A nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries and its preparation method.
By constructing a carbon framework with porous structure and defect sites through nitrogen-sulfur co-doped Si/Fe₃O₄/C composite anode material, the problems of insufficient specific capacity, large volume change and limited electron transport capability of existing lithium-ion battery anode materials are solved, and the electrochemical performance of high energy density and long life is improved.
Patent Information
- Application Number
- CN202611666069.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-27
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium-ion battery anode materials suffer from insufficient specific capacity of graphite, large volume changes of silicon-based materials during charge and discharge, limited electron transport capacity of Fe₃O₄, insufficient electronic structure regulation of MOF-derived carbon materials, limited lithium-ion adsorption capacity, and slow interfacial reaction kinetics, all of which affect electrochemical performance.
A nitrogen-sulfur co-doped Si/Fe₃O₄/C composite anode material is adopted. A porous structure and defect sites of N/S co-doped carbon framework are constructed by using silicon-based modifying liquid, nitrogen source modifier and sulfur source modifier. This provides continuous electron transport channels and volume buffer space, regulates local electronic structure and interface properties, and enhances Li⁺ adsorption and migration capabilities.
It improves the specific capacity, rate performance, and cycle stability of lithium-ion battery anode materials, reduces charge transport impedance and ion diffusion resistance, exhibits high reversible specific capacity and capacity retention, and is suitable for high energy density and long life lithium-ion batteries.
Smart Images

Figure CN123151401A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of anode material technology, specifically to a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries and its preparation method. Background Technology
[0002] With the rapid development of new energy technologies, lithium-ion batteries, due to their advantages such as high energy density, long cycle life, and high operating voltage, are widely used in portable electronic devices, electric vehicles, and large-scale energy storage systems. As a crucial component of lithium-ion batteries, the specific capacity, electron transport capability, ion diffusion kinetics, and structural stability of the anode material directly affect the overall electrochemical performance of the battery.
[0003] Currently, graphite is the primary anode material for commercial lithium-ion batteries, but its theoretical specific capacity is approximately 372 mAh·g. -1 The current technology is insufficient to meet the development requirements of high-energy-density lithium-ion batteries. Therefore, developing novel anode materials with high theoretical specific capacity and good cycle stability has become an important research direction. Silicon has a high theoretical specific capacity and a low lithium intercalation potential, making it a promising next-generation lithium-ion battery anode material. However, silicon undergoes significant volume changes during charge and discharge, which can easily lead to electrode structure damage, active material pulverization, and decreased interface stability. Furthermore, its intrinsic electronic conductivity is low, limiting its practical applications.
[0004] Transition metal oxides possess high theoretical capacities and can participate in lithium-ion storage through conversion reactions. Among them, Fe3O4 exhibits high theoretical specific capacity and low cost, making it a promising anode material for lithium-ion batteries. However, Fe3O4 is also prone to volume changes and particle agglomeration during cycling, and its limited electron transport capacity leads to significant electrochemical polarization and capacity decay. Therefore, combining silicon with Fe3O4 and introducing carbon materials with good conductivity and structural buffering properties holds promise for achieving synergistic effects between different active components and improving the electrochemical performance of composite anode materials.
[0005] Metal-organic frameworks (MOFs) possess characteristics such as tunable composition, ordered structure, abundant porosity, and uniform distribution of metal elements. After high-temperature heat treatment, they can form porous metal / carbon composite materials, making them ideal precursors for preparing transition metal oxide / carbon composite anode materials. Among them, MIL-101(Fe) contains abundant iron and organic ligands. After high-temperature carbonization, it can form a carbon framework and generate Fe3O4 nanoparticles in situ, thereby improving the dispersion of active components and providing structural buffer space to a certain extent.
[0006] However, simply using MOF-derived carbon materials still suffers from problems such as insufficient control over the electronic structure of carbon materials, limited lithium-ion adsorption capacity, and slow interfacial reaction kinetics. Furthermore, even after introducing nano-silicon into the MOF-derived Fe3O4 / carbon system, the volume change of silicon during cycling can still affect the composite structure. Therefore, further controlling the defect structure and local electronic environment of the carbon framework to improve lithium-ion adsorption and transport capabilities, and enhancing the synergistic effect between silicon, Fe3O4, and the carbon framework, is key to improving the electrochemical performance of this type of composite anode material.
[0007] Non-metallic elements such as nitrogen and sulfur possess different atomic structures and electronegativity. Introducing them into carbon materials can modulate the local electronic structure of the carbon materials, increase defects and active sites, and improve the interfacial interaction between the material and the electrolyte. Through nitrogen and sulfur co-doping, it is expected to further optimize the structure and surface properties of MOF-derived carbon frameworks, promote lithium-ion adsorption, interfacial charge transport and diffusion, thereby improving the rate performance and cycle stability of silicon-based composite anode materials.
[0008] Therefore, developing a composite anode material with MIL-101(Fe) as a precursor, combined with nano-silicon and nitrogen-sulfur co-doped carbon framework, and its preparation method, is of great significance for improving the specific capacity, rate performance and cycle stability of lithium-ion battery anode materials. Summary of the Invention
[0009] To address the shortcomings of existing technologies, the present invention aims to provide a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries and its preparation method.
[0010] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries includes the following preparation steps: S1. Dissolve 2.6-2.8 parts by weight of ferric chloride hexahydrate in 28-32 parts of N,N-dimethylformamide and stir thoroughly until completely dissolved to obtain an iron salt solution; S2. Slowly add the iron salt solution obtained in S1 to 28-32 parts of silicon-based modified solution, then add 0.4-0.6 parts of nitrogen source modifier and 0.4-0.6 parts of sulfur source modifier, and mix by ultrasonication to fully disperse the components to obtain the reaction precursor solution; S3. The reaction precursor solution obtained in step S2 is transferred to a polytetrafluoroethylene-lined reactor for solvothermal reaction. After the reaction is completed, it is naturally cooled to room temperature, centrifuged, washed and dried to obtain the Si / MIL-101(Fe) composite precursor. S4. The Si / MIL-101(Fe) composite precursor obtained in S3 is thoroughly ground and subjected to high-temperature carbonization under argon atmosphere protection (to derive MIL-101(Fe) into a porous carbon framework and generate Fe3O4 nanoparticles in situ, while achieving co-doping of nitrogen and sulfur elements in the carbon framework), finally obtaining nitrogen and sulfur co-doped Si / Fe3O4 / C composite anode material (Si / Fe3O4 / N, SC composite anode material). The preparation of the silicon-based modified liquid includes the following steps: S11. Dissolve 0.7-0.9 parts by weight of terephthalic acid in 28-32 parts of N,N-dimethylformamide, and stir at 300-500 r / min for 25-30 min at room temperature to obtain a preliminary mixture; S12. Add 0.02-0.03 parts of cetyltrimethylammonium bromide, 0.01-0.02 parts of PVP-K30, and 0.01-0.02 parts of PEG-400 to the preliminary mixture obtained in step S11, and continue stirring for 10-15 minutes to obtain the secondary mixture; S13. Add 0.09-0.11 parts of nano-silicon and 0.007-0.009 parts of KH-570 to the secondary mixture obtained in step S12, and disperse it ultrasonically in an ultrasonic cleaner for 28-32 minutes to obtain a silicon-based modified liquid.
[0011] Preferably, the preparation of the nitrogen source modifier includes the following steps: S21. By weight, add 0.03-0.04 parts of urea and 0.002-0.004 parts of dicyandiamide to 0.4-0.6 parts of N,N-dimethylformamide, and stir at 200-400 r / min for 8-10 min. S22. Add 0.001-0.003 parts of glycine and 0.001-0.003 parts of hexamethylenetetramine to the mixture obtained in step S21, and disperse by ultrasonication for 5-8 minutes to finally obtain the nitrogen source modifier.
[0012] Preferably, the preparation of the sulfur source modifier includes the following steps: S31. By weight, mix 0.01-0.02 parts of thiourea and 0.4-0.6 parts of N,N-dimethylformamide and stir at 200-400 r / min for 8-10 min; S32. Add 0.001-0.003 parts of L-cysteine and 0.001-0.002 parts of thioacetamide to the mixture obtained in step S31, and disperse it ultrasonically at a frequency of 40 kHz for 5-8 min to finally obtain the sulfur source modifier.
[0013] Preferably, the reaction temperature of the solvothermal reaction is 105-115℃, and the reaction time is 18-22h.
[0014] Preferably, the washing in step S3 is performed by alternating between N,N-dimethylformamide and deionized water.
[0015] Preferably, the drying in step S3 is vacuum drying at 58-62°C for 11-13 hours.
[0016] Preferably, in step S4, the heating rate of the high-temperature carbonization treatment is 4-6℃ / min, the carbonization temperature is 590-610℃, and the holding time is 2-4h.
[0017] Preferably, the frequency of ultrasonic dispersion in step S22 is 40 kHz.
[0018] A nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries is prepared by the above-described preparation method.
[0019] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention utilizes the synergistic effect of a silicon-based modifying liquid, a nitrogen source modifier, and a sulfur source modifier to construct an N / S co-doped carbon framework with a porous structure and defect sites. This provides continuous electron transport channels and volume buffer space for silicon and Fe3O4. Simultaneously, the invention leverages the heteroatoms of N and S to modulate the local electronic structure and interfacial properties of the carbon framework, enhancing the performance of Li. + The adsorption and migration capabilities reduce charge transport impedance and ion diffusion resistance, thereby improving the reaction kinetics and cycle stability of silicon-based anode materials. The synergistic effect of these three factors gives the resulting composite material good structural stability and electrochemical performance, exhibiting high reversible specific capacity and capacity retention during high-rate and long-cycle charge-discharge processes.
[0020] 2. The preparation process of this invention is simple, the raw materials are readily available, and the structure can be controlled. It has good repeatability and application potential, and can be used to prepare high-energy-density, long-life lithium-ion battery anode materials. Attached Figure Description
[0021] Figure 1 This is a process flow diagram of the preparation process of the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to the present invention; Figure 2 SEM images of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of the present invention, where a is Comparative Example 3, b is Comparative Example 1, c is Comparative Example 2, and d is Example 1. Figure 3The images shown are TEM images of the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries obtained in Example 1 of this invention at different magnifications, where a is the TEM image at 500 nm and b is the TEM image at 10 nm. Figure 4 The XRD patterns of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of the present invention are shown, with the right side being a partial magnified view. Figure 5 Raman plots of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention; Figure 6 The graphs show the discharge specific capacity of the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of the present invention as a function of the number of cycles under the same test conditions. Figure 7 The graphs show the changes in the long-cycle discharge specific capacity of the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of the present invention under the same test conditions. Figure 8 The nitrogen adsorption-desorption isotherms of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention are shown. Figure 9 The diagram shows the pore size distribution curves of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention. Detailed Implementation
[0022] The present invention will now be clearly and completely described in conjunction with embodiments thereof. Obviously, the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0023] Please see Figures 1-9 The present invention provides a technical solution: Example 1 A method for preparing nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries: Before preparing the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries, the following steps are taken: Preparation of silicon-based modifying solution, nitrogen source modifier, and sulfur source modifier are performed: The preparation of the silicon-based modified liquid includes the following steps: S11. Dissolve 0.7g of terephthalic acid in 28g of N,N-dimethylformamide and stir at 300r / min for 25min at room temperature to obtain a preliminary mixture; S12. Add 0.02g cetyltrimethylammonium bromide, 0.01g PVP-K30, and 0.01g PEG-400 to the preliminary mixture obtained in step S11, and continue stirring for 10 minutes to obtain the secondary mixture; S13. Add 0.09g of nano-silicon and 0.007g of KH-570 to the secondary mixture obtained in step S12, and disperse it in an ultrasonic cleaner for 28 minutes to obtain a silicon-based modified liquid.
[0024] The preparation of nitrogen source modifiers includes the following steps: S21. Add 0.03g urea and 0.002g dicyandiamide to 0.4g N,N-dimethylformamide and stir at 200r / min for 8min; S22. Add 0.001g glycine and 0.001g hexamethylenetetramine to the mixture obtained in step S21, and disperse it by ultrasonication at a frequency of 40kHz for 5min to finally obtain the nitrogen source modifier.
[0025] The preparation of the sulfur source modifier includes the following steps: S31. Mix 0.01g thiourea and 0.4g N,N-dimethylformamide and stir at 200r / min for 8min; S32. Add 0.001g L-cysteine and 0.001g thioacetamide to the mixture obtained in step S31, and disperse it ultrasonically at a frequency of 40kHz for 5min to finally obtain the sulfur source modifier.
[0026] The preparation of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries includes the following steps: S1. Dissolve 2.6g of ferric chloride hexahydrate in 28g of N,N-dimethylformamide and stir thoroughly until completely dissolved to obtain an iron salt solution; S2. Slowly add the iron salt solution obtained in S1 to 28g of silicon-based modified solution, then add 0.4g of nitrogen source modifier and 0.4g of sulfur source modifier, and mix by ultrasonication to fully disperse the components to obtain the reaction precursor solution; S3. The reaction precursor solution obtained in step S2 is transferred to a polytetrafluoroethylene-lined reactor for solvothermal reaction (reaction temperature is 105℃, reaction time is 18h). After the reaction is completed, it is naturally cooled to room temperature, centrifuged, washed (using N,N-dimethylformamide and deionized water alternately for washing), and dried (vacuum drying at 58℃ for 11h) to obtain the Si / MIL-101(Fe) composite precursor. S4. The Si / MIL-101(Fe) composite precursor obtained in S3 was thoroughly ground and subjected to high-temperature carbonization treatment under argon atmosphere protection (heating rate of 4℃ / min, carbonization temperature of 590℃, and holding time of 2h) to finally obtain nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material, which was further named Si / Fe3O4@N,SC.
[0027] Example 2 A method for preparing nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries: Before preparing the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries, the following steps are taken: Preparation of silicon-based modifying solution, nitrogen source modifier, and sulfur source modifier are performed: The preparation of the silicon-based modified liquid includes the following steps: S11. Dissolve 0.9g of terephthalic acid in 32g of N,N-dimethylformamide and stir at 500r / min for 30min at room temperature to obtain a preliminary mixture; S12. Add 0.03g cetyltrimethylammonium bromide, 0.02g PVP-K30, and 0.02g PEG-400 to the preliminary mixture obtained in step S11, and continue stirring for 15 minutes to obtain the secondary mixture; S13. Add 0.11g of nano-silicon and 0.009g of KH-570 to the secondary mixture obtained in step S12, and disperse it in an ultrasonic cleaner for 32 minutes to obtain a silicon-based modified liquid.
[0028] The preparation of nitrogen source modifiers includes the following steps: S21. Add 0.04g urea and 0.004g dicyandiamide to 0.6g N,N-dimethylformamide and stir at 400r / min for 10min; S22. Add 0.003g glycine and 0.003g hexamethylenetetramine to the mixture obtained in step S21, and disperse it by ultrasonication at a frequency of 40kHz for 8 minutes to finally obtain the nitrogen source modifier.
[0029] The preparation of the sulfur source modifier includes the following steps: S31. Mix 0.02g thiourea and 0.6g N,N-dimethylformamide and stir at 400r / min for 10min; S32. Add 0.003g L-cysteine and 0.002g thioacetamide to the mixture obtained in step S31, and disperse it ultrasonically at a frequency of 40kHz for 8min to finally obtain the sulfur source modifier.
[0030] The preparation of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries includes the following steps: S1. Dissolve 2.8g of ferric chloride hexahydrate in 32g of N,N-dimethylformamide and stir thoroughly until completely dissolved to obtain an iron salt solution; S2. Slowly add the iron salt solution obtained in S1 to 32g of silicon-based modified solution, then add 0.6g of nitrogen source modifier and 0.6g of sulfur source modifier, and mix by ultrasonication to fully disperse the components to obtain the reaction precursor solution; S3. The reaction precursor solution obtained in step S2 was transferred to a polytetrafluoroethylene-lined reactor for solvothermal reaction (reaction temperature 115℃, reaction time 22h). After the reaction was completed, it was naturally cooled to room temperature, centrifuged, washed (using N,N-dimethylformamide and deionized water alternately for washing), and dried (vacuum drying at 62℃ for 13h) to obtain the Si / MIL-101(Fe) composite precursor. S4. The Si / MIL-101(Fe) composite precursor obtained in S3 is thoroughly ground and subjected to high-temperature carbonization treatment under argon atmosphere protection (heating rate is 6℃ / min, carbonization temperature is 610℃, and holding time is 4h) to finally obtain nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material.
[0031] Example 3 A method for preparing nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries: Before preparing the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries, the following steps are taken: Preparation of silicon-based modifying solution, nitrogen source modifier, and sulfur source modifier are performed: The preparation of the silicon-based modified liquid includes the following steps: S11. Dissolve 0.8g of terephthalic acid in 30g of N,N-dimethylformamide and stir at 400r / min for 28min at room temperature to obtain a preliminary mixture; S12. Add 0.025g cetyltrimethylammonium bromide, 0.015g PVP-K30, and 0.015g PEG-400 to the preliminary mixture obtained in step S11, and continue stirring for 12 minutes to obtain the secondary mixture; S13. Add 0.01g of nano-silicon and 0.008g of KH-570 to the secondary mixture obtained in step S12, and disperse it in an ultrasonic cleaner for 30 minutes to obtain a silicon-based modified liquid.
[0032] The preparation of nitrogen source modifiers includes the following steps: S21. Add 0.035g urea and 0.003g dicyandiamide to 0.5g N,N-dimethylformamide and stir at 300r / min for 9min; S22. Add 0.002g glycine and 0.002g hexamethylenetetramine to the mixture obtained in step S21, and disperse it by ultrasonication at a frequency of 40kHz for 6min to finally obtain the nitrogen source modifier.
[0033] The preparation of the sulfur source modifier includes the following steps: S31. Mix 0.015g thiourea and 0.5g N,N-dimethylformamide and stir at 300r / min for 9min; S32. Add 0.002g L-cysteine and 0.0015g thioacetamide to the mixture obtained in step S31, and disperse it by ultrasonication at a frequency of 40kHz for 6min to finally obtain the sulfur source modifier.
[0034] The preparation of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries includes the following steps: S1. Dissolve 2.7g of ferric chloride hexahydrate in 30g of N,N-dimethylformamide and stir thoroughly until completely dissolved to obtain an iron salt solution; S2. Slowly add the iron salt solution obtained in S1 to 30g of silicon-based modified solution, then add 0.5g of nitrogen source modifier and 0.5g of sulfur source modifier, and mix by ultrasonication to fully disperse the components to obtain the reaction precursor solution; S3. The reaction precursor solution obtained in step S2 is transferred to a polytetrafluoroethylene-lined reactor for solvothermal reaction (reaction temperature is 110℃, reaction time is 20h). After the reaction is completed, it is naturally cooled to room temperature, centrifuged, washed (using N,N-dimethylformamide and deionized water alternately for washing), and dried (vacuum drying at 60℃ for 12h) to obtain the Si / MIL-101(Fe) composite precursor. S4. The Si / MIL-101(Fe) composite precursor obtained in S3 is thoroughly ground and subjected to high-temperature carbonization treatment under argon atmosphere protection (heating rate of 5℃ / min, carbonization temperature of 600℃, and holding time of 3h) to finally obtain nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material.
[0035] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that no sulfur source modifier was added in this comparative example. The remaining steps are exactly the same in Comparative Example 1 and Example 1. Furthermore, the product of this comparative example is named Si / Fe3O4@NC.
[0036] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that no nitrogen source modifier was added in this comparative example. The remaining steps are exactly the same in Comparative Example 2 and Example 1. Furthermore, the product of this comparative example is named Si / Fe3O4@SC.
[0037] Comparative Example 3 The only difference between Comparative Example 3 and Example 1 is that no sulfur source modifier or nitrogen source modifier was added in this comparative example. The remaining steps are exactly the same in Comparative Example 3 and Example 1. Furthermore, the product of this comparative example is named Si / Fe3O4@C.
[0038] Performance testing: Appendix Figure 2 SEM images of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention are shown, where a is Comparative Example 3, b is Comparative Example 1, c is Comparative Example 2, and d is Example 1. The Si / Fe3O4@C material exhibits a regular octahedral morphology with clear crystal outlines and a relatively smooth surface, maintaining the complete shape of the MOF-derived carbon framework. The Si / Fe3O4@NC material maintains the octahedral framework, but the crystal surface shows slight roughening, indicating that nitrogen doping modification affects the surface morphology of the material. The Si / Fe3O4@SC material still retains the octahedral configuration, but the surface wrinkling is further enhanced, with sulfur doping causing more uneven structures on the carbon layer surface. The Si / Fe3O4@N,SC material still maintains the octahedral macroscopic framework, but the surface wrinkling and roughness are significantly increased, indicating that the nitrogen and sulfur co-doping in the nitrogen and sulfur source modifiers work synergistically on the carbon matrix, modifying the material surface while retaining the original framework structure.
[0039] Appendix Figure 3 The images show TEM images of the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries obtained in Example 1 of this invention at different magnifications. Image a is a TEM image at 500 nm, and image b is a TEM image at 10 nm. The images show that the material maintains an octahedral framework structure, with various phase particles embedded within the octahedrons. Dark spherical particles are visible dispersed within the carbon framework in localized areas, corresponding to the Fe3O4 component. Simultaneously, larger particles, corresponding to the elemental Si component, are observed within the framework. The high-resolution images clearly show two lattice fringes: a 0.309 nm lattice fringe matching the (111) crystal plane of elemental Si, and a 0.246 nm lattice fringe matching the (311) crystal plane of Fe3O4. Both phase particles are encapsulated and fixed by the carbon matrix, indicating that the Si and Fe3O4 particles were successfully confined within the MOF-derived carbon framework under the action of the silicon-based modification liquid, thus constructing a composite structure.
[0040] Appendix Figure 4 The XRD patterns of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention are shown, with a magnified view on the right. As can be seen from the figures, multiple sharp characteristic diffraction peaks were detected in all four groups of samples. The positions of these diffraction peaks match the characteristic peak positions of the Si standard card PDF#27-1402 and the Fe3O4 standard card PDF#08-8866, confirming the presence of crystalline silicon and iron(III) oxide phases in the composite material. Comparison of the magnified areas reveals a slight shift in the characteristic diffraction peaks of the nitrogen-sulfur co-doped samples compared to the Si / Fe3O4@C samples, indicating that the doping of nitrogen and sulfur heteroatoms in the nitrogen and sulfur source modifiers can cause lattice micro-distortions, thus regulating the crystal structure of the material. Furthermore, the absence of obvious heterodiffraction peaks in the spectra indicates that the prepared series of composite materials have high phase purity.
[0041] Appendix Figure 5 The figures show the Raman spectroscopy of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention. It can be observed from the figures that different samples exhibit variations at approximately 1350 cm⁻¹. -1 and 1580cm -1 Distinct characteristic peaks appeared in the vicinity, corresponding to the D and G bands of the carbon material, respectively, indicating the presence of a carbon phase structure in the composite material. The undoped sample had the lowest ID / IG value. In contrast, the nitrogen-sulfur co-doped Si / Fe3O4 / N obtained in Example 1 showed the highest ID / IG value in the SC sample, reflecting that the co-doping of nitrogen and sulfur heteroatoms in the nitrogen and sulfur source modifiers can introduce more structural defects into the carbon matrix, increasing the disorder of the carbon material.
[0042] Appendix Figure 6 The graphs show the discharge specific capacity of the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention as a function of cycle number under the same test conditions. As can be seen from the graphs, different samples exhibited high discharge specific capacity in the initial cycling stage. Subsequently, with the increase of cycle number, the specific capacity gradually decreased and tended to stabilize relatively. In the middle and later cycling stages, the change in discharge specific capacity of each sample decreased, showing relatively stable cycling characteristics. Compared with the samples with single nitrogen doping and single sulfur doping, the nitrogen-sulfur co-doped modified Si / Fe3O4 / C composite material maintained a higher discharge specific capacity throughout the entire cycling process, with slower capacity decay in the long cycling stage, maintaining stable capacity output. This demonstrates the synergistic effect of the silicon-based modifying liquid, nitrogen source modifier, and sulfur source modifier on the synergistic improvement of electrochemical lithium storage performance.
[0043] Appendix Figure 7This is a graph showing the change in discharge specific capacity as a function of cycle number for the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention, under the same test conditions. The discharge specific capacity curves show that the discharge specific capacity of each sample fluctuates somewhat in the initial cycling stage, and then gradually stabilizes with increasing cycle number. During long cycling, all samples maintain relatively stable capacity output, indicating that the prepared materials possess good cycling stability. Comparison of different samples reveals that the nitrogen-sulfur co-doped modified Si / Fe3O4 / C composite material maintains a higher discharge specific capacity and smaller capacity fluctuation during long cycling, demonstrating the regulatory effect of the synergistic action of the silicon-based modifier, nitrogen source modifier, and sulfur source modifier on the electrochemical lithium storage behavior of the material.
[0044] Appendix Figure 8 The figures show nitrogen adsorption-desorption isotherms of the nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention. Figure 9 The attached diagram shows the pore size distribution curves of nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode materials for lithium-ion batteries obtained in Example 1 and Comparative Examples 1-3 of this invention. Figure 8 and attached Figure 9 As the relative pressure increases, the nitrogen adsorption capacity of each sample group gradually increases. Comparing the four samples, the nitrogen-sulfur co-doped Si / Fe3O4 / C obtained in Example 1 has the highest gas adsorption capacity, indicating that its specific surface area and pore volume are superior to those of the single-doped and undoped samples. The pore size distribution results show that heteroatom doping can effectively regulate the pore structure of the material and increase the pore volume, and nitrogen-sulfur co-doping modification can construct more abundant pores within the carbon framework. This porous structure facilitates the full wetting of the material interior by the electrolyte, shortens the lithium-ion diffusion distance, and effectively alleviates the huge volume expansion of silicon-based materials during charging and discharging, maintaining the stability of the electrode structure.
[0045] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries, characterized in that, The preparation steps include the following: S1. Dissolve 2.6-2.8 parts by weight of ferric chloride hexahydrate in 28-32 parts of N,N-dimethylformamide and stir thoroughly until completely dissolved to obtain an iron salt solution; S2. Slowly add the iron salt solution obtained in S1 to 28-32 parts of silicon-based modified solution, then add 0.4-0.6 parts of nitrogen source modifier and 0.4-0.6 parts of sulfur source modifier, and mix by ultrasonication to fully disperse the components to obtain the reaction precursor solution; S3. The reaction precursor solution obtained in step S2 is transferred to a polytetrafluoroethylene-lined reactor for solvothermal reaction. After the reaction is completed, it is naturally cooled to room temperature, centrifuged, washed and dried to obtain the Si / MIL-101(Fe) composite precursor. S4. The Si / MIL-101(Fe) composite precursor obtained in S3 is thoroughly ground and subjected to high-temperature carbonization under argon atmosphere protection to finally obtain nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material. The preparation of the silicon-based modified liquid includes the following steps: S11. Dissolve 0.7-0.9 parts by weight of terephthalic acid in 28-32 parts of N,N-dimethylformamide, and stir at 300-500 r / min for 25-30 min at room temperature to obtain a preliminary mixture; S12. Add 0.02-0.03 parts of cetyltrimethylammonium bromide, 0.01-0.02 parts of PVP-K30, and 0.01-0.02 parts of PEG-400 to the preliminary mixture obtained in step S11, and continue stirring for 10-15 minutes to obtain the secondary mixture; S13. Add 0.09-0.11 parts of nano-silicon and 0.007-0.009 parts of KH-570 to the secondary mixture obtained in step S12, and disperse it ultrasonically in an ultrasonic cleaner for 28-32 minutes to obtain a silicon-based modified liquid; The nitrogen source modifiers include: urea, dicyandiamide, N,N-dimethylformamide, glycine, and hexamethylenetetramine; The sulfur source modifiers include: thiourea, N,N-dimethylformamide, L-cysteine, and thioacetamide.
2. The method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to claim 1, characterized in that, The preparation of the nitrogen source modifier includes the following steps: S21. By weight, add 0.03-0.04 parts of urea and 0.002-0.004 parts of dicyandiamide to 0.4-0.6 parts of N,N-dimethylformamide, and stir at 200-400 r / min for 8-10 min. S22. Add 0.001-0.003 parts of glycine and 0.001-0.003 parts of hexamethylenetetramine to the mixture obtained in step S21, and disperse by ultrasonication for 5-8 minutes to finally obtain the nitrogen source modifier.
3. The method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to claim 1, characterized in that, The preparation of the sulfur source modifier includes the following steps: S31. By weight, mix 0.01-0.02 parts of thiourea and 0.4-0.6 parts of N,N-dimethylformamide and stir at 200-400 r / min for 8-10 min; S32. Add 0.001-0.003 parts of L-cysteine and 0.001-0.002 parts of thioacetamide to the mixture obtained in step S31, and disperse it ultrasonically at a frequency of 40 kHz for 5-8 min to finally obtain the sulfur source modifier.
4. The method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to claim 1, characterized in that, The solvothermal reaction is carried out at a temperature of 105-115℃ for 18-22 hours.
5. The method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to claim 1, characterized in that, The washing in step S3 is performed by alternating between N,N-dimethylformamide and deionized water.
6. The method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to claim 1, characterized in that, The drying in step S3 is vacuum drying at 58-62℃ for 11-13 hours.
7. The method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to claim 1, characterized in that, In step S4, the heating rate of the high-temperature carbonization treatment is 4-6℃ / min, the carbonization temperature is 590-610℃, and the holding time is 2-4h.
8. The method for preparing a nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries according to claim 2, characterized in that, In step S22, the frequency of ultrasonic dispersion is 40 kHz.
9. A nitrogen-sulfur co-doped Si / Fe3O4 / C composite anode material for lithium-ion batteries, characterized in that, It is prepared by the preparation method described in any one of claims 1-8.