A method of curing concrete applied to the interior surface of a steel form
By coating the inner surface of the steel formwork with a water-based release and curing agent, an adhesive-reversing isolation coating is formed by the concrete hydration reaction, which solves the problem of separation between the release and curing processes in traditional construction. This achieves a seamless water retention and curing effect, avoiding early micro-cracks and resource waste.
Patent Information
- Application Number
- CN202611367041.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-24
AI Technical Summary
The "curing gap" caused by the separation of demolding and curing processes in traditional concrete construction can easily induce early microcracks. Furthermore, the incompatibility between the release agent and the curing agent leads to the failure of the water-retaining barrier, resulting in the waste of a large amount of water resources and labor costs.
A water-based release and curing agent is applied to the inner surface of the steel formwork to form an isolation coating. The physical and chemical cross-linking activated by the concrete hydration reaction makes the adhesion between the isolation coating and the concrete surface surpass that of the steel formwork, forming a continuous curing film, achieving water retention and sealing, and avoiding the time gap between demolding and curing.
It effectively avoids micro-cracks caused by early moisture loss, overcomes the interface defects of release agent residue repelling curing agent, achieves efficient water retention and curing without manual watering, optimizes construction efficiency and saves water resources.
Smart Images

Figure CN123150145A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of concrete building material curing technology, specifically to a method for curing concrete by coating the inner surface of a steel mold. Background Technology
[0002] In existing precast concrete component or cast-in-place structure construction projects, the use of steel formwork is a common industry practice. Traditional construction techniques typically treat demolding and curing as two completely separate physical and temporal processes: first, a mineral oil-based or emulsified oil-based release agent is applied to the inner surface of the steel formwork to meet physical demolding requirements; after the concrete reaches demolding strength and demolding is carried out, a water-based or solvent-based curing agent is sprayed onto the exposed concrete surface, or manual continuous watering is used for post-curing. However, with the increasing demands for early appearance quality and internal durability of concrete, the above-mentioned traditional process has revealed the following two major technical defects in practical engineering applications: First, the unavoidable time gap between demolding and post-curing processes easily induces early drying shrinkage microcracks in concrete. In the initial stage after pouring, concrete is at the peak of its hydration reaction, releasing a large amount of heat of hydration. In traditional processes, the instant the steel formwork is removed, the concrete surface, at a high core temperature, is suddenly exposed to a relatively dry and cool atmospheric environment. Before subsequent curing measures (such as spraying curing agents or covering with water) are implemented, capillary pore water on the concrete surface evaporates and escapes into the atmosphere at a high rate, driven by both high temperature and external humidity gradients. This unobstructed early moisture escape leads to severe volume shrinkage of the concrete surface. When the early tensile strength of the concrete is insufficient to resist the drying shrinkage stress, irreversible network microcracks are easily induced on the concrete surface, thus reducing the overall durability of the component.
[0003] Secondly, an interfacial repulsion effect exists between residual release agent and post-curing agent, leading to the failure of the water-retaining barrier. Traditional release agents rely on low-polarity hydrophobic substances to form an isolation layer on the steel mold surface. After demolding, some hydrophobic oily substances inevitably remain and become embedded in the micropores of the concrete surface. When conventional curing agents are subsequently sprayed onto the concrete surface, the residual oily substances significantly reduce the solid-phase surface free energy of the concrete surface, preventing the liquid curing agent from achieving uniform wetting and distribution. The liquid curing agent is prone to localized shrinkage or aggregation due to surface tension, resulting in a discontinuous coating with uneven thickness or numerous pinholes after curing. This discontinuous physical film cannot effectively seal the capillary channels of the concrete surface, leading to persistently high water vapor permeability and ultimately a significant reduction in the actual water-retaining capacity of the post-curing agent. Summary of the Invention
[0004] This invention aims to solve the problem of "curing gap" caused by the separation of demolding and curing processes in traditional concrete construction. In particular, it addresses the technical pain points of microcracks easily generated in the early hydration and heat release stage of concrete, the incompatibility between traditional release agents and curing agents, and the high water and labor costs of traditional curing methods.
[0005] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a concrete curing method for coating the inner surface of a steel formwork, comprising the following steps: S100, before the steel formwork is installed, a water-based release and curing agent is applied to the inner surface of the steel formwork that is in contact with the concrete, and after it dries completely, an isolation coating with initial adhesion is formed on the inner surface. S200, assemble the steel formwork and pour concrete. During the curing stage with the formwork, the isolation coating forms a water-retaining and sealing layer between the steel formwork and the concrete. At the same time, the isolation coating is activated by the hydration reaction of the concrete, causing the isolation coating to bond with the surface of the concrete, and its adhesion to the concrete surface increases accordingly. S300, after the concrete reaches the demolding strength, the steel formwork is removed. Due to the fact that the adhesion of the isolation coating to the concrete surface is greater than its initial adhesion to the steel formwork, the isolation coating is peeled off from the inner surface of the steel formwork and transferred to the surface of the concrete to form a curing film. S400, after the steel formwork is removed, the concrete is continuously moisturized and cured using the curing film transferred to the concrete surface.
[0006] Furthermore, prior to step S100, a step of pre-treating the base of the steel template is also included; The substrate pretreatment specifically involves removing the adhering substances from the inner surface of the steel template until the metal substrate is exposed, and keeping the inner surface dry and free of standing water.
[0007] Further, in step S100, the film thickness of the isolation coating is controlled to be 20-50 micrometers; preferably, the water-based release and curing agent is uniformly coated on the inner surface by airless spraying, roller coating or brush coating.
[0008] Furthermore, the polymer film-forming base material of the water-based release and curing agent simultaneously contains hydrophobic segments and alkali-sensitive hydrophilic groups; When the isolation coating is in a fully dry state, the hydrophobic segments face the side of the steel template to provide the initial adhesion and release isolation effect to the steel template.
[0009] Furthermore, during the pouring and curing process in step S200: During the pouring and compaction of the concrete, the vibration equipment is kept at a preset distance from the inner surface of the steel formwork to prevent physical damage to the integrity of the isolation coating. Furthermore, the curing stage under the formwork shall last for no less than 3 days to ensure that the hydration reaction of the concrete is fully carried out, so that the adhesion of the isolation coating to the concrete surface reaches the critical threshold that meets the subsequent peeling and transfer conditions.
[0010] Furthermore, in step S200, the activation of the isolation coating by the concrete hydration reaction specifically includes the following microscopic physicochemical changes: During the hydration process of the concrete, heat of hydration is released at the solid-liquid interface where it adheres to the isolation coating, forming a highly alkaline environment. The alkali-sensitive hydrophilic groups in the isolation coating facing the concrete side undergo polar bonding or micro-crosslinking reactions with the hydrated calcium silicate gel precipitated on the concrete surface under the dual stimulation of the highly alkaline environment and the heat of hydration, thereby causing the adhesion of the isolation coating to the concrete surface to continuously increase with the hydration process.
[0011] Furthermore, in step S300, the process of peeling and transferring the isolation coating from the inner surface of the steel template is specifically manifested as the in-situ overall peeling of the phase interface. At the moment the steel formwork is removed, based on the mechanical reversal characteristic that the adhesion of the isolation coating to the concrete surface is greater than its initial adhesion to the steel formwork, the isolation coating completely detaches from the metal substrate of the steel formwork and transforms in situ into the curing film adhering to the concrete surface without damage.
[0012] Furthermore, the curing film transferred and attached to the concrete surface is continuous and semi-transparent; Furthermore, the curing film tightly covers the surface micropores of the concrete to form a closed barrier between the concrete and the outside air, preventing the evaporation of moisture from the inside of the concrete.
[0013] Furthermore, during the continuous water retention curing in step S400: the moisture balance inside the concrete is maintained independently by the extremely low water vapor permeability of the curing film, without the need for and to avoid additional water replenishment to the surface of the concrete; and the cycle of water retention curing using the curing film is not less than 14 days.
[0014] Furthermore, the curing film possesses environmental self-degradation characteristics; after the water-retaining curing cycle ends, the curing film undergoes photodegradation or weathering and powdering when exposed to the natural environment, without the need for physical peeling or chemical cleaning, so that subsequent construction operations can be carried out directly on the concrete surface. Beneficial effects
[0015] This invention utilizes a water-based release and curing agent containing hydrophobic segments and alkali-sensitive hydrophilic groups. During the concrete hydration stage with the formwork in place, it leverages a high-temperature, strongly alkaline microenvironment to trigger physicochemical cross-linking at the phase interface. This allows the coating's adhesion to the concrete to surpass its adhesion to the steel formwork, enabling the coating to be completely peeled off in situ and transferred to the concrete surface as a film upon demolding. This method places the curing action before demolding, eliminating the gap between demolding and curing in terms of physical timing. This effectively avoids micro-cracks caused by early moisture loss from the concrete surface. It also overcomes the interface defect in traditional processes where release agent residue repels the curing agent film. The formed curing film independently maintains high humidity inside the concrete due to its extremely low water vapor permeability, eliminating the need for manual watering. Furthermore, the film exhibits natural photodegradation characteristics, significantly optimizing the efficiency of subsequent finishing work while saving water resources. Attached Figure Description
[0016] Figure 1 This is a flowchart illustrating the overall process flow of the present invention. Figure 2 This is a cross-sectional view of the interface structure during the coating and film-forming stage of the present invention. Figure 3 This is a comparison diagram of the anhydrous water retention and photodegradation processes of the present invention. Detailed Implementation
[0017] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0018] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but includes other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.
[0019] The present invention will now be described in further detail with reference to the accompanying drawings: Example
[0020] like Figures 1 to 3 As shown, a method for curing concrete applied to the inner surface of a steel mold includes the following steps: S100, before the steel formwork is installed, a water-based release and curing agent is applied to the inner surface of the steel formwork in contact with the concrete. After it dries completely, an isolation coating with initial adhesion is formed on the inner surface. S200, assembling steel formwork and pouring concrete, during the curing stage with the formwork, the isolation coating forms a water-retaining and sealing layer between the steel formwork and the concrete. At the same time, the isolation coating is activated by the hydration reaction of the concrete, causing the isolation coating to bond with the surface of the concrete, and its adhesion to the concrete surface increases accordingly. S300: After the concrete reaches the demolding strength, the steel formwork is removed. Because the adhesion of the isolation coating to the concrete surface is greater than its initial adhesion to the steel formwork, the isolation coating peels off from the inner surface of the steel formwork and transfers to the surface of the concrete to form a curing film. S400 utilizes a curing film transferred to the concrete surface to continuously maintain the concrete's moisture content after the steel formwork is removed.
[0021] Furthermore, the specific implementation process of step S100 is as follows: Step S100 specifically covers the pretreatment of the steel formwork substrate, the microscopic film-forming mechanism of the water-based release and curing agent, and strict control of coating construction parameters.
[0022] Before applying the water-based release and curing agent, the steel formwork substrate is pre-treated. The pre-treatment involves using an angle grinder with a wire wheel or industrial sandblasting equipment to physically grind the inner surface of the steel formwork that contacts the concrete. This removes rust, residual cement paste, and oil deposits until the entire metal substrate is exposed. To ensure proper wetting and spreading of the water-based release and curing agent in its liquid state and its physical anchoring force after curing, the surface roughness Ra of the metal substrate is strictly controlled within the range of 1.6 to 3.2 micrometers by adjusting the abrasive particle size and grinding speed. After physical grinding, the inner surface is blown with high-pressure oil-free compressed air, and then kept absolutely dry and free of standing water under natural conditions or heating conditions using an industrial hot air blower.
[0023] Regarding the material composition and film-forming mechanism of the water-based release and curing agent, it is a polymer composite system using water as the continuous phase dispersion medium. The polymer film-forming base of the water-based release and curing agent is copolymerized and grafted with two types of microscopic functional groups of opposite polarities, comprising low-polarity hydrophobic segments and high-polarity alkali-sensitive hydrophilic groups. Specifically, the hydrophobic segments are composed of polysiloxane segments or long-chain alkyl groups; the alkali-sensitive hydrophilic groups are composed of carboxyl groups (-COOH) and active hydroxyl groups (-OH). After liquid-phase coating, as the water dispersion medium evaporates, the system transitions from a liquid phase to a solid phase. During the curing physical changes, based on the principle of minimum surface free energy in thermodynamic systems, the low-surface-energy hydrophobic segments spontaneously orient and accumulate towards the metal substrate of the steel template, and bond with the metal substrate through van der Waals forces, providing initial adhesion to the steel template. Meanwhile, the hydrophobic segments construct a steric hindrance layer on the inner surface, blocking the direct contact between the cement hydrates produced by subsequent pouring and the metal substrate; while the alkali-sensitive hydrophilic groups are enriched and exposed on the side away from the metal substrate (i.e. the side facing the concrete interface later) under polar repulsion, forming a high potential energy surface with chemical reactivity, ready to be directionally excited in the subsequent highly alkaline hydration environment.
[0024] As a preferred embodiment, the polymeric film-forming base material of the waterborne release and curing agent specifically adopts a styrene-acrylate copolymer waterborne emulsion or waterborne polyurethane resin with side-chain carboxyl functional groups. The low-polarity hydrophobic segments are composed of long-chain fatty acid ester groups or polydimethylsiloxane segments, with a mass ratio controlled between 55% and 70% of the total solid content of the system; the high-polarity alkali-sensitive hydrophilic groups are provided by side-chain carboxyl groups (-COOH), with an acid value controlled between 35 mg KOH / g and 60 mg KOH / g. By precisely controlling the above acid value range, it ensures steric stability during normal neutral or slightly acidic liquid spraying, while encountering a strongly alkaline cement hydration microenvironment with a pH greater than 12, the carboxyl groups undergo instantaneous dissociation, providing sufficient active anion sites for subsequent interfacial ionic bonding.
[0025] For the coating application, a high-pressure airless spraying system is used to uniformly spray a homogenized water-based release and curing agent onto the pre-treated inner surface. The system pressure of the airless spraying system is set to 12 MPa to 15 MPa, and it is equipped with a fan-shaped spray nozzle with an orifice diameter of 0.015 inches to 0.019 inches. During the application, the spray gun nozzle axis is vertically aligned with the inner surface, the vertical distance between the nozzle tip and the inner surface is maintained between 250 mm and 300 mm, the spray gun movement speed is constantly controlled between 400 mm / s and 500 mm / s, and the overlap of the coating width between two adjacent spray strokes is set to 50%.
[0026] By adjusting the flow rate and spray gun speed of the spraying equipment, the dry film thickness of the cured isolation coating is strictly controlled between 20 and 50 micrometers. Within this thickness range, the isolation coating possesses sufficient mechanical toughness to withstand the shear friction stress generated by subsequent concrete pouring and vibration, while also limiting the disorderly growth of internal shrinkage stress within the coating, preventing cohesive failure or premature peeling of the isolation coating on the metal substrate surface. After coating, the coating is left to dry in an atmospheric environment. Once all moisture has evaporated and a finger pressure test shows no physical indentation, the isolation coating is considered to have reached a fully dry state, completing step S100.
[0027] Experimental verification scenario: To verify the physical influence of the dry film thickness parameter of the isolation coating on the final demolding integrity and transfer state, a set of specific comparative experimental scenarios are provided here.
[0028] The experiment used a standard cubic cast steel mold with dimensions of 150 mm × 150 mm × 150 mm. The inner surfaces of the five sets of molds underwent identical substrate pretreatment to ensure a uniform surface roughness Ra of 2.5 micrometers. Then, water-based release and curing agents of varying thicknesses were sprayed onto each mold using a high-pressure airless spraying device. After the release coating had fully dried, C30 grade silicate cement concrete blocks with the same water-cement ratio were poured. After curing in the mold for 72 hours, physical demolding was performed. The residual state of the steel mold metal substrate surface and the physical characterization of the integrity of the transfer film on the concrete surface were recorded and observed. Specific experimental parameters and observation records are shown in Table 1.
[0029] As shown in Table 1, strictly controlling the film thickness within the range of 20 to 50 micrometers is a key physical parameter threshold to ensure that the isolation coating can successfully detach from the metal substrate and be transferred intact to the concrete surface in a continuous film form. Exceeding this range will cause micromechanical damage, leading to the failure of the curing barrier.
[0030] Furthermore, the specific implementation process of step S200 is as follows: Step S200 specifically covers the operational specifications for steel formwork assembly and concrete pouring, as well as the interfacial physicochemical crosslinking mechanism of the isolation coating in a hydration microenvironment.
[0031] After the water-based release and curing agent has dried and formed a film, the assembly of steel formwork and concrete pouring proceed. According to the engineering structural design dimensions, multiple steel formwork panels are locked and fixed using joint connectors to ensure no physical gaps for grout leakage at the joints. Concrete is then placed into the mold cavity formed by the assembled steel formwork. After the concrete is placed, an immersion vibrator is used for compaction. During the mechanical vibration stage, a preset distance of 50 mm to 80 mm is strictly maintained between the working end of the vibrator and the inner surface coated with the release coating. This preset distance is designed to prevent direct physical collision between the rigid vibrator and the dried release coating while the liquid concrete undergoes rheological compaction through high-frequency vibration, thus avoiding localized damage to the release coating or premature peeling from the metal substrate caused by mechanical shear stress.
[0032] After the concrete is vibrated and compacted and the surface finishing is completed, the curing stage begins. During this stage, the silicate cement clinker mineral phases (including tricalcium silicate and dicalcium silicate) inside the concrete spontaneously undergo a vigorous hydration reaction with the mixing water. This hydration reaction is accompanied by a large amount of free calcium hydroxide. The crystallization and precipitation of ions release a large amount of hydration exothermic peaks. The above-mentioned exothermic and hydration ion precipitation phenomena cause the local microenvironment temperature at the solid-liquid interface where the concrete and the isolation coating are in direct contact to rise rapidly to 40 degrees Celsius to 65 degrees Celsius. At the same time, a highly alkaline liquid microenvironment with a stable pH value between 12.5 and 13.5 is established at the solid-liquid interface.
[0033] Under the combined physicochemical excitation of the aforementioned high-temperature and highly alkaline liquid-phase microenvironment, the alkali-sensitive hydrophilic groups (including carboxyl-COOH and hydroxyl-OH) located on the outer side of the isolation coating and facing the concrete undergo a directional deprotonation reaction, transforming in situ into anionic segments with highly polar negative charges. As the concrete hydration process progresses, a large number of nanoscale hydrated calcium silicate gels (CSH gels) generated on the concrete surface continuously grow towards the phase interface. The deprotonated anionic segments interact with calcium ions in the hydrated calcium silicate gel lattice. A strong ionic bonding reaction occurs, establishing a polar micro-crosslinked curing network across the interface. Simultaneously, the growing hydrated calcium silicate gel crystals continuously embed into the microporous structure of the isolation coating surface, superimposing to form a nanoscale mechanical anchoring and intercalation.
[0034] The dual mechanism of ionic bonding and mechanical anchoring leads to an exponential increase in the adhesion of the isolation coating to the concrete surface. To ensure that the reaction conversion rate of the aforementioned micro-crosslinking reaction reaches the critical threshold, the curing time in the formwork is strictly limited to no less than 72 hours (i.e., 3 days). After reaching this time span, the adhesion strength of the isolation coating to the concrete surface completely surpasses the van der Waals force of the hydrophobic segments within the isolation coating on the steel formwork metal substrate, achieving a complete reversal of the adhesion mechanical state at the phase interface.
[0035] For different construction operation environments, the time threshold for curing with formwork in step S200 is dynamically and adaptively adjusted: When the ambient temperature at the construction site is between 5 and 15 degrees Celsius during winter or low-temperature seasons, the duration of the curing stage with formwork is extended to 120 to 168 hours (i.e., 5 to 7 days) due to the slowdown in cement hydration reaction rate and the delayed release of hydration heat, to ensure that the amount of hydrated calcium silicate gel generated and the ion bonding conversion rate at the phase interface reach the aforementioned critical threshold; When the ambient temperature at the construction site is above 35 degrees Celsius during summer or high-temperature and windy seasons, the cement hydration reaction intensifies, and the duration of the curing stage with formwork can be shortened to 48 to 60 hours, but necessary shading and moisturizing measures must be taken on the outside of the assembled steel formwork to prevent excessive shrinkage stress inside the isolation coating caused by excessive local water loss.
[0036] Experimental verification scenario: To accurately determine the quantitative impact of curing time under mold and pH value of the hydration microenvironment on the reversal phenomenon of interfacial adhesion, a set of mechanical pull-out test scenarios is presented. The experiment employed a hydraulic pull-out apparatus equipped with a digital display force gauge. In a standard curing chamber under strictly controlled temperature and humidity conditions, positive pull-out failure tests were performed on concrete-coating-steel plate composite layers with different curing times under mold. The critical pull-out force of the coating against the steel plate side (defined as the initial adhesion force) was recorded. The critical pull-out force of the coating against the concrete side (defined as the derived adhesion) and the degree of peeling. The specific test parameters and fracture state of the pull-out failure surface are shown in Table 2. Table 2: Test Record of the Effect of Curing Time on the Mechanical Evolution of Coating Interfacial Adhesion:
[0037] The pull-out mechanics test data in Table 2 clearly reveal that when the curing time with the formwork is less than 48 hours, due to the low pH value of the interfacial microenvironment and insufficient hydration reaction conversion rate, the anionic segments fail to establish a sufficient ionic bonding network. Forcibly removing the formwork at this time will inevitably result in the isolation coating failing to adhere to the concrete surface. Conversely, when the curing time with the formwork exceeds 72 hours, the interfacial microenvironment reaches the strongly alkaline triggering condition. The numerical breakthrough has achieved a breakthrough and established an absolute dominant position, thus establishing the necessary and sufficient mechanical conditions for the subsequent in-situ peeling of the overall phase interface.
[0038] Furthermore, the specific implementation process of step S300 is as follows: Step S300 specifically covers non-destructive demolding operation based on mechanical reversal mechanism, and the physical characteristics of thin film transformation morphology after in-situ overall peeling off of phase interface.
[0039] Once the concrete's cured strength reaches the standard demolding strength defined in the building structural design code, the demolding and transfer peeling operation begins. Construction workers release the locking bolts and joint connectors securing the external steel formwork and apply normal tensile stress along a direction perpendicular to the normal to the metal substrate, forcing the steel formwork to shift outwards. During the transient phase of releasing the formwork constraint with normal tensile stress, combined with the mechanical boundary conditions established in step S200, the derivative adhesion of the isolation coating to the concrete surface numerically surpasses its initial adhesion to the metal substrate. Simultaneously, based on the rheological properties of polymers, the interwoven macromolecular chains within the dry state of the isolation coating possess an internal cohesive force higher than the initial adhesion to the metal substrate.
[0040] Under the combined effect of the aforementioned mechanical boundary conditions, when the externally applied demolding tensile stress exceeds the physical critical point of the van der Waals force on the metal substrate, the fracture failure surface is precisely limited to the physical contact surface between the hydrophobic segments of the isolation coating and the metal substrate. The isolation coating detaches completely from the metal substrate of the steel formwork, and no large-scale elastic deformation cracking or cohesive tearing occurs during the peeling force transmission, achieving 100% in-situ overall peeling of the phase interface. With the complete removal of the steel formwork, the isolation coating, which originally relied on the inner surface of the metal substrate, transforms in situ into a curing film tightly adhering to the concrete surface without any displacement deviation in physical space.
[0041] The curing film, transferred and attached to the concrete surface, appears as a continuously distributed, semi-transparent structure in its macroscopic optical appearance. At the microscopic topological level, the curing film, through its initial liquid-phase distribution and the nanoscale mechanical interlocking formed during the hydration reaction, seamlessly covers and seals the gaps between the hydrated calcium silicate crystals and the capillary microporous network on the concrete surface. By blocking the connection between these capillary pores and the external atmosphere, the curing film constructs a closed barrier between the concrete and the outside air, preventing the outward permeation and diffusion of liquid water molecules and gaseous water vapor. This establishes the structural foundation for subsequently maintaining the internal humidity balance of the concrete independently.
[0042] Experimental verification scenario: To quantify and verify the integrity of in-situ overall peeling caused by the phase interface mechanical reversal phenomenon, and the water vapor transmission rate blocking efficiency after film formation, a set of image recognition analysis and water vapor transmission rate test experiments are presented. Three solid concrete shear wall test sections with a surface area of 2 square meters were selected for the experiment. The control group was treated with a conventional mineral oil-based release agent and manually sprayed with a conventional water-based curing agent; test group 1 used a 30-micron thick water-based release and curing agent; test group 2 used a 45-micron thick water-based release and curing agent. All test wall sections underwent standard demolding operations under the same meteorological conditions and after 72 hours of curing in the formwork. After demolding, a high-precision surface defect optical scanner was used to perform a gridded scan of the coating coverage integrity on the wall section surface and image algorithm area integration to calculate the percentage of the physical transfer film area. Subsequently, a water vapor transmission rate tester (cup method, test conditions: ambient temperature 38 degrees Celsius, relative humidity 90%) was used to in-situ cut surface slices with the film on the wall section surface for water vapor transmission rate (WVTR) testing. The specific test parameters and data are shown in Table 3: Table 3: Comparison of Thin Film In-situ Transfer Integrity and Surface Moisture Barrier Performance Tests
[0043] The cross-test data of optical scanning calculations and water vapor transmission rate in Table 3 clearly reveal that by strictly controlling the film thickness and establishing mechanical reversal conditions, the isolation coating achieved a physical in-situ transfer coverage rate of over 99% during the peeling process. The extremely excellent continuous coverage ensured an extremely low water vapor transmission rate, verifying from a physical testing perspective that the protective film fully possesses a strong sealing function that blocks the outward migration and diffusion of water molecules.
[0044] Furthermore, the specific implementation process of step S400 is as follows: The following details step S400 of the concrete curing method applied to the inner surface of the steel mold. Step S400 specifically covers the operational specifications for continuous curing using the film generated in situ from the preceding steps for anhydrous media intervention, as well as the connection mechanism between the natural degradation of the film's polymer chain segments and subsequent construction operations.
[0045] After demolding and confirmation of complete coverage by the curing film, a continuous water-retaining curing cycle begins. During this period, the curing film, adhering to the concrete surface, forms a closed barrier, cutting off the evaporation and escape path of pore water from the concrete to the dry external atmosphere. Due to its extremely low water vapor permeability, the curing film independently impedes the interfacial mass transfer of water molecules, maintaining a balanced humidity gradient and high autogenous relative humidity within the concrete. This allows the deep, unhydrated cement clinker particles to continue their hydration reaction in a constant, water-filled microporous environment.
[0046] During the designated water-retention curing period of no less than 14 days, strict restrictions on on-site operational interventions are enforced: any additional moisture replenishment operations, such as spraying, sprinkling, or covering with wet materials, on the concrete surface are prohibited. The purpose of implementing the aforementioned negative restrictions is that concrete components in the hydration exothermic stage have a high internal core temperature. If low-temperature liquid water is sprayed directly onto the surface, it will instantly generate a huge abrupt change in the thermodynamic temperature gradient of the concrete surface. The huge temperature shrinkage stress, combined with the low tensile strength of the early concrete, can easily induce high-density micro-network shrinkage cracks that penetrate the surface. Relying on the self-locking water mechanism of the curing film, the risk of thermodynamic cracking caused by external cold water shock is completely eliminated from the source of physical operation.
[0047] After the set water retention and curing period ends, the process enters the stage of environmental self-degradation of the surface film and connection with subsequent construction operations. Under conditions of complete exposure to the outdoor natural environment, the polymer film-forming matrix in its constituent system continuously absorbs ultraviolet photon energy from the natural sunlight spectrum. Ultraviolet photons with energy higher than the dissociation energy of polymer chemical bonds cause photochemical oxidation and bond breaking degradation of covalent bonds on the polymer backbone, triggering the breakage and depolymerization of macroscopic macromolecular chain segments; at the same time, the alternating diurnal temperature difference and cyclical changes in atmospheric humidity further accelerate the physical weathering and embrittlement of the polymer three-dimensional network structure.
[0048] With the continuous superposition of the aforementioned photochemical oxidative degradation and physical weathering, the curing film gradually loses its continuous physical structural strength and interfacial adhesion to the concrete surface within the 30-60 day exposure period, eventually resulting in powdering and peeling. The microscopic residue after complete powdering and degradation is inert powder form and does not possess the oil-based hydrophobic barrier effect of traditional mineral oil-based release agents. Therefore, after the powdering and degradation cycle is completed, on-site construction personnel do not need to use high-pressure water jets, manual scraping, mechanical grinding wheels, or chemical cleaning solvents for any surface removal work. They can directly apply building leveling layers, finishing plaster, or exterior wall decorative coatings to the self-degraded concrete surface. The residue does not hinder the subsequent crystal intercalation and chemical bonding between cement-based or polymer-based building mortar and the concrete surface substrate.
[0049] Experimental verification scenario: To quantify and verify the water-retention efficiency of the waterless isolation method and its actual impact on the interfacial bonding strength after self-degradation, a series of full-cycle solid component tests were conducted. Three groups of C40 strength grade reinforced concrete wall and column components were cast. Control group 1 underwent continuous manual watering for 7 days after demolding; control group 2 underwent demolding with a conventional release agent followed by surface spraying with a commercially available film-forming curing agent; the experimental group followed the entire standard procedure from S100 to S400, with strict prohibition of external watering during the curing period, followed by 30 days of natural environmental exposure for degradation. After reaching the specified age, a pre-embedded humidity sensor was used to read the internal relative humidity at the center of the component, and standard core samples were drilled to test the 28-day axial compressive strength. Simultaneously, a 5 mm thick standard polymer cement mortar leveling layer was uniformly applied to the surface of the components after 30 days of exposure. After curing, a pull-out tester was used to test the interfacial bond pull-out strength between the mortar layer and the substrate. Specific test parameters and mechanical data are shown in Table 4. Table 4: Humidity retention rate during waterless curing and interfacial adhesion mechanical tests after environmental degradation:
[0050] The comprehensive mechanical and humidity monitoring cross-test data in Table 4 clearly reveal that by strictly implementing the S400 step without additional water intervention, the relative humidity inside the component is locked at an extremely high level of 96.8%, which promotes the maximum development of strength after 28 days. Moreover, the natural light degradation and pulverization characteristics completely eliminate the hidden dangers of hydrophobic isolation at the interface, resulting in an interfacial bond pull-out strength of up to 1.15 MPa for the subsequent leveling layer, which far exceeds that of ordinary curing agents. This physically verifies the core value of self-degradation characteristics in achieving seamless connection of processes.
[0051] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for curing concrete applied to the inner surface of a steel mold, characterized in that, Includes the following steps: S100, before the steel formwork is installed, a water-based release and curing agent is applied to the inner surface of the steel formwork that is in contact with the concrete. After it dries completely, an isolation coating with initial adhesion is formed on the inner surface. S200, assemble the steel formwork and pour concrete. During the curing stage with the formwork, the isolation coating forms a water-retaining and sealing layer between the steel formwork and the concrete. At the same time, the isolation coating is activated by the hydration reaction of the concrete, causing the isolation coating to bond with the surface of the concrete, and its adhesion to the concrete surface increases accordingly. S300, after the concrete reaches the demolding strength, the steel formwork is removed. Due to the fact that the adhesion of the isolation coating to the concrete surface is greater than its initial adhesion to the steel formwork, the isolation coating is peeled off from the inner surface of the steel formwork and transferred to the surface of the concrete to form a curing film. S400, after the steel formwork is removed, the concrete is continuously moisturized and cured using the curing film transferred to the concrete surface.
2. The method for curing concrete applied to the inner surface of a steel mold according to claim 1, characterized in that, Before step S100, a step of pre-treating the base of the steel template is also included; The substrate pretreatment specifically involves removing the adhering substances from the inner surface of the steel template until the metal substrate is exposed, and keeping the inner surface dry and free of standing water.
3. The method for curing concrete applied to the inner surface of a steel mold according to claim 2, characterized in that, In step S100, the film thickness of the isolation coating is controlled to be between 20 and 50 micrometers; preferably, the water-based release and curing agent is uniformly coated onto the inner surface by airless spraying, roller coating or brush coating.
4. The method for curing concrete applied to the inner surface of a steel mold according to claim 3, characterized in that, The polymer film-forming base material of the water-based release and curing agent contains both hydrophobic segments and alkali-sensitive hydrophilic groups. When the isolation coating is in a fully dry state, the hydrophobic segments face the side of the steel template to provide the initial adhesion and release isolation effect to the steel template.
5. A method for curing concrete applied to the inner surface of a steel mold according to claim 4, characterized in that, During the pouring and curing process in step S200: During the pouring and compaction of the concrete, the vibration equipment is kept at a preset distance from the inner surface of the steel formwork to prevent physical damage to the integrity of the isolation coating. Furthermore, the curing stage under the formwork shall last for no less than 3 days to ensure that the hydration reaction of the concrete is fully carried out, so that the adhesion of the isolation coating to the concrete surface reaches the critical threshold that meets the subsequent peeling and transfer conditions.
6. A method for curing concrete applied to the inner surface of a steel mold according to claim 5, characterized in that, In step S200, the activation of the isolation coating by the concrete hydration reaction specifically includes the following microscopic physicochemical changes: During the hydration process of the concrete, heat of hydration is released at the solid-liquid interface where it adheres to the isolation coating, forming a highly alkaline environment. The alkali-sensitive hydrophilic groups in the isolation coating facing the concrete side undergo polar bonding or micro-crosslinking reactions with the hydrated calcium silicate gel precipitated on the concrete surface under the dual stimulation of the highly alkaline environment and the heat of hydration, thereby causing the adhesion of the isolation coating to the concrete surface to continuously increase with the hydration process.
7. A method for curing concrete applied to the inner surface of a steel mold according to claim 6, characterized in that, In step S300, the process of peeling and transferring the isolation coating from the inner surface of the steel template is specifically manifested as the in-situ overall peeling of the phase interface. At the moment the steel formwork is removed, based on the mechanical reversal characteristic that the adhesion of the isolation coating to the concrete surface is greater than its initial adhesion to the steel formwork, the isolation coating completely detaches from the metal substrate of the steel formwork and transforms in situ into the curing film adhering to the concrete surface without damage.
8. A method for curing concrete applied to the inner surface of a steel mold according to claim 7, characterized in that, The curing film transferred and attached to the concrete surface is continuous and semi-transparent; Furthermore, the curing film tightly covers the surface micropores of the concrete to form a closed barrier between the concrete and the outside air, preventing the evaporation of moisture from the inside of the concrete.
9. A method for curing concrete applied to the inner surface of a steel mold according to claim 8, characterized in that, During the continuous water retention curing in step S400: the moisture balance inside the concrete is maintained independently by the extremely low water vapor permeability of the curing film, without the need for and to avoid additional water replenishment to the surface of the concrete; and the cycle of water retention curing using the curing film is not less than 14 days.
10. A method for curing concrete applied to the inner surface of a steel mold according to claim 9, characterized in that, The curing film has environmental self-degradation characteristics; after the water retention curing cycle ends, the curing film will undergo photodegradation or weathering and powdering when exposed to the natural environment, without the need for physical peeling or chemical cleaning, so that subsequent construction operations can be carried out directly on the concrete surface.