Resin-metal semi-interpenetrating network composite bonding agent diamond grinding wheel and preparation method thereof
By introducing Cu-Sn alloy powder into the resin diamond grinding wheel to form a semi-interpenetrating network structure, the problems of thermal conductivity and heat resistance of the resin diamond grinding wheel are solved, realizing efficient silicon carbide wafer thinning processing, extending the grinding wheel life and improving the processing quality.
Patent Information
- Application Number
- CN202611669627.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-27
- Publication Date
- 2026-11-24
AI Technical Summary
Existing resin-bonded diamond grinding wheels suffer from poor thermal conductivity, heat accumulation leading to thermal damage, and premature abrasive shedding during silicon carbide wafer thinning, affecting processing quality and lifespan.
A diamond grinding wheel using a resin-metal semi-interpenetrating network composite binder is constructed by introducing Cu-Sn alloy powder into the resin binder to form a semi-interpenetrating network structure, combined with thermally conductive fillers and solid lubricating fillers, to build an efficient heat conduction channel and enhance the heat resistance and toughness of the binder.
It significantly improves the thermal conductivity of the grinding wheel, reduces heat accumulation, avoids damage to the wafer surface, extends the grinding wheel life, and improves grinding accuracy and efficiency.
Smart Images

Figure CN123149889A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor wafer ultra-precision processing tools, and in particular to a resin-metal semi-interpenetrating network composite binder diamond grinding wheel and its preparation method, which is suitable for thinning processing of silicon carbide and silicon substrate wafers. Background Technology
[0002] With the continuous development of the semiconductor industry, silicon carbide wafers, as an important semiconductor material, are playing an increasingly vital role in fields such as electronic device manufacturing. Thinning silicon carbide wafers is a crucial step in manufacturing high-performance electronic devices, directly affecting their performance and stability. Against this backdrop, grinding wheel technology used for silicon carbide wafer thinning has attracted considerable attention, as its performance is of great significance for improving processing quality and efficiency. However, existing grinding wheel technologies still face many challenges in meeting the ever-increasing processing demands.
[0003] In silicon carbide wafer thinning, existing resin-bonded diamond grinding wheels are commonly used tools. These wheels primarily rely on resin binders to hold the diamond abrasive together, thereby enabling the grinding of the silicon carbide wafer. In addition, some technologies explore adding polyimide resin to the metal binder to improve the wheel's performance.
[0004] However, existing resin-bonded diamond grinding wheels have significant drawbacks. Due to the high Mohs hardness of silicon carbide, a large amount of heat is generated during grinding. The low thermal conductivity of pure resin binders leads to heat accumulation in the grinding zone, easily causing thermal damage to the wafer surface, such as microcracks and deepening of the subsurface damage layer. Simultaneously, the limited heat resistance of resin means the binder softens at high temperatures, causing premature abrasive detachment and shortening wheel life. Furthermore, existing technologies that add polyimide resin to the metal binder are essentially still metal-based, with the resin serving only as an auxiliary phase, and cannot solve the thermal conductivity problem of resin-based grinding wheels. Summary of the Invention
[0005] To address the problems in the prior art, this application provides a resin-metal semi-interpenetrating network composite bonded diamond grinding wheel and its preparation method.
[0006] This application provides a resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, which adopts the following technical solution: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel comprises the following components by volume fraction: 15-30% diamond abrasive, 35-55% resin binder, 8-25% metal powder, 3-15% thermally conductive filler, 1-8% solid lubricating filler, and 1-5% pore-forming agent.
[0007] It should be noted that the "resin-metal semi-interpenetrating network" described in this application is not a semi-interpenetrating polymer network in the traditional sense of two polymer chains interpenetrating each other in the polymer field. The structure in this application is defined as follows: the resin binder undergoes a cross-linking reaction during hot pressing and curing to form a three-dimensional cross-linked polymer network; the Cu-Sn alloy metal powder does not melt under hot pressing and achieves cold welding and overlapping between particles through plastic deformation, thus constructing an interconnected continuous metal phase inside the resin matrix; the interconnected metal phase is interpenetrated and distributed in the gaps of the resin cross-linked three-dimensional network, and the two phases are interpenetrated and nested in space. Therefore, this composite spatial structure is named resin-metal semi-interpenetrating network in this application.
[0008] Preferably, the metal powder is Cu-Sn alloy powder, wherein the Sn content is 5-15 wt%, and the particle size D50 of the metal powder is 0.5-15 μm.
[0009] By adopting the above technical solution, the resin binder undergoes cross-linking and curing during the subsequent hot-pressing process to form a three-dimensional network structure. Due to the good fluidity and ductility of the metal powder itself, under hot pressing, the metal particles, although not melting, undergo plastic deformation and cold welding, gradually connecting together. As the curing reaction proceeds, the metal powder forms a continuous overlapping semi-interpenetrating network structure in the resin matrix. This structure, combined with the thermally conductive filler, can create a highly efficient heat conduction channel, rapidly transferring the heat generated during grinding and effectively reducing heat accumulation in the grinding zone. Simultaneously, the interface between the metal particles and the resin matrix generates microcracks during grinding, resulting in a toughening effect. Compared to the lower thermal conductivity of pure resin binders, this structure significantly improves the overall thermal conductivity of the diamond grinding wheel, avoiding thermal damage to the wafer surface caused by heat accumulation, such as microcracks or deepening of the subsurface damage layer. It also reduces binder softening and premature abrasive shedding at high temperatures, extending the service life of the grinding wheel.
[0010] Preferably, the metal powder is pretreated with a silane coupling agent, and the mass of the silane coupling agent is 0.5-3% of the mass of the metal powder. More preferably, the silane coupling agent is one of KH-550, KH-560, and KH-570.
[0011] Preferably, the volume fraction of the metal powder is 12-25%.
[0012] Preferably, the resin binder is one or more of phenolic resin, polyimide resin, epoxy resin, and bismaleimide resin.
[0013] Preferably, the thermally conductive filler is one or more of hexagonal boron nitride nanosheets, silicon carbide whiskers, nano-alumina, and graphene nanosheets.
[0014] Preferably, the solid lubricating filler is one or more of molybdenum disulfide, tungsten disulfide, graphite, and graphite oxide.
[0015] Preferably, the particle size D50 of the solid lubricating filler is 0.5-10μm, and the particle size of the diamond abrasive is 320# to 8000#.
[0016] By adopting the above technical solution, when the particle size of the solid lubricating filler is in the range of 0.5-10μm, the grinding wheel can play a better lubricating role during the grinding process. At the same time, diamond abrasive with appropriate particle size helps to improve grinding accuracy and efficiency.
[0017] Preferably, the pore-forming agent is one or more of phenolic resin microspheres, polymethyl methacrylate microspheres, polyvinyl alcohol microspheres, and ammonium bicarbonate particles, with a particle size D50 of 10-50 μm.
[0018] Preferably, the resin binder is cured by hot pressing to form a three-dimensional cross-linked network, and the metal powder is plastically deformed and cold-welded under hot pressing to form a continuous metal phase that is interspersed in the gaps of the three-dimensional cross-linked network. The resin three-dimensional cross-linked network and the continuous metal phase are interspersed and nested in space to form a resin-metal semi-interpenetrating network structure.
[0019] This application further provides a method for preparing a resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, comprising the following steps: S1. Metal powder pretreatment: Add the metal powder to an ethanol solution containing silane coupling agent, ultrasonically disperse for 15-30 min, stir at 60-80℃ for 1-2 h, filter and dry to obtain surface-modified metal powder. S2. Dry mix the resin binder, surface-modified metal powder, thermally conductive filler, and solid lubricating filler for 20-40 minutes, then add the wetting agent and continue mixing for 10-20 minutes. Finally, add the diamond abrasive and mix for 15-30 minutes. Sieve to obtain the molding material. S3. After hot pressing and curing the molding material, perform a stepped post-curing treatment, and then cool it with the furnace. S4. Process the cured grinding wheel blank to obtain a diamond grinding wheel; In step S3, the hot pressing temperature is 160-230℃ and the pressure range is 10-50MPa; the step-curing treatment in step S3 is as follows: heat preservation at 120-150℃ for 2-4 hours, heat preservation at 180-200℃ for 4-8 hours, and heat preservation at 200-220℃ for 2-4 hours.
[0020] By adopting the above technical solution, the stepped post-curing treatment involves heat preservation at different temperature stages. Heat preservation at 120-150℃ allows the resin binder to initially cure, stabilizing the basic structure of the grinding wheel. Prolonged heat preservation at 180-200℃ further promotes the resin cross-linking reaction, enhancing the bonding force between the binder and its components. A second heat preservation at 200-220℃ ensures complete curing of the binder, improving the hardness and strength of the grinding wheel. This stepped curing method avoids problems such as internal stress concentration and binder cracking that can occur with one-time high-temperature curing, resulting in a more uniform and stable internal structure of the grinding wheel, thereby improving its overall performance and service life.
[0021] In summary, this application has the following beneficial effects: 1. This application improves the thermal conductivity of the grinding wheel by adding metal powder and thermally conductive filler, reduces heat accumulation in the grinding zone, avoids abnormal phenomena such as microcracks and deepening of subsurface damage layer on the wafer surface, and the metal powder forms a semi-interpenetrating network structure in the resin matrix, which enhances the strength of the resin binder, improves heat resistance, prevents the resin binder from softening at high temperature and the abrasive from falling off prematurely, and extends the service life of the grinding wheel.
[0022] 2. Solid lubricating fillers can reduce friction during the grinding process, reduce heat generation, and further improve the grinding performance of the grinding wheel. Attached Figure Description
[0023] Figure 1 is a SEM microstructure of the fracture surface of the diamond grinding wheel obtained in Example 1 of this application, used to show the microstructure of the resin-metal semi-interpenetrating network described in this application. Detailed Implementation
[0024] The present application will be further described in detail below with reference to the embodiments. All details in this application, unless otherwise specified, are based on conventional conditions or conditions recommended by the manufacturer. All reagents or instruments, unless otherwise stated below, are commercially available conventional reagent products.
[0025] Example 1: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, comprising the following components by volume fraction: 25% 320# diamond, 42% polyimide resin (PMDA-ODA type, Tg=310℃), 18% Cu-Sn alloy powder (Sn content 10wt%, particle size D50 0.5μm, obtained by gas atomization), 8% hexagonal boron nitride nanosheets (sheet diameter 1-3μm, thickness 50nm), 4% molybdenum disulfide (D50 3μm), and 3% phenolic resin microsphere pore-forming agent (D50 30μm). Its preparation method includes the following steps: S1. Metal powder pretreatment: Cu-Sn alloy powder was added to an ethanol solution containing KH-550, ultrasonically dispersed for 15 min, stirred at 60℃ for 2 h, filtered, and dried to obtain surface-modified metal powder. The mass of KH-550 was 0.5% of the mass of Cu-Sn alloy powder. S2. Dry mix polyimide resin, surface-modified metal powder, hexagonal boron nitride nanosheets, molybdenum disulfide, and phenolic resin microsphere pore-forming agent for 20 minutes, then add wetting agent (acetone), wherein the amount of wetting agent (acetone) added is 5% of the mass of resin powder, continue mixing for 10 minutes, and finally add diamond abrasive and mix for 15 minutes, and sieve to obtain molding material. S3. Pour the molding material into the mold, and hot-press curing at a temperature of 200℃ and a pressure of 15MPa for 90 minutes. S4. Post-curing treatment: heat to 120℃ and hold for 4 hours, heat to 180℃ and hold for 8 hours, heat to 200℃ and hold for 4 hours, then cool with the furnace. S5. The cured grinding wheel blank is subjected to end face grinding, inner hole and outer circle machining to obtain a diamond grinding wheel.
[0026] Figure 1 The image shows the SEM microstructure of the fracture surface of the diamond grinding wheel obtained in the embodiment of this application. The image shows the resin cross-linked matrix, the Cu-Sn alloy particles overlapping to form a continuous metal channel, and the metal phase interspersed in the gaps of the resin network.
[0027] Example 2: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, comprising the following components by volume fraction: 30% 320# diamond, 30% polyimide resin (PMDA-ODA type, Tg=310℃), 13% epoxy resin (618 type, epoxy value 0.54eq / 100g, Tg=120℃), 12% Cu-Sn alloy powder (Sn content 10wt%, particle size D50 0.5μm, obtained by gas atomization), 5% silicon carbide whiskers, 5% tungsten disulfide (D50 0.5μm), 3% phenolic resin microsphere pore-forming agent (D50 30μm), and 2% polyvinyl alcohol microsphere pore-forming agent (D50 40μm). Its preparation method includes the following steps: S1. Metal powder pretreatment: Cu-Sn alloy powder was added to an ethanol solution containing KH-550, ultrasonically dispersed for 20 min, stirred at 70℃ for 1.5 h, filtered, and dried to obtain surface-modified metal powder. The mass of KH-550 was 0.5% of the mass of Cu-Sn alloy powder. S2. Dry mix polyimide resin, epoxy resin, surface-modified metal powder, silicon carbide whiskers, tungsten disulfide, phenolic resin microsphere pore-forming agent, and polyvinyl alcohol microsphere pore-forming agent for 30 min. Then add wetting agent (acetone), wherein the amount of wetting agent (acetone) added is 6% of the mass of resin powder. Continue mixing for 15 min. Finally, add diamond abrasive and mix for 25 min. Sieve to obtain molding material. S3. Pour the molding material into the mold, and heat-press curing at a temperature of 215℃ and a pressure of 40MPa for 30 minutes. S4. Post-curing treatment: heat to 135℃ and hold for 3 hours, heat to 190℃ and hold for 6 hours, heat to 210℃ and hold for 3 hours, then cool with the furnace. S5. The cured grinding wheel blank is subjected to end face grinding, inner hole and outer circle machining to obtain a diamond grinding wheel.
[0028] Example 3: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, comprising the following components by volume fraction: 15% 3000# diamond, 30% epoxy resin (type 618, epoxy value 0.54eq / 100g, Tg=120℃), 20% bismaleimide resin (Tg=340℃), 25% Cu-Sn alloy powder (Sn content 10wt%, particle size D50 0.5μm, obtained by gas atomization), 2% hexagonal boron nitride nanosheets (sheet diameter 1-3μm, thickness 50nm), 1% silicon carbide whiskers, 3% graphite (D50 10μm), 3% molybdenum disulfide (D50 5μm), and 1% ammonium bicarbonate granular pore-forming agent (D50 20μm). Its preparation method includes the following steps: S1. Metal powder pretreatment: Cu-Sn alloy powder was added to an ethanol solution containing KH-550, ultrasonically dispersed for 30 min, stirred at 80℃ for 1 h, filtered, and dried to obtain surface-modified metal powder. The mass of KH-550 was 0.5% of the mass of Cu-Sn alloy powder. S2. Dry mix epoxy resin, bismaleimide resin, surface-modified metal powder, hexagonal boron nitride nanosheets, silicon carbide whiskers, graphite, molybdenum disulfide, and ammonium bicarbonate granular pore-forming agent for 40 min, then add wetting agent (acetone), wherein the amount of wetting agent (acetone) added is 8% of the resin powder mass, continue mixing for 20 min, and finally add diamond abrasive and mix for 30 min, and sieve to obtain the molding material. S3. Pour the molding material into the mold, and heat-press curing at a temperature of 185℃ and a pressure of 25MPa for 60 minutes. S4. Post-curing treatment: heat to 150℃ and hold for 2 hours, heat to 200℃ and hold for 4 hours, heat to 220℃ and hold for 2 hours, then cool with the furnace. S5. The cured grinding wheel blank is subjected to end face grinding, inner hole and outer circle machining to obtain a diamond grinding wheel.
[0029] Example 4: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, comprising the following components by volume fraction: 22% 320# diamond, 15% polyimide resin (PMDA-ODA type, Tg=310℃), 10% phenolic resin (2123 type, Tg=140℃), 10% epoxy resin (618 type, epoxy value 0.54eq / 100g, Tg=120℃), 20% Cu-Sn alloy powder (Sn content 10wt%, particle size D50 0.5μm, obtained by gas atomization), 15% nano-alumina (D50 50nm), 7% molybdenum disulfide (D50 10μm), and 1% polyvinyl alcohol microsphere pore-forming agent (D50 30μm). Its preparation method includes the following steps: S1. Metal powder pretreatment: Cu-Sn alloy powder was added to an ethanol solution containing KH-550, ultrasonically dispersed for 15 min, stirred at 70℃ for 1 h, filtered, and dried to obtain surface-modified metal powder. The mass of KH-550 was 0.5% of the mass of Cu-Sn alloy powder. S2. Dry mix polyimide resin, phenolic resin, epoxy resin, surface modified metal powder, nano alumina, molybdenum disulfide, and polyvinyl alcohol microsphere pore-forming agent for 30 min, then add wetting agent (acetone), wherein the amount of wetting agent (acetone) added is 5% of the resin powder mass, continue mixing for 20 min, and finally add diamond abrasive and mix for 25 min, and sieve to obtain molding material. S3. Pour the molding material into the mold, and heat-press curing at a temperature of 215℃ and a pressure of 40MPa for 30 minutes. S4. Post-curing treatment: heat to 150℃ and hold for 2 hours, heat to 200℃ and hold for 4 hours, heat to 220℃ and hold for 2 hours, then cool with the furnace. S5. The cured grinding wheel blank is subjected to end face grinding, inner hole and outer circle machining to obtain a diamond grinding wheel.
[0030] Example 5: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, comprising the following components by volume fraction: 21% 320# diamond, 43% phenolic resin (type 2123, Tg=140℃), 8% Cu-Sn alloy powder (Sn content 10wt%, particle size D50 0.5μm, obtained by gas atomization), 10% graphene nanosheets (thickness 6-8nm, width 15μm), 5% hexagonal boron nitride nanosheets (sheet diameter 1-3μm, thickness 50nm), 8% graphite oxide (D50 3μm), and 5% polymethyl methacrylate microsphere pore-forming agent (D50 30μm). Its preparation method includes the following steps: S1. Metal powder pretreatment: Cu-Sn alloy powder was added to an ethanol solution containing KH-550, ultrasonically dispersed for 30 min, stirred at 60℃ for 2 h, filtered, and dried to obtain surface-modified metal powder. The mass of KH-550 was 0.5% of the mass of Cu-Sn alloy powder. S2. Phenolic resin, surface-modified metal powder, graphene nanosheets, hexagonal boron nitride nanosheets, graphene oxide, and polymethyl methacrylate microsphere pore-forming agent are dry-mixed for 30 minutes. Then, a wetting agent (acetone) is added, wherein the amount of wetting agent (acetone) added is 4% of the mass of the resin powder. Mixing is continued for 15 minutes. Finally, diamond abrasive is added and mixed for 15 minutes. The mixture is then sieved to obtain the molding material. S3. Pour the molding material into the mold, and heat-press curing at a temperature of 180℃ and a pressure of 30MPa for 70 minutes. S4. Post-curing treatment: heat to 120℃ and hold for 4 hours, heat to 180℃ and hold for 8 hours, heat to 200℃ and hold for 4 hours, then cool with the furnace. S5. The cured grinding wheel blank is subjected to end face grinding, inner hole and outer circle machining to obtain a diamond grinding wheel.
[0031] Example 6: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, which differs from Example 1 in that the Sn content in the Cu-Sn alloy powder is 5wt%, the particle size D50 is 8μm, and the other components and preparation process are the same as in Example 1.
[0032] Example 7: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, which differs from Example 1 in that the Sn content in the Cu-Sn alloy powder is 15wt%, the particle size D50 is 15μm, and the other components and preparation process are the same as in Example 1.
[0033] Example 8: A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, which differs from Example 1 in that step S1 is omitted, i.e., no surface treatment is performed on the Cu-Sn alloy powder, while the other steps are the same as in Example 1.
[0034] A polyimide resin diamond grinding wheel differs from Example 1 in that the grinding wheel does not contain Cu-Sn alloy powder, the amount of diamond abrasive is 35%, the amount of polyimide resin is 50%, and the other components and preparation process are the same as in Example 1.
[0035] A polyimide resin diamond grinding wheel differs from Example 1 in that copper powder and tin powder are used instead of Cu-Sn alloy powder. The volume percentage of copper powder is 15% and the volume percentage of tin powder is 3%. Other components, dosages, and preparation conditions are the same as in Example 1.
[0036] A polyimide resin diamond grinding wheel differs from Example 1 in that the particle size D50 of the Cu-Sn alloy powder is 25 μm, while the other components, dosages, and preparation conditions are the same as in Example 1.
[0037] A polyimide resin diamond grinding wheel differs from Example 1 in that the molybdenum disulfide particle size D50 is 20 μm, while the other components, dosages, and preparation conditions are the same as in Example 1.
[0038] A polyimide resin diamond grinding wheel differs from Example 1 in that an equal amount of Cu-Al alloy powder (Al content of 5wt%, D50 of 5μm) is used instead of Cu-Sn alloy powder, while other components, amounts, and preparation conditions are the same as in Example 1.
[0039] A polyimide resin diamond grinding wheel differs from Example 1 in that the post-curing treatment in step S4 is performed in a non-step manner, directly maintaining the temperature at 200°C for 16 hours, while the other steps are the same as in Example 1.
[0040] A polyimide resin diamond grinding wheel differs from Example 1 in that the post-curing treatment in step S4 is performed in a non-step manner, directly maintaining the temperature at 180°C for 16 hours, while the other steps are the same as in Example 1.
[0041] The thermal conductivity, grinding temperature during silicon carbide wafer grinding, wear ratio (grinding wheel life), feed rate, TTV, surface roughness of silicon carbide after grinding, and subsurface damage layer depth of the resin diamond grinding wheels obtained in the above embodiments and comparative examples were tested. The test results are shown in the table below.
[0042] Wear ratio = silicon carbide wafer thickness removed / diamond wheel wear amount; Wear ratio test conditions: install the diamond wheel on the JSG WG12D thinning machine, use an 8-inch silicon carbide wafer (initial thickness of 500μm, target thickness of 200μm) as the processing object, the wheel speed is 3000rpm, the table speed is 300rpm, the coolant (deionized water) flow rate is 8L / min, measure the wear amount of the wheel after continuous processing, and calculate the wear ratio = 300μm / wheel wear amount. The higher the wear ratio, the higher the wheel life.
[0043] TTV (Total Thickness Variation, a core indicator of silicon carbide wafer flatness): After grinding, the silicon carbide wafer is placed on a precision measurement platform, and a high-precision probe is used to scan along the wafer surface to calculate the difference between the maximum and minimum thickness, which is the TTV value.
[0044] Detection of the depth of the subsurface damage layer on a wafer: The test sample was prepared by cross-section polishing. The cross-section was obtained by cutting along the test area of the wafer with a focused ion beam (FIB) at an accelerating voltage of 30 kV and a beam current of 10 nA. The cross-sectional morphology was observed by transmission electron microscopy (TEM) or scanning electron microscopy (SEM). The vertical depth from the wafer processing surface to the crystal region without subsurface damage was measured in the cross-sectional image. At least 5 different locations were measured for each sample, and the average value was taken as the depth of the subsurface damage layer of the wafer.
[0045] Table 1 Results of various performance tests
[0046] The grinding temperature of the diamond grinding wheel obtained in this embodiment is lower than that in Comparative Example 1, and the wear ratio is higher than that in Comparative Example 1. This indicates that the wear of the grinding wheel in this embodiment is significantly lower than that in Comparative Example 1, thereby significantly improving the grinding wheel life. The change in total TTV thickness is lower than that in Comparative Example 1, indicating that the grinding wheel in this embodiment produces better flatness after grinding the silicon carbide wafer, with lower surface roughness and less subsurface damage, thus having higher application value.
[0047] Compared with Example 1, when copper powder and tin powder were used instead of Cu-Sn alloy powder, the grinding temperature of Comparative Example 2 increased significantly and the wear ratio decreased. This indicates that the wear of the grinding wheel in Comparative Example 2 was higher than that in Example 1, so the grinding wheel life was lower than that in Example 1. The feed rate was low during grinding, and the damage to the wafer subsurface was greater. This further demonstrates that the Cu-Sn alloy powder in this application can effectively improve the performance of the grinding wheel.
[0048] Compared with Example 1, when the particle size D50 of Cu-Sn alloy powder exceeded 15 μm, the thermal conductivity of the diamond grinding wheel in Comparative Example 3 decreased, the grinding temperature increased, the service life of the grinding wheel decreased, and the damage to the surface of the silicon carbide wafer was greater. The reason may be that when the particle size of the alloy powder is too large, the number of alloy powder particles is significantly reduced, the contact points between particles are greatly reduced, and an effective semi-interpenetrating network heat conduction channel cannot be formed in the resin matrix, so the thermal conductivity is reduced. In addition, large-diameter metal particles are prone to become stress concentration points during grinding, resulting in abnormal abrasive shedding and a significant reduction in grinding wheel life. Furthermore, large-diameter metal particles lead to a decrease in the uniformity of the grinding wheel structure, and the surface roughness and subsurface damage depth of the silicon carbide wafer after processing are significantly increased.
[0049] Compared with Example 1, in Comparative Example 4, when the particle size D50 of molybdenum disulfide is greater than 10 μm, it is difficult to disperse evenly in the resin binder, resulting in uneven lubrication and increased local frictional heat. More seriously, large-diameter molybdenum disulfide particles may fall off during grinding and get stuck between the grinding wheel and the wafer, scratching the wafer surface and causing a significant increase in wafer surface roughness.
[0050] Compared with Example 1, when Cu-Al alloy powder was replaced with an equal amount of Cu-Al alloy powder, the hardness of Cu-Al alloy was higher than that of Cu-Sn alloy. The degree of plastic deformation during hot pressing was reduced, the cold welding lap joint effect was weaker than that of Cu-Sn alloy, the continuity of the semi-interpenetrating network structure formed was poor, and the interfacial compatibility between Cu-Al alloy and resin matrix was not as good as that of Cu-Sn alloy. Therefore, the thermal conductivity and the overall performance of the grinding wheel were lower than those of Example 1.
[0051] Compared to Example 1, Comparative Examples 6-7, where post-curing treatment involved directly holding the material at 200℃ for 16 hours or 180℃ for 16 hours, lacked the slow curing process at low temperatures. This resulted in uneven resin crosslinking, stress concentration, and microcracks within the resin matrix, leading to lower thermal conductivity, mechanical properties, and service life of the grinding wheels compared to Example 1. Furthermore, the non-step-cured grinding wheels were more prone to micro-fractures in the resin binder during grinding due to internal stress release, causing increased grinding temperature and decreased processing quality. This further illustrates that simply extending the low-temperature curing time cannot compensate for the adverse effects of lacking a step-heating process. The embodiments described in this specific implementation are merely preferred embodiments of this application and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made to the structure, shape, and principle of this application should be included within the scope of protection of this application.
Claims
1. A resin-metal semi-interpenetrating network composite bonded diamond grinding wheel, characterized in that, It includes the following components by volume fraction: diamond abrasive 15-30%, resin binder 35-55%, metal powder 8-25%, thermally conductive filler 3-15%, solid lubricating filler 1-8%, and pore-forming agent 1-5%.
2. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The metal powder is a Cu-Sn alloy powder, wherein the Sn content is 5-15wt% and the particle size D50 of the metal powder is 0.5-15μm.
3. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The volume fraction of the metal powder is 12-25%.
4. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The metal powder is pretreated with a silane coupling agent, the mass of which is 0.5-3% of the mass of the metal powder.
5. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The resin binder is one or more of phenolic resin, polyimide resin, epoxy resin, and bismaleimide resin.
6. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The thermally conductive filler is one or more of hexagonal boron nitride nanosheets, silicon carbide whiskers, nano-alumina, and graphene nanosheets.
7. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The solid lubricating filler is one or more of molybdenum disulfide, tungsten disulfide, graphite, and graphite oxide.
8. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The particle size D50 of the solid lubricating filler is 0.5-10μm, and the particle size of the diamond abrasive is 320# to 8000#.
9. The resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to claim 1, characterized in that: The pore-forming agent is one or more of phenolic resin microspheres, polymethyl methacrylate microspheres, polyvinyl alcohol microspheres, and ammonium bicarbonate particles, with a particle size D50 of 10-50 μm.
10. A method for preparing a resin-metal semi-interpenetrating network composite bonded diamond grinding wheel according to any one of claims 1-9, characterized in that: Includes the following steps: S1. Metal powder pretreatment: Add the metal powder to an ethanol solution containing silane coupling agent, ultrasonically disperse for 15-30 min, stir at 60-80℃ for 1-2 h, filter and dry to obtain surface-modified metal powder. S2. Dry mix the resin binder, surface-modified metal powder, thermally conductive filler, and solid lubricating filler for 20-40 minutes, then add the wetting agent and continue mixing for 10-20 minutes. Finally, add the diamond abrasive and mix for 15-30 minutes. Sieve to obtain the molding material. S3. After hot pressing and curing the molding material, perform a stepped post-curing treatment, and then cool it with the furnace. S4. Process the cured grinding wheel blank to obtain a diamond grinding wheel; In step S3, the hot pressing temperature is 160-230℃ and the pressure range is 10-50MPa; the step-curing treatment in step S3 is as follows: heat preservation at 120-150℃ for 2-4 hours, heat preservation at 180-200℃ for 4-8 hours, and heat preservation at 200-220℃ for 2-4 hours.