constant, with units of μm. 2 / s, Q is the activation energy of tungsten-copper interdiffusion, in J / mol; R is the ideal gas constant, taken as 8.314 J / (mol·K); Combining formulas (2) to (5), we obtain formula (1): The casting is carried out under vacuum or a protective atmosphere.
[0014] Furthermore, the diffusion constant D0 ranges from 0.5 × 10⁻⁶. 5 ~5×10 5 μm 2 / s, where the diffusion activation energy Q is the activation energy Q for the diffusion of copper to tungsten. Cu→W =86kJ / mol.
[0015] Note: The activation energy of copper diffusion into tungsten is used as the main control parameter, and the range of the diffusion constant D0 is limited. Based on the physical reality that copper is a liquid phase and tungsten is a solid phase during the casting process, the physical uniqueness and calculation accuracy of the parameters in the process control equation are ensured.
[0016] Furthermore, the thermal diffusion depth L of the electron beam in the tungsten sheet is determined by the following formula: L=0.1E 1.5 / r Where E is the electron beam energy in keV, and ρ is the density of the tungsten sheet in g / cm³. 3 The equivalent thermal conductivity λ of the tungsten-copper interface W-Cu The value ranges from 180 to 260 W / (m·K).
[0017] Note: The electron beam thermal diffusion depth L and the equivalent thermal conductivity λ at the interface are given. W-Cu The specific calculation formulas and value ranges are provided to ensure that each physical quantity has a clear way of being obtained.
[0018] Furthermore, in S3, the welding temperature of the vacuum brazing is 810~850℃, and the holding time is 3~15min; the vacuum degree of the vacuum brazing furnace is not less than 5×10⁻⁶. -3Pa, the silver-copper solder sheet is an AgCu28 solder sheet, wherein the silver content is 72wt% and the copper content is 28wt%. The degreasing cleaning is performed using organic solvent cleaning or alkaline cleaning solution. The organic solvent is acetone or anhydrous ethanol, and the alkaline cleaning solution is NaOH aqueous solution with a mass percentage concentration of 1.5~5%, a cleaning temperature of 40~60℃, and a cleaning time of 10~20min. After cleaning, the workpiece is taken out and rinsed with deionized water 2~3 times, each time for 1~2min, then dehydrated with anhydrous ethanol, and then dried with hot air at 80~100℃. The deoxidation treatment is performed using pickling solution. The pickling solution is sulfuric acid aqueous solution with a volume percentage concentration of 5~20%, a pickling temperature of 30~60℃, and a pickling time of 5~15min.
[0019] Note: By reasonably selecting the welding temperature and related parameters, a reliable connection between the cast target blank and the extended copper rod under relatively low heat input conditions was achieved, avoiding the adverse effects of high-temperature long-term brazing on the formed tungsten-copper diffusion layer.
[0020] Furthermore, in step S4, after machining on the precision lathe, the surface roughness Ra of the working surface of the finished microfocal anode is ≤0.1, the surface roughness Ra of the remaining part is ≤0.8, and the machining dimensional tolerance is controlled within ±0.01mm.
[0021] Explanation: By controlling the dimensional error of the finished product, the smoothness of the tungsten target surface and the assembly accuracy of the anode assembly are ensured, reducing the deterioration of the effective focal spot size caused by electron beam scattering and assembly deviation.
[0022] The beneficial effects of this invention are: (1) This invention provides a method for preparing a microfocus anode for an X-ray tube. A tungsten target is bonded to a copper body using a back casting method, and the copper body is extended using vacuum brazing. Subsequently, the microfocus fixed anode is obtained by precision machining. During the melting and infiltration process, a good bonding surface is formed between the two materials through atomic diffusion, and the bonding strength is much higher than that of welding. There is no weld seam on the tungsten-copper working surface. The reason for extending the copper body by vacuum brazing is that the melting and infiltration method melts and resolidifies the copper, resulting in a relatively soft copper body. However, the microfocus anode is usually quite long, and direct processing can easily cause deformation. Therefore, brazing is used to extend a portion of the copper body with higher hardness, reducing the processing difficulty and ensuring the overall strength.
[0023] (2) This invention, for the first time, uses the nominal focal size Φ0 and the allowable focal thermal drift rate ε of the final performance indicators of the microfocus X-ray tube as input boundary conditions for the casting process design. By simultaneously solving the heat conduction equation and the atomic diffusion kinetics equation, the characteristic control equation of the casting process, namely Formula 1, is derived. This equation quantitatively reveals the complete transmission chain from the focal performance requirements to the maximum allowable temperature rise at the interface, and then to the required diffusion layer thickness and the optimal casting parameters (T, t), upgrading the setting of casting process parameters from traditional trial and error to precise calculation based on mathematical and physical models. This allows the diffusion layer thickness to be precisely controlled within the optimal range according to the target focal size, avoiding process defects of being too thin or too thick; the interface heat conduction capability is precisely matched with the power loading conditions of the X-ray tube, ensuring that the focal spot thermal drift rate is controlled within 5%, guaranteeing the high resolution and stability of microfocus imaging; the diffusion layer thickness deviation of different batches of products can be controlled within ±15%, greatly improving product consistency and manufacturing yield, and reducing the cost of scrapping the entire tube due to anode failure.
[0024] (3) The method of the present invention is adaptable to different production scenarios. When small-batch, multi-variety production is required, the absolute temperature T of the melting and casting can be fixed first, and the holding time t can be adjusted by calculation to adapt to different models. Thus, when changing models, only the holding time t needs to be changed, without waiting for the furnace to heat up or cool down. When large-batch, single-variety production is required, the production cycle can be optimized by fixing the holding time t first, and the absolute temperature T of the melting and casting can be adjusted by calculation. The highest allowable temperature corresponding to the shortest holding time can be found. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of the overall structure of the microfocus anode of the X-ray tube prepared according to the present invention. Detailed Implementation
[0026] Example 1: A method for preparing a microfocus anode for an X-ray tube, wherein the microfocus anode is a small-focus, low-power type suitable for semiconductor chip detection, and includes the following steps: S1. Parts preparation: S1-1. Tungsten sheet pretreatment: The tungsten sheet blank is cut into pieces, then polished, then cleaned, and finally heat-treated for purification to obtain pretreated tungsten sheets. Polishing is performed using a vibratory polishing machine filled with green resin abrasive stones at 35Hz and 2.5mm amplitude for 1.5 hours. Cleaning is performed using ultrasonic cleaning at 40Hz for 20 minutes. The heat treatment purification temperature is 1000℃, and the holding time is 60 minutes. The heat treatment is carried out under vacuum. S1-2 Preparation of cast copper rods: The blank of cast copper rods is processed and then cleaned to obtain cast copper rods; S1-3. Preparation of the extended copper rod: The blank of the extended copper rod is processed and then cleaned to obtain the extended copper rod; Both the cast copper rod blank and the extended copper rod blank are oxygen-free copper rods. The machining is turning. After machining, the size of the cast copper rod is Φ30 and the size of the extended copper rod is Φ20. The cleaning is done by ultrasonic cleaning at 25Hz for 20 minutes. S2, Back Casting Blank: S2-1. The pretreated tungsten sheet and cast copper rod are assembled in a graphite mold and cast in a graphite casting furnace to allow copper to penetrate the surface of the tungsten sheet and form a tungsten-copper bonding surface through atomic diffusion to obtain a casting target blank. The absolute temperature T of the melting and casting and the holding time t satisfy the formula (1): In the formula, T is the absolute temperature of melting and casting, in K, t is the holding time, in s, and D0 is the diffusion constant, in μm. 2 / s, Q is the activation energy of tungsten-copper interdiffusion, in J / mol; R is the ideal gas constant, taken as 8.314 J / (mol·K); β is the dimensionless comprehensive conversion factor, ranging from 80 to 160; ε is the maximum allowable focal thermal drift rate of the microfocal anode in the X-ray tube, in % F 0 α is the target nominal focal size of the microfocal anode in the X-ray tube, in μm; W Let be the average linear thermal expansion coefficient of the tungsten sheet over the range of room temperature to operating temperature, taken as 4.5 × 10⁻⁶. -6 K -1 L represents the thermal diffusion depth of the electron beam in the tungsten sheet, in μm; λ W-Cu denoted as , where is the equivalent thermal conductivity of the tungsten-copper interface, in W / (m·K); and A is the effective heat dissipation area of the tungsten-copper interface, in m². 2 P is the X-ray tube power, in W, and P = U·I; where U is the tube voltage, in kV, and I is the tube current, in mA. The holding time t is calculated by first fixing the absolute temperature T of the melting and casting process; Alternatively, the absolute temperature T of the melting and casting can be calculated by first fixing the holding time t; When the absolute temperature T of the melting and casting is fixed, the absolute temperature T ranges from 1100 to 1350℃. When the heat preservation time t is fixed first, the value of heat preservation time t is in the range of 10~60min; In this embodiment, the absolute temperature T of the melting and casting is preferably fixed at 1250°C, or 1523K. Formula (1) is derived by combining formulas (2) to (5), where the maximum allowable temperature rise ΔT at the tungsten-copper interface is first determined. max As shown in formula (2): In the formula, ΔT max ε is the maximum allowable temperature rise at the tungsten-copper interface, in K; ε is the maximum allowable focal thermal drift rate of the X-ray tube microfocus anode, taken as 3%; Φ0 is the target nominal focal size of the X-ray tube microfocus anode, taken as 10 μm; α W Let be the average linear thermal expansion coefficient of the tungsten sheet over the range of room temperature to operating temperature, taken as 4.5 × 10⁻⁶. -6 K -1 L represents the thermal diffusion depth of the electron beam in the tungsten sheet, measured in μm, and is determined by the following formula: L=0.1E 1.5 / r Where E is the electron beam energy, taken as 80 keV, and ρ is the density of the tungsten sheet, taken as 19.3 g / cm³. 3 ; ΔT was calculated max It is 17969K; Secondly, the target diffusion layer thickness x at the tungsten-copper interface is determined as shown in formula (3): In the formula, x is the target diffusion layer thickness at the tungsten-copper interface, in μm; λ W-Cu Let be the equivalent thermal conductivity of the tungsten-copper interface, expressed in W / (m·K). The equivalent thermal conductivity λ of the tungsten-copper interface is... W-Cu The value is taken as 220 W / (m·K); A is the effective heat dissipation area of the tungsten-copper interface, taken as 2.5 × 10⁻⁶. -5 m 2 P is the X-ray tube power, in W, and P = U·I, where U is the tube voltage, taken as 80kV, and I is the tube current, taken as 0.1mA. The calculated value of x is 12.35 μm; Meanwhile, the target diffusion layer thickness x at the tungsten-copper interface satisfies formula (4): In the formula, β is a dimensionless comprehensive conversion coefficient, ranging from 80 to 160. Specifically, β includes the product of the following three factors: β1, β2, and β3: Correction for the deviation between the actual heat dissipation area of the interface and the effective heat dissipation area A of the tungsten-copper interface: β1=4~5. This is because the tungsten-copper interface is not completely planar at the microscale, and the actual effective contact area is smaller than the effective heat dissipation area A of the tungsten-copper interface. The equivalent thermal conductivity λ of the tungsten-copper interface W-Cu Deviation correction from theoretical value: β2=5~6, the actual diffusion layer has micropores and grain boundaries, and the equivalent thermal conductivity λ of the tungsten-copper interface. W-Cu Lower than the theoretical value; The conversion correction between the effective bonding layer thickness and the target diffusion layer thickness x at the tungsten-copper bonding interface: β3=4~5, the actual effective metallurgical bonding layer is only a part of the penetration depth; In this embodiment, β1=5, β2=6, β3=4, and β is 120; D is the interdiffusion coefficient of the tungsten-copper system, in μm. 2 / s, expressed by formula (5): In the formula, D0 is the diffusion constant, with units of μm. 2 / s, the diffusion constant D0 ranges from 0.5 × 10⁻⁶. 5 ~5×10 5 μm 2 / s, in this embodiment, is taken as 2×10 5 μm 2 / s, where Q is the activation energy for tungsten-copper interdiffusion, expressed in J / mol, using the activation energy Q for copper diffusion into tungsten. Cu→W =86kJ / mol; R is the ideal gas constant, taken as 8.314J / (mol·K); The calculated value of D is 225.2 μm. 2 / s; Combining formulas (2) to (5), we obtain formula (1): The final calculation yields t = 2438.1 s ≈ 40.6 min. The casting process is carried out under vacuum. S2-2. Roughly machine the cast target blank to obtain the cast target blank in the welding preparation state; S3. Vacuum Brazing: Take the silver-copper brazing sheet and perform pre-brazing cleaning on the cast target blank obtained in S2-2 and the extended copper rod obtained in S1-3. The pre-brazing cleaning includes degreasing and deoxidation treatment. Then, assemble and fix the cast target blank, silver-copper brazing sheet, and extended copper rod in sequence. Place the assembled workpiece into a vacuum brazing furnace for vacuum brazing. After welding, a semi-finished product is obtained. The welding temperature of vacuum brazing is 820℃, and the holding time is 10min. The vacuum degree of the vacuum brazing furnace is 4×10⁻⁶. -3Pa, the silver-copper solder sheet is AgCu28 solder sheet, with a silver content of 72wt% and a copper content of 28wt%. Degreasing and cleaning are performed using anhydrous ethanol at 50℃ for 15 minutes. After cleaning, the workpiece is rinsed three times with deionized water for 2 minutes each time, then dehydrated with anhydrous ethanol, and finally dried with hot air at 90℃. Deoxidation is achieved using a pickling solution of 10% sulfuric acid aqueous solution at 40℃ for 10 minutes. S4. Finished product machining: such as Figure 1 As shown, the welded semi-finished product obtained in S3 is machined to the finished size using a precision lathe. After precision lathe machining, the surface roughness Ra of the working surface of the finished micro-focus anode is ≤0.1, and the surface roughness Ra of the remaining parts is ≤0.8. The machining dimensional tolerance is controlled within ±0.01mm.
[0027] Example 2: The difference between this example and Example 1 is that the microfocus anode of the finished X-ray tube is of medium focus and medium power type, which is suitable for medical diagnostic imaging. In this example, the absolute temperature T of the melting and casting is preferably fixed at 1250℃, that is, 1523K. ε represents the maximum permissible focal thermal drift rate of the microfocal anode in the X-ray tube, taken as 4%; Φ0 is the target nominal focal size of the microfocal anode of the X-ray tube, taken as 50 μm; U is the tube voltage, taken as 120kV; I is the tube current, taken as 0.5mA; E is the electron beam energy, taken as 120 keV; A represents the effective heat dissipation area of the tungsten-copper interface, taken as 4 × 10⁻⁶. -5 m 2 ; The equivalent thermal conductivity λ of the tungsten-copper interface W-Cu The value is taken as 220 W / (m·K); The diffusion constant D0 is 2 × 10 5 μm 2 / s; The melting and casting process is carried out under a protective argon atmosphere. The calculated heat preservation time t is 24.5 min.
[0028] Example 3: The difference between this example and Example 1 is that the finished X-ray tube microfocal anode is a large focal point, high power type, which is suitable for industrial non-destructive testing. In this example, the absolute temperature T of the melting and casting is preferably fixed at 1250℃, that is, 1523K. ε represents the maximum permissible focal thermal drift rate of the microfocal anode in the X-ray tube, taken as 5%; Φ0 is the target nominal focal size of the microfocal anode of the X-ray tube, taken as 200 μm; U is the tube voltage, taken as 160kV; I is the tube current, taken as 2mA; E is the electron beam energy, taken as 160 keV; A represents the effective heat dissipation area of the tungsten-copper interface, taken as 5 × 10⁻⁶. -5 m 2 ; The equivalent thermal conductivity λ of the tungsten-copper interface W-Cu The value is taken as 220 W / (m·K); The diffusion constant D0 is 2 × 10 5 μm 2 / s; The calculated heat preservation time t is 14.1 min.
[0029] Example 4: The difference between this example and Example 1 is that the microfocus anode of the finished X-ray tube is an ultra-microfocus, ultra-low power type, which is suitable for high-resolution semiconductor detection. In this example, the absolute temperature T of the melting and casting is preferably fixed at 1250℃, i.e. 1523K. ε represents the maximum permissible focal thermal drift rate of the microfocal anode in the X-ray tube, taken as 2%; Φ0 is the target nominal focal size of the microfocal anode of the X-ray tube, taken as 5μm; U is the tube voltage, taken as 60kV; I is the tube current, taken as 0.05mA; E is the electron beam energy, taken as 60 keV; A represents the effective heat dissipation area of the tungsten-copper interface, taken as 2 × 10⁻⁶. -5 m 2 ; The equivalent thermal conductivity λ of the tungsten-copper interface W-Cu The value is taken as 220 W / (m·K); The diffusion constant D0 is 2 × 10 5 μm 2 / s; The calculated heat preservation time t is 49.2 min.
[0030] Example 5: This example differs from Example 1 in that, in S1-1, the vibratory polishing machine is filled with green resin grinding stones and polished at 40Hz and 2mm amplitude for 1 hour; the cleaning is performed by ultrasonic cleaning at 40Hz for 15 minutes; the heat treatment purification temperature is 1200℃ and the holding time is 30 minutes, and the heat treatment is carried out under a protective atmosphere of argon.
[0031] Example 6: The difference between this example and Example 1 is that in S1-1, the vibratory polishing machine is filled with green resin grinding stones and polished at 30Hz and 3mm amplitude for 2 hours; the cleaning is done by ultrasonic cleaning at 25Hz for 20 minutes; the heat treatment purification temperature is 800℃ and the holding time is 120 minutes, and the heat treatment is carried out under vacuum.
[0032] Example 7: The difference between this example and Example 1 is that both the cast copper rod and the extended copper rod are oxygen-free copper rods, and the machining is turning. After machining, the size of the cast copper rod is Φ20 and the size of the extended copper rod is Φ15. The cleaning is done by ultrasonic cleaning at 40Hz for 15 minutes.
[0033] Example 8: This example differs from Example 1 in that, in S3, the welding temperature for vacuum brazing is 850℃, and the holding time is 3 minutes; the vacuum degree of the vacuum brazing furnace is 2×10⁻⁶. -3 Pa, the silver-copper solder sheet is AgCu28 solder sheet, with a silver content of 72wt% and a copper content of 28wt%. The degreasing and cleaning are carried out using an organic solvent, namely acetone, at a cleaning temperature of 40℃ for 20min. After cleaning, the workpiece is removed and rinsed three times with deionized water for 1min each time, then dehydrated with anhydrous ethanol, and then dried with hot air at 80℃. The deoxidation treatment is carried out using pickling solution, which is sulfuric acid aqueous solution with a volume percentage concentration of 5%, at a pickling temperature of 30℃ for 15min.
[0034] Example 9: This example differs from Example 1 in that, in S3, the welding temperature for vacuum brazing is 810℃, and the holding time is 15 minutes; the vacuum degree of the vacuum brazing furnace is 3×10⁻⁶. -3 Pa, the silver-copper solder sheet is AgCu28 solder sheet, with a silver content of 72wt% and a copper content of 28wt%. Degreasing and cleaning are performed using an alkaline cleaning solution, specifically a NaOH aqueous solution with a mass percentage concentration of 3%, at a cleaning temperature of 60℃ for 10 minutes. After cleaning, the workpiece is removed and rinsed twice with deionized water for 2 minutes each time, then dehydrated with anhydrous ethanol, and finally dried with hot air at 100℃. Deoxidation is achieved using an acid pickling solution, specifically a sulfuric acid aqueous solution with a volume percentage concentration of 20%, at a pickling temperature of 60℃ for 5 minutes.
[0035] Example 10: This example differs from Example 1 in that the diffusion constant D0 is taken as 0.5 × 10⁻⁶. 5 μm 2 / s.
[0036] Example 11: This example differs from Example 1 in that the diffusion constant D0 is taken as 5 × 10⁻⁶. 5 μm2 / s.
[0037] Experimental Example: The key parameters calculated according to Examples 1 to 4 are shown in Table 1, where the absolute temperature T for controlling the melting and casting is the same: Table 1 Key parameters calculated in Examples 1-4
[0038] As can be seen from Examples 1 to 4, when we need to produce small batches of multiple varieties, we can first fix the absolute temperature T of the melting and casting, and then adjust the holding time t by calculation to adapt to different models. Thus, when changing models, we only need to change the holding time t, without waiting for the furnace to heat up or cool down.
[0039] It can be seen that the performance requirements of the four operating conditions are very different. By quantifying the heat preservation time, the minimum effective bonding layer thickness required to meet the heat conduction requirements is different. The larger the value, the greater the risk of thermal expansion of the focal point that the unit power needs to bear, the thicker the bonding layer required, and the longer the heat preservation time. In actual production, β is not fixed; it depends on specific conditions such as tungsten powder particle size, tungsten sheet grain size, melting and infiltration temperature, and time. The β value range of 80~160 proposed in this invention covers the normal fluctuation range of this ratio under different process conditions. Each manufacturer can calibrate the actual β value under its own equipment conditions through metallographic testing (SEM-EDS) and adjust the process parameters accordingly. Under four typical working conditions, the heat preservation time t calculated by formula (1) can produce qualified anodes.
Claims
1. A method for preparing a microfocus anode for an X-ray tube, characterized in that, Includes the following steps: S1. Parts preparation: S1-1. Tungsten sheet pretreatment: The tungsten sheet blank is cut into blanks, then polished, then cleaned, and finally heat-treated for purification to obtain pretreated tungsten sheets. S1-2 Preparation of cast copper rods: The blank of cast copper rods is processed and then cleaned to obtain cast copper rods; S1-3. Preparation of the extended copper rod: The blank of the extended copper rod is processed and then cleaned to obtain the extended copper rod; S2, Back Casting Blank: S2-1. The pretreated tungsten sheet and cast copper rod are assembled in a graphite mold and cast in a graphite casting furnace to allow copper to penetrate the surface of the tungsten sheet and form a tungsten-copper bonding surface through atomic diffusion to obtain a casting target blank. S2-2. Roughly machine the cast target blank to obtain the cast target blank in the welding preparation state; S3. Vacuum brazing: Take silver-copper brazing sheet and clean the cast target blank obtained in S2-2 and the extended copper rod obtained in S1-3 before welding. The pre-welding cleaning includes degreasing and deoxidation treatment in sequence. Then, the cast target blank, silver-copper brazing sheet and extended copper rod are assembled and fixed in sequence. The assembled workpiece is placed into a vacuum brazing furnace for vacuum brazing. After welding is completed, a semi-finished welded product is obtained. S4. Finished product machining: The welded semi-finished product obtained in S3 is machined to the finished product size using a precision lathe.
2. The method for preparing a microfocus anode for an X-ray tube according to claim 1, characterized in that, In S1-1, the polishing is performed using a vibratory polishing machine filled with green resin abrasive stones at a frequency of 30-40 Hz and an amplitude of 2-3 mm for 1-2 hours; the cleaning is performed using ultrasonic cleaning at a frequency of 25-40 Hz for 15-20 minutes; the heat treatment purification temperature is 800-1200℃, the holding time is 30-120 minutes, and the heat treatment is carried out under vacuum or a protective atmosphere.
3. The method for preparing a microfocus anode for an X-ray tube according to claim 1, characterized in that, In S1-2 and S1-3, both the cast copper rod blank and the extended copper rod blank are oxygen-free copper rods. The processing is turning. After processing, the size of the cast copper rod is Φ20~30 and the size of the extended copper rod is Φ15-20. The cleaning is ultrasonic cleaning at 25~40Hz for 15~20 minutes.
4. The method for preparing a microfocus anode for an X-ray tube according to claim 1, characterized in that, In step S2-1, the absolute temperature T of the melting and casting and the holding time t satisfy formula (1): In the formula, T is the absolute temperature of melting and casting, in K, t is the holding time, in s, and D0 is the diffusion constant, in μm. 2 / s, Q is the activation energy of tungsten-copper interdiffusion, in J / mol; R is the ideal gas constant, taken as 8.314 J / (mol·K); β is the dimensionless comprehensive conversion factor, ranging from 80 to 160; ε is the maximum allowable focal thermal drift rate of the microfocal anode in the X-ray tube, in % Φ 0 α is the target nominal focal size of the microfocal anode in the X-ray tube, in μm; W Let be the average linear thermal expansion coefficient of the tungsten sheet over the range of room temperature to operating temperature, taken as 4.5 × 10⁻⁶. -6 K -1 L represents the thermal diffusion depth of the electron beam in the tungsten sheet, in μm; λ W-Cu denoted as , where is the equivalent thermal conductivity of the tungsten-copper interface, in W / (m·K); and A is the effective heat dissipation area of the tungsten-copper interface, in m². 2 P is the X-ray tube power, in W, and P = U·I; where U is the tube voltage, in kV, and I is the tube current, in mA. The holding time t is calculated by first fixing the absolute temperature T of the melting and casting process; Alternatively, the absolute temperature T of the melting and casting can be calculated by first fixing the holding time t; When the absolute temperature T of the melting and casting is fixed, the absolute temperature T ranges from 1100 to 1350℃. When the heat preservation time t is fixed first, the value of heat preservation time t is in the range of 10~60min; The casting is carried out under vacuum or a protective atmosphere.
5. The method for preparing a microfocus anode for an X-ray tube according to claim 4, characterized in that, The diffusion constant D0 ranges from 0.5 × 10⁻⁶. 5 ~5×10 5 μm 2 / s, where the diffusion activation energy Q is the activation energy Q for the diffusion of copper to tungsten. Cu→W =86kJ / mol.
6. The method for preparing a microfocus anode for an X-ray tube according to claim 4, characterized in that, The thermal diffusion depth L of the electron beam in the tungsten sheet is determined by the following formula: L=0.1E 1.5 / ρ Where E is the electron beam energy in keV, and ρ is the density of the tungsten sheet in g / cm³. 3 The equivalent thermal conductivity λ of the tungsten-copper interface W-Cu The value ranges from 180 to 260 W / (m·K).
7. The method for preparing a microfocus anode for an X-ray tube according to claim 1, characterized in that, In step S3, the welding temperature for vacuum brazing is 810~850℃, and the holding time is 3~15min; the vacuum degree of the vacuum brazing furnace is not less than 5×10⁻⁶. -3 Pa, the silver-copper solder sheet is an AgCu28 solder sheet, wherein the silver content is 72wt% and the copper content is 28wt%, the degreasing cleaning is performed by organic solvent cleaning or alkaline cleaning solution cleaning; the deoxidation treatment is performed by pickling solution pickling.
8. The method for preparing a microfocus anode for an X-ray tube according to claim 1, characterized in that, In step S4, after machining on the precision lathe, the surface roughness Ra of the working surface of the finished microfocal anode is ≤0.1, the surface roughness Ra of the remaining part is ≤0.8, and the machining dimensional tolerance is controlled within ±0.01mm.