Reinforced PVC geomembrane and method for producing the same

By forming an interface treatment layer of silane coupling agent and film-forming agent on the surface of glass fiber fabric, the problems of dimensional stability, tear resistance and interfacial bonding of PVC geomembrane are solved, and the high strength and flexibility of reinforced PVC geomembrane are achieved.

CN123150366APending Publication Date: 2026-11-24SUZHOU CANLON POLYMER NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611633157.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing composite reinforced PVC waterproof materials suffer from problems such as insufficient dimensional stability, limited tear and puncture resistance, insufficient interfacial bonding, and decreased flexibility and elongation.

Method used

A glass fiber reinforcement layer is used. An interface treatment layer is formed on the surface of the glass fiber fabric. The interfacial bonding strength between the glass fiber and the PVC matrix is ​​improved by using a composite treatment of silane coupling agent and film-forming agent. The reinforced PVC geomembrane is then prepared by calendering composite process.

Benefits of technology

It significantly improves the tensile strength, tear strength, puncture resistance and thermal dimensional stability of PVC geomembranes, while maintaining the flexibility and low-temperature performance of geomembranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123150366A_ABST
    Figure CN123150366A_ABST
Patent Text Reader

Abstract

This invention relates to the field of polymer waterproofing materials technology, and discloses a reinforced PVC geomembrane and its preparation method. The reinforced PVC geomembrane includes a first PVC layer, a second PVC layer, and a glass fiber reinforcing layer disposed between the two layers. An interface treatment layer formed by a silane coupling agent and a film-forming agent is attached to the surface of the glass fiber. The preparation method includes: preparing a surface treatment solution containing a silane coupling agent and a film-forming agent; impregnating the glass fiber fabric with the solution and drying it in stages to form a film; and then laminating the treated glass fiber fabric between the two PVC layers. Through the synergistic treatment of the silane coupling agent and the film-forming agent, the interfacial bonding between the glass fiber and the PVC matrix can be enhanced, improving the tensile strength, puncture resistance, and thermal dimensional stability of the geomembrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer waterproofing materials technology, and in particular to an enhanced PVC geomembrane and its preparation method. Background Technology

[0002] Polyvinyl chloride geomembrane, also known as PVC geomembrane, refers to a polymer waterproof membrane made primarily of polyvinyl chloride resin, along with plasticizers, stabilizers, fillers, and other additives, through calendering, extrusion, or other molding processes.

[0003] As the application fields place increasing demands on the mechanical properties and laying reliability of geomembranes, composite reinforced PVC waterproof materials have gradually been developed in the industry.

[0004] Existing composite reinforced PVC waterproof materials still have the following shortcomings: Firstly, the dimensional stability is insufficient. PVC material has large thermal expansion and contraction characteristics. When subjected to long-term solar radiation, high temperature and diurnal temperature difference, the geomembrane is prone to dimensional changes, which can cause shrinkage, wrinkles and local stress concentration during large-area laying construction. Secondly, it has limited tear and puncture resistance. Ordinary PVC geomembranes mainly rely on the PVC matrix itself to bear external loads. When subjected to concentrated stress caused by sharp objects, construction machinery, or unevenness of the base layer, they are prone to tearing or puncture damage. Third, the interfacial bonding between PVC and the reinforcing material is insufficient, resulting in micropores and debonding at the interface between glass fiber and PVC, which reduces the stability of the reinforcing layer during long-term use. Fourth, while increasing strength, it is difficult to maintain the original flexibility and elongation properties of PVC geomembrane, and the mechanical properties retention rate is low after long-term aging. Summary of the Invention

[0005] The main objective of this invention is to propose an enhanced PVC geomembrane and its preparation method, which aims to improve the tensile strength, tear strength, puncture resistance and thermal dimensional stability of the PVC geomembrane, and improve the interfacial bonding strength between glass fiber and PVC matrix, while maintaining the flexibility of the geomembrane while improving strength.

[0006] To achieve the above objectives, the reinforced PVC geomembrane proposed in this invention is characterized by comprising: First PVC layer; The second PVC layer is stacked on top of the first PVC layer; A glass fiber reinforced layer is disposed between the first PVC layer and the second PVC layer; the glass fiber reinforced layer is composed of a glass fiber fabric with an interface treatment layer attached to its surface, the interface treatment layer being formed by curing a surface treatment liquid containing a silane coupling agent and a film-forming agent.

[0007] In one embodiment, the silane coupling agent is a combination of aminosilane and epoxysilane.

[0008] In one embodiment, the aminosilane is γ-aminopropyltriethoxysilane, and the epoxysilane is γ-glycidoxypropyltrimethoxysilane.

[0009] In one embodiment, the film-forming agent is an aqueous polyurethane dispersion.

[0010] In one embodiment, the glass fiber fabric is an E-glass fiber continuous fabric, which can be a plain glass fiber fabric, a twill glass fiber fabric, a glass fiber mesh fabric, or a warp-knitted glass fiber fabric, and the unit area mass of the continuous fiber fabric is 50 g / m². 2 ~300g / m 2 .

[0011] In one embodiment, the amount of the interface treatment layer attached to the glass fiber fabric is 0.5% to 2.0% of the mass of the glass fiber fabric.

[0012] In one embodiment, the reinforced PVC geomembrane further includes a nonwoven fabric layer disposed on the side of the first PVC layer opposite to the glass fiber reinforcement layer, and / or on the side of the second PVC layer opposite to the glass fiber reinforcement layer.

[0013] This invention also proposes a method for preparing a reinforced PVC geomembrane, characterized in that the method for preparing the reinforced PVC geomembrane as described above includes: The silane coupling agent is added to the acidic aqueous phase and stirred to hydrolyze. After hydrolysis, the film-forming agent is added and mixed evenly to obtain the surface treatment solution. The fiberglass fabric is immersed in the surface treatment liquid, and the excess surface treatment liquid is removed by squeezing with extrusion rollers; The impregnated glass fiber fabric is sequentially subjected to low-temperature dehydration and high-temperature film-forming and drying in stages to obtain a glass fiber fabric with an interface treatment layer attached to the surface. The PVC mixture is plasticized and extruded, and then calendered to form the first PVC layer; A glass fiber fabric with an interface treatment layer attached to its surface is continuously introduced into the surface of the first PVC layer, pressed by a composite roller, and a second PVC layer is formed by calendering on the side of the glass fiber fabric away from the first PVC layer. After cooling and shaping, the reinforced PVC geomembrane is obtained.

[0014] In one embodiment, the silane coupling agent is an aminosilane and an epoxysilane, and the film-forming agent is an aqueous polyurethane dispersion; based on the total mass of the surface treatment liquid, the mass fraction of the aminosilane is 0.1% to 1.0%, the mass fraction of the epoxysilane is greater than 0 and not more than 1.0%, the mass fraction of the aqueous polyurethane dispersion is 0.5% to 5.0%, and the balance is water; the pH of the acidic aqueous phase is 3.5 to 4.5.

[0015] In one embodiment, the immersion time of the glass fiber fabric in the surface treatment solution is 10s to 60s; the temperature of the low-temperature dehydration treatment is 80℃ to 100℃ and the time is 1min to 3min; the temperature of the high-temperature film-forming and setting treatment is 120℃ to 140℃ and the time is 1min to 3min; after the segmented drying is completed, the glass fiber fabric is cooled to below 40℃; the amount of the interface treatment layer adhering to the glass fiber fabric is 0.5% to 2.0% of the mass of the glass fiber fabric.

[0016] The technical solution of this invention involves a composite surface treatment of glass fiber fabric with silane coupling agent and film-forming agent, which forms an interface treatment layer containing silane coupling component and film-forming component on the glass fiber surface: the hydrolyzable groups of the silane coupling agent chemically bond with the hydroxyl groups on the glass fiber surface, and its organic functional groups are compatible with or react with the PVC matrix; the film-forming agent forms a flexible organic film layer on the glass fiber surface, filling the defects on the glass fiber surface and improving the interfacial contact. The two work synergistically to significantly improve the interfacial bonding strength between the glass fiber and PVC. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0018] Figure 1 This is a schematic diagram of the structure of an embodiment of the reinforced PVC geomembrane provided by the present invention; Figure 2 This is a flowchart illustrating an embodiment of the preparation method of the reinforced PVC geomembrane provided by the present invention.

[0019] Explanation of icon numbers: 100, First PVC layer; 200, Second PVC layer; 300, Glass fiber reinforced layer.

[0020] The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0022] It should be noted that if the embodiments of the present invention involve directional indicators (such as up, down, left, right, front, back, etc.), the directional indicators are only used to explain the relative positional relationship and movement of the components in a specific posture. If the specific posture changes, the directional indicators will also change accordingly.

[0023] Furthermore, if the embodiments of this invention involve descriptions such as "first" or "second," these descriptions are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the use of "and / or" or "and / or" throughout the text includes three parallel solutions. For example, "A and / or B" includes solution A, solution B, or a solution where both A and B are satisfied simultaneously. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.

[0024] In this invention, PVC geomembrane refers to a polymer waterproof membrane made primarily of polyvinyl chloride resin; glass fiber fabric refers to a cloth or mesh material made from continuous glass fibers through a weaving process; silane coupling agent refers to an organosilicon compound containing both hydrolyzable groups and organic functional groups in its molecule, wherein the hydrolyzable groups can react with the hydroxyl groups on the surface of the glass fiber, and the organic functional groups can undergo compatibility, adsorption, or chemical reaction with organic polymer materials; film-forming agent refers to a polymer material that can form a continuous or semi-continuous organic protective layer on the surface of glass fiber; and waterborne polyurethane dispersion refers to a system in which polyurethane is stably dispersed in water in the form of microparticles, forming a flexible polyurethane membrane after drying.

[0025] Furthermore, unless otherwise specified, the mass parts mentioned in this invention refer to mass parts; and the percentages mentioned refer to mass percentages unless otherwise specified.

[0026] Reference Figure 1 This invention provides an enhanced PVC geomembrane, comprising a first PVC layer 100, a second PVC layer 200, and a glass fiber reinforcement layer 300. The glass fiber reinforcement layer 300 is disposed between the first PVC layer 100 and the second PVC layer 200. The glass fiber reinforcement layer 300 is composed of glass fiber fabric with an interface treatment layer attached to its surface. The interface treatment layer is formed by curing a surface treatment liquid containing a silane coupling agent and a film-forming agent.

[0027] In this embodiment, the first PVC layer 100 and the second PVC layer 200 form the waterproof main body and continuous phase of the geomembrane, and the glass fiber reinforcement layer 300 is located inside the PVC material to improve the material's mechanical properties and dimensional stability. The first PVC layer 100 and the second PVC layer 200 can use the same PVC formulation or different PVC formulations; this embodiment does not impose any restrictions on this.

[0028] Furthermore, the reinforced PVC geomembrane also includes a non-woven fabric layer, which is disposed on the side of the first PVC layer 100 opposite to the glass fiber reinforcement layer 300, and / or the side of the second PVC layer 200 opposite to the glass fiber reinforcement layer 300. The non-woven fabric layer is used to improve the contact performance between the geomembrane and the base layer and its construction adaptability.

[0029] As an example, the composite structure can be: a first PVC layer 100 / a surface-treated glass fiber fabric / a second PVC layer 200 / a non-woven fabric layer, or it can be: a non-woven fabric layer / a first PVC layer 100 / a glass fiber fabric / a second PVC layer 200.

[0030] It should be noted that, in this embodiment, E-glass fiber is preferably used. The glass fiber fabric can be plain glass fiber fabric, twill glass fiber fabric, glass fiber mesh fabric, warp-knitted glass fiber fabric, or other continuous glass fiber fabrics, with continuous glass fiber fabrics being preferred. The unit area mass of the glass fiber reinforcement layer 300 can be adjusted according to the product thickness and mechanical property requirements, with a preferred range of 50 g / m². 2 ~300g / m 2 More preferably 80g / m 2 ~200g / m 2 .

[0031] The above-mentioned unit area mass range is derived from the inventor's comparative study on the composite effect of glass fiber fabrics with different areal densities and 3.0mm thick PVC geomembranes: when the areal density is less than 50g / m²... 2 When the spacing between glass fiber bundles is too large, the reinforcing layer's ability to constrain the thermal deformation of the PVC matrix is ​​insufficient; when the areal density is higher than 300 g / m³... 2 When the glass fiber bundles are too dense, the PVC melt cannot fully wet and penetrate the gaps between the glass fiber bundles, leaving micropores at the interface and reducing the flexibility of the geomembrane.

[0032] It should be noted that the silane coupling agent can be selected from one or more of aminosilanes, epoxysilanes, vinylsilanes, and methacryloxysilanes, preferably a combination of aminosilanes and epoxysilanes, wherein the aminosilane is γ-aminopropyltriethoxysilane and the epoxysilane is γ-glycidoxypropyltrimethoxysilane. It should also be noted that commercially available brands of γ-aminopropyltriethoxysilane include KH-550, and commercially available brands of γ-glycidoxypropyltrimethoxysilane include KH-560. This invention does not limit the source of the silane coupling agent; commercially available products with the same brand or composition can be used.

[0033] Furthermore, the film-forming agent is preferably a polymeric film-forming material with good compatibility with the PVC system. It can be one or more of the following: aqueous polyurethane dispersion, polyurethane emulsion, acrylic emulsion, and PVC-compatible polymer, with aqueous polyurethane dispersion being preferred. The aqueous polyurethane dispersion forms an organic film layer on the glass fiber surface, which can reduce surface defects and improve the interfacial contact between the glass fiber and PVC. Preferably, the aqueous polyurethane dispersion is anionic or nonionic, with a solid content of 30%–40%, small particle size, good compatibility with silane systems, and a certain degree of flexibility after drying.

[0034] In this embodiment, in the interface treatment layer, the silane coupling agent is chemically bonded to the glass fiber surface by condensing its hydrolyzable groups with the hydroxyl groups on the glass fiber surface to form siloxane bonds. The film-forming agent and the organic segments of the silane coupling agent interact to form a flexible organic film layer on the glass fiber surface, thereby forming a composite treatment layer on the glass fiber surface that can form a strong interfacial bond with PVC.

[0035] This invention also provides a glass fiber surface treatment process for preparing glass fiber fabrics with an interface treatment layer attached to their surface. The glass fiber surface treatment solution uses water as the main dispersion medium, and a preferred composition of the solution is shown in Table 1. Table 1. Composition of glass fiber surface treatment solution (by mass fraction)

[0036] It should be noted that the proportions in Table 1 are the experimental development ranges determined through comparative experiments of the examples. The actual formulation can be adjusted within this range according to the glass fiber specifications, PVC formulation, and target performance. The acid regulator is not added at a fixed mass, but rather pH is used as the control index. It should also be noted that the content of the waterborne polyurethane dispersion in Table 1 is based on the dispersion. When the solid content of the waterborne polyurethane dispersion is 30% to 40%, the corresponding solid content is 0.2% to 2.0%, and more preferably 0.5% to 1.2%.

[0037] The glass fiber surface treatment process includes the following steps: Step S10: Prepare the aqueous phase and adjust the pH.

[0038] First, add deionized water to an acid-resistant container equipped with a stirrer. Taking the final preparation of 100 kg of glass fiber surface treatment solution as an example, add 80 kg to 90 kg of deionized water first, start stirring, and control the stirring speed at 200 rpm to 500 rpm. Then, add an acid adjuster to bring the pH of the system into the acidic range. The acid adjuster is preferably an organic acid, including one or more of glacial acetic acid, formic acid, lactic acid, and citric acid, with glacial acetic acid being preferred. Glacial acetic acid not only adjusts the pH of the system but also facilitates the hydrolysis of aminosilanes in the aqueous system.

[0039] It should be noted that, based on 100 kg of treatment solution, the initial addition of glacial acetic acid is preferably 0.05 kg to 0.30 kg, more preferably 0.08 kg to 0.15 kg. In actual production, it is not added at a fixed mass, but rather the final pH value is used as the control indicator. Preferably, the initial aqueous phase pH is adjusted to 3.5 to 4.5, more preferably 4.0 to 4.5. The above pH range is derived from the hydrolysis reaction characteristics of aminosilanes: the hydrolysis rate of aminosilanes in a weakly acidic aqueous phase is moderate, and the generated silanols have good stability, which can inhibit the self-condensation reaction of silanes and ensure the stability of the treatment solution.

[0040] Step S20: Hydrolysis of aminosilane.

[0041] After the pH of the aqueous phase reaches 4.0–4.5, aminosilane is slowly added. γ-aminopropyltriethoxysilane is preferably used as the main silane coupling agent, accounting for 0.50% of the total mass of the treated solution. The γ-aminopropyltriethoxysilane is slowly added to the acidified aqueous phase, preferably over a period of 5–15 minutes, with stirring maintained during the addition process. After the addition is complete, stirring continues for 20–30 minutes, preferably 25 minutes, while maintaining the temperature at 20–30°C.

[0042] It should be noted that the hydrolysis temperature of aminosilane is controlled at 20℃~30℃ and the hydrolysis time is controlled at 25min. This is due to the hydrolysis reaction rate characteristics of aminosilane in a weakly acidic aqueous phase. It is not advisable to hydrolyze for a long time under high temperature conditions in order to reduce the risk of silane self-condensation and ensure the activity of the hydrolysis product silanol.

[0043] Step S30: Add epoxy silane.

[0044] After the aminosilane hydrolysis is completed, an epoxy silane is further added, preferably γ-glycidoxypropyltrimethoxysilane as the second silane coupling agent, used in conjunction with the aminosilane to improve the interfacial bonding properties of the glass fiber surface. The amount of γ-glycidoxypropyltrimethoxysilane added is 0.10% to 0.80%, preferably 0.20% to 0.50%.

[0045] Step S40: Add water-based polyurethane film-forming agent.

[0046] After the silane system has completed hydrolysis, an aqueous polyurethane dispersion is added. The role of the aqueous polyurethane dispersion is not simply to provide coupling, but to form a flexible organic film layer on the glass fiber surface, thereby improving the interfacial contact and load transfer between the glass fiber and PVC. Based on the final processed liquid, the solid content of the aqueous polyurethane dispersion is preferably 0.2% to 2.0%, more preferably 0.5% to 1.2%.

[0047] The above-mentioned solid content range is derived from the preferred range determined by the inventors after conducting comparative experiments on the interfacial peel strength and tensile strength of each group of treatment liquids in the examples: when the solid content is less than 0.2%, the film formation on the glass fiber surface is incomplete and the improvement of interfacial bonding is not obvious; when the solid content is greater than 2.0%, the treatment layer is too thick, and compatibility problems arise between the treatment layer and PVC, and the mechanical interlocking between glass fiber and PVC is weakened.

[0048] Step S50: Add wetting agent and defoamer.

[0049] To improve the wetting ability of the treatment solution on glass fiber fabrics, a small amount of nonionic wetting agent can be added. The preferred addition amount is 0.05 kg to 0.50 kg per 100 kg of treatment solution, more preferably 0.10 kg to 0.30 kg per 100 kg of treatment solution. Nonionic wetting agents are preferred to reduce their impact on silane hydrolysis and the stability of the waterborne polyurethane dispersion. The defoamer addition amount is 0.01 kg to 0.10 kg per 100 kg of treatment solution, preferably 0.02 kg to 0.05 kg per 100 kg of treatment solution, and an aqueous defoamer compatible with the waterborne polyurethane system is used.

[0050] Step S60, final pH adjustment.

[0051] After all components have been added, the pH of the treated solution is checked again. The final treated solution is preferably controlled at pH 4.5–5.5, more preferably pH 4.8–5.2. If the pH is higher than the target range, it can be adjusted by diluting glacial acetic acid solution. Prepare a 10% glacial acetic acid aqueous solution in advance, and then slowly add it dropwise. Stir for 2 to 5 minutes after each small amount of addition and check the pH again to gradually adjust it to the target range. If the pH is lower than the target range, it can be finely adjusted by dilute ammonia or a low-concentration ammonium hydroxide (5%–10%) solution.

[0052] The aforementioned final pH range is derived from the balance between the storage stability requirements of the surface treatment solution and the activity of silane hydrolysis products: when the pH is higher than 5.5, the silane hydrolysis products tend to self-condense, shortening the storage period of the treatment solution; when the pH is lower than 4.5, the glass fiber is at greater risk of corrosion in the acidic treatment solution.

[0053] Step S70: Glass fiber impregnation.

[0054] After the treatment solution is prepared and stabilized, the glass fiber fabric is continuously passed through the treatment tank. The glass fiber should be completely immersed in the treatment solution. The immersion time is preferably 10s to 60s, more preferably 20s to 40s. Then, excess treatment solution is removed by a pair of extrusion rollers. The amount of liquid carried by the glass fiber is controlled by adjusting the pressure of the extrusion rollers, the roller gap, and the production line speed.

[0055] The above-mentioned impregnation time range is derived from the matching relationship between the impregnation rate of the glass fiber fabric and the operating speed of the production line: when the impregnation time is less than 10s, the treatment liquid cannot fully impregnate the interior of the glass fiber bundle; when the impregnation time is greater than 60s, the production efficiency decreases and there is too much liquid adhering to the surface of the glass fiber, which increases the subsequent drying load.

[0056] Step S80: Control the final amount of glass fiber processed.

[0057] Further control the amount of final organic treatment material adhering to the glass fiber surface, preferably to 0.5% to 2.0%, more preferably 0.8% to 1.2%.

[0058] The above-mentioned adhesion amount range is derived from the comparative experimental results of the embodiments: when the treatment amount is too low, the improvement in the interface bonding between glass fiber and PVC is not significant; when the treatment amount is too high, an excessively thick organic film forms on the surface of the glass fiber, causing compatibility problems between the treated layer and PVC, weakening the mechanical interlocking between the glass fiber and PVC, and increasing material costs. For example, if the weight of glass fiber before treatment is 1000g and after treatment and drying is 1010g, then the increase in organic treatment material is 10g, corresponding to a treatment amount of 1.0%.

[0059] Step S90: Segmented drying.

[0060] After passing through the extrusion rollers, the glass fiber fabric enters an oven for segmented drying. The first stage is low-temperature dehydration, with a temperature of 80℃~100℃, preferably 90℃, for 1min~3min, the specific time depending on the production line speed and oven length. This mainly removes free water, reduces surface defects caused by rapid boiling, and prevents internal moisture from being trapped due to rapid film formation of the waterborne polyurethane dispersion. The second stage is film formation and setting, with a temperature of 120℃~140℃, preferably 125℃~135℃, for 1min~3min. This removes residual moisture, promotes film formation of the waterborne polyurethane dispersion, and forms a stable glass fiber surface treatment layer. After processing, the glass fiber is cooled to below 40℃.

[0061] It should be noted that the upper limit of the first stage low-temperature dehydration temperature of 100℃ is derived from the boiling and evaporation characteristics of water and the thermal stability requirements of the treatment layer components, in order to avoid water boiling and damaging the film layer; the second stage film-forming and shaping temperature range is derived from the film-forming characteristics of the waterborne polyurethane dispersion. A continuous film layer can only be formed when the temperature reaches above its minimum film-forming temperature, and it does not exceed 140℃ to ensure that the interface treatment layer does not undergo thermal degradation.

[0062] For ease of understanding, the complete process flow is shown here.

[0063] The entire glass fiber treatment process is as follows: deionized water → add glacial acetic acid → adjust pH to 4.0-4.5 → add γ-aminopropyltriethoxysilane → stir at 20℃-30℃ for 20-30 minutes → add γ-glycidyl etheroxypropyltrimethoxysilane → continue stirring → add pre-diluted waterborne polyurethane dispersion → add wetting agent and defoamer → finally adjust pH to 4.5-5.5 → glass fiber impregnation → control the liquid flow rate with extrusion rollers → dehydration at 80℃-100℃ → film formation at 120℃-140℃ → cooling → obtain surface-treated glass fiber fabric → proceed to the PVC composite process.

[0064] It should be noted that the PVC substrate can use a conventional PVC geomembrane formulation. As an example, the PVC mixture, by weight, includes: 90-110 parts PVC resin with a degree of polymerization of 1350-1500; 60-70 parts plasticizer, which is diisononyl phthalate; 0.3-0.5 parts calcium-zinc heat stabilizer; 20-30 parts heavy calcium carbonate filler; 0.3-0.5 parts polyethylene wax lubricant; 0.3-0.5 parts antioxidant 1010, used in amounts of rutile; and 15-20 parts titanium dioxide.

[0065] It should be noted that the above proportions are derived from the comprehensive requirements of PVC geomembrane for mechanical properties, weather resistance and processing performance, as well as the commercially available specifications of the raw materials used in the examples: PVC resin with a degree of polymerization of 1350 to 1500 can balance processing fluidity and mechanical strength; plasticizer dosage of 60 to 70 parts can enable the geomembrane to obtain the required flexibility; calcium-zinc heat stabilizer is used to inhibit the thermal decomposition of PVC at extrusion and calendering processing temperatures.

[0066] Please continue to refer to Figure 1 And refer to Figure 2 The present invention also provides a method for preparing an enhanced PVC geomembrane, which employs a calendering composite process.

[0067] It should be noted that the preparation method of this embodiment is implemented on a calendering composite production line consisting of two twin-screw extruders, a calendering roll group, a composite roll, a cooling roll group and a winding device. The two twin-screw extruders are used for plasticizing extrusion of the first PVC layer 100 and the second PVC layer 200, respectively.

[0068] The preparation method includes the following steps: Step S201, PVC mixing.

[0069] According to the established PVC formula, PVC resin, plasticizer, stabilizer, filler, pigment and other additives are mixed at high speed.

[0070] Specific steps: Add the powder at 600 rpm, add the plasticizer when the powder temperature reaches 65℃, then increase the speed to 1000 rpm to 1200 rpm. When the mixing temperature reaches 110℃, reduce the speed to 300 rpm and turn on the cooling to cool the mixture down. Release the mixture when the mixing temperature is below 40℃.

[0071] It should be noted that the basis for adding plasticizer when the powder temperature reaches 65℃ is the absorption characteristics of PVC resin powder for plasticizer. Within this temperature range, the plasticizer can be fully absorbed by PVC resin powder without causing agglomeration.

[0072] Step S202: Plasticize and extrude.

[0073] The mixed PVC powder is added to a twin-screw extruder. The screw temperature is set to 175℃~185℃, the die temperature to 200℃~210℃, and the screw speed to 70rpm~100rpm. The PVC powder is plasticized in the extruder screw and extruded through the die. Two extruders are used simultaneously to form a first PVC layer 100 and a second PVC layer 200, respectively, achieving lamination with fiberglass fabric.

[0074] It should be noted that the above extrusion temperature range is derived from the plasticizing processing window of PVC resin and the inhibitory effect of calcium-zinc heat stabilizer on the thermal decomposition of PVC. PVC can be fully plasticized at a screw temperature of 175℃~185℃, while calcium-zinc heat stabilizer is used to prevent thermal decomposition.

[0075] Step S203: Form the first PVC layer 100.

[0076] The extruded material is calendered using a calendering device to form the first PVC layer 100.

[0077] Step S204: Laying the glass fiber reinforcement layer 300. The surface-treated and dried glass fiber fabric is continuously introduced onto the surface of the first PVC layer 100.

[0078] Step S205, compounding.

[0079] The glass fiber fabric is fully bonded to the first PVC layer 100 by calendering rollers or composite rollers, allowing the PVC melt to penetrate into the gaps between the glass fiber bundles.

[0080] Step S206, forming the second PVC layer 200.

[0081] A second PVC layer 200 is formed by calendering on the side of the glass fiber fabric away from the first PVC layer 100, so that the glass fiber reinforcement layer 300 is embedded between the first PVC layer 100 and the second PVC layer 200.

[0082] Step S207: Composite nonwoven fabric.

[0083] According to the product structure requirements, a non-woven fabric layer is laminated on the surface of the PVC layer.

[0084] Step S208: Cooling and shaping.

[0085] The composite material is cooled and shaped using cooling rollers.

[0086] Step S209: Rewind.

[0087] The reinforced PVC geomembrane, after being cooled and shaped, is rolled up to obtain the finished reinforced PVC geomembrane.

[0088] Furthermore, to better understand the present invention, the reinforced PVC geomembrane and its preparation method provided by the present invention will be specifically described below with reference to embodiments. All embodiments of the present invention use commercially available raw materials.

[0089] Examples 1-6 PVC geomembranes containing a glass fiber reinforcement layer 300 were prepared according to the above preparation method. The thickness of the PVC geomembrane was 3.0 mm. The PVC mixture formulation and preparation process parameters were the same in all embodiments; the only change was the surface treatment method of the glass fibers. The glass fiber treatment conditions for each embodiment are as follows: Example 1: Group G0, using untreated original glass fiber fabric as a blank control group.

[0090] Example 2: Group G1, the glass fiber fabric was surface treated with aminosilane, and the concentration of γ-aminopropyltriethoxysilane in the treatment solution was controlled at 0.5%.

[0091] Example 3: Group G2, which was treated with a composite of γ-aminopropyltriethoxysilane and aqueous polyurethane dispersion, to verify whether the silane coupling agent and the organic film-forming agent produce a synergistic effect.

[0092] Example 4: Group G3, which was treated with γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane and aqueous polyurethane dispersion. This group was the key research group.

[0093] Example 5: Group G4, treated with γ-aminopropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane, without the addition of aqueous polyurethane dispersion. This group was used to determine the contribution of aqueous polyurethane dispersion to the interface enhancement effect.

[0094] Example 6: Group G5, using γ-aminopropyltriethoxysilane and aqueous polyurethane dispersion system, but increasing the amount of treatment agent used, so that the amount of interface treatment layer adhesion exceeds 2.0%. This group was used to study the relationship between the amount of glass fiber surface treatment and PVC composite performance.

[0095] The reinforced PVC geomembranes prepared in Examples 1-6 were subjected to performance tests, including tensile strength, elongation at break, tear strength, puncture resistance, thermal dimensional change, fiberglass-PVC interfacial peel strength, low-temperature performance, and weld peel strength. All tests were conducted on products from the same batch, with five samples tested for each test and the arithmetic mean calculated. The testing environment followed the standard environmental requirements for conditioning and testing of plastic products.

[0096] Among them, the heat treatment dimensional change rate is the key technical effect of this invention: glass fiber has a low coefficient of thermal expansion, and through glass fiber reinforcement, the dimensional change of PVC matrix in high temperature environment can be limited; when the surface-treated glass fiber and PVC have a higher interfacial bonding strength, the glass fiber can more effectively limit the thermal deformation of PVC matrix, that is, to form a progressive relationship of "glass fiber surface treatment → interfacial bonding enhancement → glass fiber constraint ability enhancement → thermal dimensional change reduction".

[0097] The test results are shown in Table 2: Table 2 Performance test results of reinforced PVC geomembranes in Examples 1-6

[0098] As can be seen from Table 2: Comparing groups G0 and G1, after treatment with aminosilane alone, the tensile strength increased from 29 kN / m to 32 kN / m, the interfacial peel strength increased from 3.8 N / mm to 4.3 N / mm, and the thermal dimensional change decreased from 1.5% to 1.3%, indicating that the silane coupling agent can improve the interfacial bonding between glass fiber and PVC matrix. Comparing groups G1 and G2, after introducing an aqueous polyurethane dispersion on the basis of aminosilane, the tensile strength further increased to 34 kN / m, the interfacial peel strength increased to 4.7 N / mm, and the thermal dimensional change decreased to 0.8%, indicating that the silane coupling agent and the organic film-forming agent have a synergistic effect.

[0099] Comparing groups G3 and G4, based on the aminosilane and epoxysilane bissilane system, group G3, after further introducing an aqueous polyurethane dispersion, showed an increase in tensile strength from 36 kN / m to 38 kN / m, elongation at break from 276% to 284%, tear strength from 66 N / mm to 69 N / mm, puncture resistance from 552 N to 572 N, a decrease in thermal dimensional change from 0.6% to 0.3%, and an increase in interfacial peel strength from 5.2 N / mm to 5.9 N / mm. This indicates that the aqueous polyurethane dispersion film layer makes a significant contribution to improving interfacial bonding and maintaining flexibility.

[0100] Comparing groups G2 and G5, in group G5, after increasing the amount of treatment agent used to exceed 2.0% of the interface treatment layer, the tensile strength decreased from 34 kN / m to 32 kN / m, the elongation at break decreased from 264% to 261%, the thermal dimensional change increased from 0.8% to 0.9%, and the interfacial peel strength decreased from 4.7 N / mm to 4.5 N / mm. This indicates that when the amount of interface treatment layer adhesion is too high, the treatment layer becomes too thick, causing compatibility problems between the treatment layer and PVC. The mechanical bonding between glass fiber and PVC weakens, and the performance actually decreases. Therefore, the reasonable range for the amount of interface treatment layer adhesion is determined to be 0.5% to 2.0%.

[0101] Table 2 also shows that the low-temperature performance of groups G0 to G5 is -35℃ and the weld peel strength is maintained at 7.2N / mm to 7.5N / mm. This indicates that the present invention improves the mechanical properties and thermal dimensional stability of the geomembrane while maintaining the original low-temperature flexibility and weldability of the geomembrane.

[0102] In this way, by using silane coupling agents and film-forming agents to perform composite surface treatment on glass fiber fabric, an interface treatment layer containing silane coupling components and film-forming components is formed on the surface of glass fiber. Then, the glass fiber fabric is composited between two PVC layers, which significantly improves the interfacial bonding strength between glass fiber and PVC matrix. This simultaneously improves the tensile strength, tear strength, puncture resistance and thermal dimensional stability of PVC geomembrane, while maintaining the flexibility of geomembrane.

[0103] The above description is merely an exemplary embodiment of the present invention and does not limit the scope of protection of the present invention. Any equivalent structural transformations made based on the technical concept of the present invention and the contents of the specification and drawings of the present invention, or direct / indirect applications in other related technical fields, are included within the scope of protection of the present invention.

Claims

1. A reinforced PVC geomembrane, characterized in that, include: First PVC layer; The second PVC layer is stacked on top of the first PVC layer; A glass fiber reinforced layer is disposed between the first PVC layer and the second PVC layer; the glass fiber reinforced layer is composed of a glass fiber fabric with an interface treatment layer attached to its surface, the interface treatment layer being formed by curing a surface treatment liquid containing a silane coupling agent and a film-forming agent.

2. The reinforced PVC geomembrane as described in claim 1, characterized in that, The silane coupling agent is a combination of aminosilane and epoxysilane.

3. The reinforced PVC geomembrane as described in claim 2, characterized in that, The aminosilane is γ-aminopropyltriethoxysilane, and the epoxysilane is γ-glycidoxypropyltrimethoxysilane.

4. The reinforced PVC geomembrane as described in claim 1, characterized in that, The film-forming agent is an aqueous polyurethane dispersion.

5. The reinforced PVC geomembrane according to any one of claims 1 to 4, characterized in that, The glass fiber fabric is an E-type continuous glass fiber fabric, which can be a plain glass fiber fabric, a twill glass fiber fabric, a mesh glass fiber fabric, or a warp-knitted glass fiber fabric. The unit area mass of the continuous fiber fabric is 50 g / m². 2 ~300g / m 2 .

6. The reinforced PVC geomembrane according to any one of claims 1 to 4, characterized in that, The amount of the interface treatment layer attached to the glass fiber fabric is 0.5% to 2.0% of the mass of the glass fiber fabric.

7. The reinforced PVC geomembrane according to any one of claims 1 to 4, characterized in that, The reinforced PVC geomembrane further includes a non-woven fabric layer, which is disposed on the side of the first PVC layer away from the glass fiber reinforcement layer, and / or on the side of the second PVC layer away from the glass fiber reinforcement layer.

8. A method for preparing an enhanced PVC geomembrane, characterized in that, A method for preparing a reinforced PVC geomembrane as described in any one of claims 1 to 7, the method comprising: The silane coupling agent is added to the acidic aqueous phase and stirred to hydrolyze. After hydrolysis, the film-forming agent is added and mixed evenly to obtain the surface treatment solution. The fiberglass fabric is immersed in the surface treatment liquid, and the excess surface treatment liquid is removed by squeezing with extrusion rollers; The impregnated glass fiber fabric is sequentially subjected to low-temperature dehydration and high-temperature film-forming and drying in stages to obtain a glass fiber fabric with an interface treatment layer attached to the surface. The PVC mixture is plasticized and extruded, and then calendered to form the first PVC layer; A glass fiber fabric with an interface treatment layer attached to its surface is continuously introduced into the surface of the first PVC layer, pressed by a composite roller, and a second PVC layer is formed by calendering on the side of the glass fiber fabric away from the first PVC layer. After cooling and shaping, the reinforced PVC geomembrane is obtained.

9. The method for preparing the reinforced PVC geomembrane as described in claim 8, characterized in that, The silane coupling agent is an aminosilane and an epoxysilane, and the film-forming agent is an aqueous polyurethane dispersion. Based on the total mass of the surface treatment liquid, the mass fraction of the aminosilane is 0.1% to 1.0%, the mass fraction of the epoxysilane is greater than 0 and not more than 1.0%, the mass fraction of the aqueous polyurethane dispersion is 0.5% to 5.0%, and the balance is water. The pH of the acidic aqueous phase is 3.5 to 4.

5.

10. The method for preparing the reinforced PVC geomembrane as described in claim 8, characterized in that, The glass fiber fabric is immersed in the surface treatment solution for 10s to 60s; the low-temperature dehydration treatment is performed at 80℃ to 100℃ for 1min to 3min; the high-temperature film-forming and setting treatment is performed at 120℃ to 140℃ for 1min to 3min; after segmented drying, the glass fiber fabric is cooled to below 40℃; the amount of the interface treatment layer adhering to the glass fiber fabric is 0.5% to 2.0% of the mass of the glass fiber fabric.