Low-expansion silicon-carbon negative electrode material, preparation method and application thereof, and lithium ion battery

By forming a polypyrrole hydrogel conductive polymer layer with gradient modulus and a single-walled carbon nanotube network on the surface of a silicon-carbon matrix, the structural damage caused by volume changes during lithiation/delithiation of silicon-based anode materials is solved, achieving efficient suppression of volume expansion and improvement of cycle stability.

CN123151402APending Publication Date: 2026-11-24ZHEJIANG GOLDEN FEATHER NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611666873.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The drastic volume changes of silicon-based anode materials during lithiation/delithiation lead to mechanical crushing of the electrode structure, loss of electrical contact between the active material and the current collector, and repeated rupture of the SEI film, resulting in rapid capacity decay of the battery. Existing conductive polymer coatings have limited flexibility and cannot provide effective protection continuously.

Method used

A phased in-situ polymerization method was used to form a polypyrrole hydrogel conductive polymer layer with gradient modulus on the surface of a silicon-carbon matrix. Combined with single-walled carbon nanotubes, the multilayer structure buffers volume expansion and constructs a highly efficient conductive network, thereby suppressing the volume expansion of silicon and improving cycle stability.

Benefits of technology

It significantly suppressed the volume expansion of silicon-carbon materials, improved cycle stability and conductivity, and extended the lifespan of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123151402A_ABST
    Figure CN123151402A_ABST
Patent Text Reader

Abstract

This invention relates to the field of electrode materials technology, and more particularly to a low-expansion silicon-carbon anode material, its preparation method, its application, and lithium-ion batteries. This invention provides a method for preparing a low-expansion silicon-carbon anode material. The preparation method of this invention utilizes gradient modulus to gradually attenuate volume expansion stress, providing a reversible compression buffer space for the sheet-like multilayer polypyrrole, using defect regions as stress dissipation sacrificial sites, and simultaneously using SWCNT bridging to suppress crack propagation. Thus, under a low-energy-consumption process that eliminates the need for high-temperature carbonization (only drying at 80-120℃), it significantly suppresses silicon volume expansion, improves cycle stability, and also ensures a highly efficient conductive network. This solves the technical problems of existing single-structure coating layers being prone to cracking, having insufficient buffering capacity, and requiring high-content conductive agents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, specifically to a low-expansion silicon-carbon anode material, its preparation method and application, and lithium-ion batteries. Background Technology

[0002] Silicon-based anode materials are considered one of the key materials for breaking through the current energy density bottleneck of lithium-ion batteries due to their ultra-high theoretical specific capacity (4200 mA·h / g). However, the drastic volume change (>300%) of silicon materials during lithiation / delithiation can lead to mechanical pulverization of the electrode structure, loss of electrical contact between the active material and the current collector, and repeated rupture and regeneration of the solid electrolyte interphase (SEI) film, resulting in rapid capacity decay and severely restricting their commercial application.

[0003] To mitigate the volume expansion problem, coating silicon-carbon materials with conductive polymers is an effective modification strategy in existing technologies. Conductive polymers combine flexibility and conductivity, and can buffer volume changes to a certain extent. Among them, polypyrrole (PPy) has attracted much attention due to its good conductivity, high environmental stability, and simple preparation process. However, polypyrrole prepared by conventional chemical oxidative polymerization methods usually exhibits a dense granular or spherical morphology, and its coating layer has limited flexibility, making it prone to cracking during long-term cycling and unable to provide effective protection continuously. Summary of the Invention

[0004] In view of this, the purpose of this invention is to provide a low-expansion silicon-carbon anode material, its preparation method, its application, and lithium-ion batteries. The low-expansion silicon-carbon anode material prepared by the method described herein can significantly suppress the volume expansion of silicon-carbon materials and improve their cycle stability.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing a low-expansion silicon-carbon anode material, comprising the following steps: A silicon-carbon matrix is ​​surface modified to obtain a modified silicon-carbon matrix; the surface modification includes surface oxidation modification. A mixed dispersion is obtained by mixing single-walled carbon nanotubes with an acidic aqueous solution containing pyrrole monomer and a dopant; the dopant in the acidic aqueous solution is one or more of sodium benzenesulfonate, sodium p-toluenesulfonate, and sodium β-naphthalenesulfonate. The modified silicon-carbon matrix was placed in the mixed dispersion for staged in-situ polymerization to obtain a product slurry; The product slurry was spray-dried to obtain the low-expansion silicon-carbon anode material; The staged in-situ polymerization is carried out under the condition of adding an oxidant, and the staged in-situ polymerization includes a first stage in-situ polymerization, a second stage in-situ polymerization and a third stage in-situ polymerization carried out sequentially; the oxidant includes one or more of anhydrous ferric chloride, ferric chloride hexahydrate, ammonium persulfate and potassium persulfate; The temperature, time, and molar ratio of oxidant to pyrrole monomer all showed an increasing trend in the first-stage in-situ polymerization, the second-stage in-situ polymerization, and the third-stage in-situ polymerization.

[0006] Preferably, the temperature of the first stage of in-situ polymerization is 0~5℃, the time is 0.3-1.0, and the molar ratio of oxidant to pyrrole monomer is (0.8~1.2):1.

[0007] Preferably, the temperature for the second stage of in-situ polymerization is 20~25℃, the time is 1.0~2.0h, and the molar ratio of oxidant to pyrrole monomer is (1.2~1.5):1; The time required to raise the temperature from the first stage in-situ polymerization temperature to the second stage in-situ polymerization temperature is 0.5~1.0 h.

[0008] Preferably, the temperature of the third-stage in-situ polymerization is 30~40℃, the time is 2.0~4.0h, and the molar ratio of oxidant to pyrrole monomer is (1.5~2.0):1; The time required to raise the temperature from the second stage in-situ polymerization temperature to the third stage in-situ polymerization temperature is 0.8 hours, not exceeding 1 hour.

[0009] Preferably, the surface oxidation modification method is a chemical oxidation method; The chemical oxidation process includes: Ammonia, hydrogen peroxide, and water are mixed to obtain a mixture; The silicon-carbon matrix is ​​placed in the mixture for surface hydrophilic modification to obtain the modified silicon-carbon matrix.

[0010] Preferably, the volume ratio of ammonia, hydrogen peroxide, and water is 1:1:5; the mass percentage concentration of ammonia is 25%, and the mass percentage concentration of hydrogen peroxide is 30%. The ratio of silicon-carbon matrix to the mixture is 1g:(10~20)mL; The surface hydrophilization modification temperature is 95~100℃, and the time is 40~60min.

[0011] Preferably, the inlet temperature of the spray dryer is 150~200℃ and the outlet temperature is 80~100℃.

[0012] The present invention also provides a low-expansion silicon-carbon anode material prepared by the preparation method described above, comprising a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; Single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer.

[0013] Preferably, the mass of the single-walled carbon nanotubes accounts for 0.02 to 0.06% of the mass of the silicon-carbon matrix.

[0014] The present invention also provides a lithium-ion battery, including a negative electrode active material, wherein the negative electrode active material is the low-expansion silicon-carbon negative electrode material described in the above technical solution.

[0015] This invention also provides a method for preparing a low-expansion silicon-carbon anode material, comprising the following steps: surface modification of a silicon-carbon matrix to obtain a modified silicon-carbon matrix; the surface modification includes surface oxidation modification; mixing single-walled carbon nanotubes with an acidic aqueous solution containing pyrrole monomer and a dopant to obtain a mixed dispersion; the dopant in the acidic aqueous solution is one or more of sodium benzenesulfonate, sodium p-toluenesulfonate, and sodium β-naphthalenesulfonate; placing the modified silicon-carbon matrix in the mixed dispersion for staged in-situ polymerization to obtain a product slurry; and then... The product slurry is spray-dried to obtain the low-expansion silicon-carbon anode material; the staged in-situ polymerization is carried out under the condition of adding an oxidant, and the staged in-situ polymerization includes a first-stage in-situ polymerization, a second-stage in-situ polymerization, and a third-stage in-situ polymerization carried out sequentially; the oxidant includes one or more of anhydrous ferric chloride, ferric chloride hexahydrate, ammonium persulfate, and potassium persulfate; the temperature, time, and molar ratio of oxidant to pyrrole monomer in the first-stage in-situ polymerization, the second-stage in-situ polymerization, and the third-stage in-situ polymerization all show an increasing trend. The polypyrrole hydrogel conductive polymer layer of this invention has gradient modulus characteristics. This design utilizes the gradient modulus to gradually attenuate the volume expansion stress, providing a reversible compression buffer space for the sheet-like multilayer polypyrrole, using the defect area as a stress dissipation sacrificial site, and at the same time, SWCNT bridging inhibits crack propagation. Thus, under a low-energy consumption process that does not require high-temperature carbonization (only drying at 80-120℃), it significantly suppresses the volume expansion of silicon, improves cycle stability, and also takes into account the high-efficiency conductive network. This solves the technical problems of existing single-structure coating layers being prone to cracking, having insufficient buffering capacity, and requiring high content of conductive agents. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the silicon-carbon matrix used in this invention; wherein, 1 is a porous carbon framework, 2 is nano-silicon, and 3 is a carbon coating layer; Figure 2 The image shows a SEM image of the low-expansion silicon-carbon anode material described in Example 1. Figure 3 The image shows a SEM image of the low-expansion silicon-carbon anode material described in Example 2. Detailed Implementation

[0017] This invention provides a method for preparing a low-expansion silicon-carbon anode material, comprising the following steps: A silicon-carbon matrix is ​​surface modified to obtain a modified silicon-carbon matrix; the surface modification includes surface oxidation modification. A mixed dispersion was obtained by mixing single-walled carbon nanotubes with an acidic aqueous solution containing pyrrole monomers and dopants. The modified silicon-carbon matrix was placed in the mixed dispersion for staged in-situ polymerization to obtain a product slurry; The product slurry was spray-dried to obtain the low-expansion silicon-carbon anode material; The staged in-situ polymerization is carried out under the condition of adding an oxidant, and the staged in-situ polymerization includes a first stage in-situ polymerization, a second stage in-situ polymerization and a third stage in-situ polymerization carried out sequentially. The temperature, time, and molar ratio of oxidant to pyrrole monomer all showed an increasing trend in the first-stage in-situ polymerization, the second-stage in-situ polymerization, and the third-stage in-situ polymerization.

[0018] In this invention, unless otherwise specified, all raw materials used in the preparation are commercially available products well known to those skilled in the art.

[0019] The present invention modifies the surface of a silicon-carbon matrix to obtain a modified silicon-carbon matrix; the surface modification includes surface oxidation modification.

[0020] In this invention, the purpose of the surface modification is to enrich the surface of the silicon-carbon matrix with hydroxyl and amino groups.

[0021] In this invention, the surface oxidation modification method is a chemical oxidation method; The preferred process of the chemical oxidation method includes: Ammonia, hydrogen peroxide, and water are mixed to obtain a mixture; The silicon-carbon matrix is ​​placed in the mixture for surface oxidation modification to obtain the modified silicon-carbon matrix.

[0022] This invention involves mixing ammonia, hydrogen peroxide, and water to obtain a mixed solution.

[0023] In this invention, the mass percentage concentration of the ammonia water is preferably 25%, the mass percentage concentration of the hydrogen peroxide is preferably 30%, and the water is preferably deionized water.

[0024] In this invention, the volume ratio of ammonia, hydrogen peroxide and water is preferably 1:1:5.

[0025] In this invention, the mixing is preferably carried out under stirring conditions. This invention does not impose any special limitations on the stirring process, and any process well known to those skilled in the art can be used.

[0026] After obtaining the mixture, the present invention places the silicon-carbon matrix in the mixture for surface oxygen hydration modification to obtain the modified silicon-carbon matrix.

[0027] In this invention, the preferred ratio of the silicon-carbon matrix to the mixture is 1g:(10~20)mL, more preferably 1g:10mL, 1g:12mL, 1g:14mL, 1g:16mL, 1g:18mL or 1g:20mL.

[0028] In this invention, the surface hydrophilic modification is preferably carried out under stirring conditions. The surface oxidation modification temperature is preferably 95~100℃, more preferably 95℃, 96℃, 97℃, 98℃, 99℃ or 100℃; the time is preferably 40~60min, more preferably 40min, 45min, 50min, 55min or 60min. This invention does not impose any special limitation on the stirring speed; any speed well known to those skilled in the art can be used.

[0029] In this invention, if the surface oxidation modification time is less than the above range, the hydroxylation will be insufficient; if it is greater than the above range, the surface oxide layer will be too thick, increasing the interfacial resistance.

[0030] After the surface oxidation modification is completed, the present invention preferably includes washing, filtering and drying in sequence; the washing is preferably repeated 3 to 5 times with deionized water until the pH of the washing solution is neutral (pH=6.5~7.5); the filtration is preferably carried out by vacuum filtration or centrifugation; the centrifugation speed is preferably 3000~5000 rpm and the time is preferably 5~10 minutes; the drying is preferably vacuum drying, the vacuum drying temperature is preferably 80~120℃ and the time is preferably 2~12 hours.

[0031] The preparation method of the present invention further includes mixing single-walled carbon nanotubes with an acidic aqueous solution containing pyrrole monomer and dopant to obtain a mixed dispersion; the dopant in the acidic aqueous solution of the dopant is one or more of sodium benzenesulfonate, sodium p-toluenesulfonate and sodium β-naphthalenesulfonate.

[0032] In this invention, the pH value of the acidic aqueous solution containing pyrrole monomer and dopant is preferably 1.5 to 2.5, more preferably 1.5, 2.0 or 2.5.

[0033] In this invention, the concentration of pyrrole monomer in the acidic aqueous solution containing pyrrole monomer and dopant is preferably 1~10 g / L, more preferably 1 g / L, 2 g / L, 4 g / L, 6 g / L, 8 g / L or 10 g / L; the concentration of dopant is preferably 0.5~5 g / L, more preferably 0.5 g / L, 1 g / L, 1.5 g / L, 2.0 g / L, 2.5 g / L, 3.0 g / L, 3.5 g / L, 4.0 g / L, 4.5 g / L or 5 g / L.

[0034] In this invention, the dopant is one or more of sodium benzenesulfonate, sodium p-toluenesulfonate, and sodium β-naphthalenesulfonate, more preferably sodium benzenesulfonate; when the dopant is two or more of the above-mentioned specific selections, this invention does not impose any special limitation on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio.

[0035] In this invention, the dopant acts as both an "emulsifier" and a structural "template". The specific dopant (preferably sodium benzenesulfonate) does not only participate in the doping of polypyrrole as a traditional "charge-balancing ion", but also undertakes four functions: emulsification and solubilization, structure guidance, interface anchoring and charge balancing. It is a key auxiliary agent to ensure the smooth polymerization of hydrophobic pyrrole monomers in the aqueous phase and the formation of a gradient hydrogel coating layer on the silicon-carbon surface, thereby directly affecting the uniformity, conductivity and volume expansion suppression effect of the coating layer.

[0036] In this invention, the mass ratio of the single-walled carbon nanotubes to the pyrrole monomer is preferably 1:200 to 1:1000, more preferably 1:200, 1:300, 1:400, 1:500, 1:600, 1:700, 1:800, 1:900 or 1:1000.

[0037] In this invention, controlling the amount of the single-walled carbon nanotubes within the above-mentioned range ensures the synergistic effect of highly efficient conductive network and mechanical enhancement with extremely low addition amount.

[0038] In this invention, the mixing is preferably performed under ultrasonic conditions, wherein the frequency of the ultrasonic waves is preferably 20-40 kHz, more preferably 20 kHz, 30 kHz or 40 kHz; and the time is preferably 10-60 min, more preferably 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0039] After obtaining the mixed dispersion, the present invention places the modified silicon-carbon matrix in the mixed dispersion for staged in-situ polymerization to obtain a product slurry; the staged in-situ polymerization is carried out under the condition of adding an oxidant, and the staged in-situ polymerization includes a first stage in-situ polymerization, a second stage in-situ polymerization and a third stage in-situ polymerization carried out sequentially; the temperature, time and the molar ratio of oxidant to pyrrole monomer in the first stage in-situ polymerization, the second stage in-situ polymerization and the third stage in-situ polymerization all show an increasing trend; the oxidant includes one or more of anhydrous ferric chloride, ferric chloride hexahydrate, ammonium persulfate and potassium persulfate.

[0040] In this invention, the oxidant preferably includes one or more of anhydrous ferric chloride, ferric chloride hexahydrate, ammonium persulfate, and potassium persulfate. When the oxidant is two or more of the above-mentioned specific selections, this invention does not impose any special limitation on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio.

[0041] In this invention, the staged in-situ polymerization is preferably carried out under stirring conditions. This invention does not impose any special limitations on the stirring process, and any process well known to those skilled in the art can be used.

[0042] In this invention, the temperature of the first stage in-situ polymerization is preferably 0~5℃, more preferably 0℃, 1℃, 2℃, 3℃, 4℃ or 5℃; the time is preferably 0.5h, and the molar ratio of the oxidant to the pyrrole monomer is preferably (0.8~1.2):1, more preferably 0.8:1, 0.9:1, 1.0:1, 1.1:1 or 1.2:1. In this invention, the preferred temperature for the second-stage in-situ polymerization is 20-25°C, more preferably 20°C, 21°C, 22°C, 23°C, 24°C, or 25°C; the preferred time is 1.0-2.0 h, more preferably 1.0 h, 1.5 h, or 2.0 h; the preferred molar ratio of oxidant to pyrrole monomer is (1.2-1.5):1, more preferably 1.2:1, 1.3:1, 1.4:1, or 1.5:1; the preferred time for heating from the temperature of the first-stage in-situ polymerization to the temperature of the second-stage in-situ polymerization is 0.5-1.0 h, more preferably 0.5 h, 0.6 h, or 0.7 h. The preferred in-situ polymerization temperature for the third stage is 30-40°C, more preferably 30°C, 35°C, or 40°C; the preferred time is 2.0-4.0h, more preferably 2.0h, 3.0h, or 4.0h; the preferred molar ratio of oxidant to pyrrole monomer is (1.5-2.0):1, more preferably 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, or 2.0:1; the preferred time for heating from the temperature of the second stage in-situ polymerization to the temperature of the third stage in-situ polymerization is 0.5-1.0h, more preferably 0.5h.

[0043] In this invention, the staged in-situ polymerization precisely constructs the polypyrrole hydrogel conductive polymer layer described above by controlling the temperature, reaction time, and amount of oxidant.

[0044] After obtaining the product slurry, the present invention performs spray drying on the product slurry to obtain the low-expansion silicon-carbon anode material.

[0045] In this invention, the inlet temperature of the spray dryer is preferably 150~200℃, more preferably 150℃, 160℃, 170℃, 180℃, 190℃ or 200℃; the outlet temperature is preferably 80~100℃, more preferably 80℃, 90℃ or 100℃.

[0046] After the spray drying is completed, the present invention preferably includes drying, which is preferably carried out in an argon atmosphere, at a temperature of 100°C and for a time of 8 hours.

[0047] In this invention, the polypyrrole hydrogel conductive polymer layer in the low-expansion silicon-carbon anode material prepared above can provide both structural support and a stress transfer interface, and can also absorb strain energy through chain segment deformation and pore compression. Simultaneously, the sheet-like multilayer polypyrrole provides a physical buffer space for the volume expansion of silicon. When the cell is charged, lithium ions enter the interior of the anode material from the positive electrode through the negative electrode interface, where they undergo an electrochemical alloying reaction with silicon atoms to form a lithium-silicon alloy (Li₂). x The lithiation of silicon (Si) is not a one-step process, but rather involves multiple phase transition stages, gradually transforming from crystalline silicon to an amorphous lithium-silicon alloy. The final product of silicon lithiation, crystalline Li, is then formed. 15 The volume expansion of Si4 reaches approximately 300%-400%. The carbon framework initially inhibits the expansion of silicon, but its ability is limited. At this point, the outer polypyrrole hydrogel conductive polymer layer can effectively inhibit the expansion of the silicon-carbon matrix, preventing excessive expansion that could lead to matrix breakage, SEI film failure, and accelerated cycle degradation. When the cell discharges, Li... 15Si4 undergoes gradual delithiation, eventually reverting to amorphous silicon. During delithiation, as silicon contracts and rebounds, the elastic recovery of the pore walls allows the pores to reopen, achieving a reversible buffering effect of compression-recovery. Without the constraint of the polypyrrole hydrogel conductive polymer layer on expansion, the rapid rebound of the silicon system would lead to the collapse of the carbon skeleton, resulting in material failure and accelerated cycle decay. Simultaneously, peroxidation defects and structurally disordered regions in the sheet-like multilayer polypyrrole become sacrificial sites for stress dissipation, absorbing expansion energy through local rearrangement and slippage of molecular chain segments. Finally, a critically low dosage (on the order of one ten-thousandth) of SWCNTs is uniformly dispersed and interspersed within the polypyrrole hydrogel conductive polymer layer, forming a three-dimensional conductive network composed of interlocking single-walled carbon nanotubes. This not only compensates for the insufficient intrinsic conductivity of polypyrrole but also inhibits crack propagation through the bridging effect of SWCNTs, enhancing the mechanical strength of the coating layer. During cell cycling, the continuous expansion and contraction of silicon-carbon materials cause the carbon skeleton to collapse continuously, leading to the SEI film to break and reorganize. This continuously consumes electrolyte, reduces lithium insertion sites, increases local impedance, and exacerbates local temperature rise, while also causing severe lithium plating and accelerating cycle degradation.

[0048] This invention provides a low-expansion silicon-carbon anode material prepared by the preparation method described above, comprising a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; Single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer.

[0049] In this invention, the particle size (D50) of the silicon-carbon matrix is ​​preferably 7.5~10.5μm, more preferably 9.0±1.0μm.

[0050] In this invention, the silicon-carbon matrix is ​​preferably vapor-deposited silicon-carbon (CVD silicon-carbon), which has a core-shell structure: nano-silicon is deposited inside a porous carbon framework, and a dense carbon shell is coated on the surface (see schematic diagram). Figure 1 (As shown).

[0051] In this invention, the preferred particle size distribution of the vapor-deposited silicon-carbon is D00 ≥ 1.0 μm, D10 = 5.0 ± 2.0 μm, D50 = 9.0 ± 1.5 μm, and D90 < 19 μm. max ≤35μm; tap density is preferably 0.9±0.2g / cm³. 3 The preferred specific surface area is 2.45 ± 1.5 m². 2 / g; Fe content preferably ≤300ppm, magnetic foreign matter preferably ≤5ppm; the mass percentage of carbon in the vapor-deposited silicon-carbon is preferably 52.0±4.0%; the delithiation specific capacity is preferably 1900±100mA·h / g; the first discharge efficiency is preferably ≥89%.

[0052] In this invention, the thickness of the polypyrrole hydrogel conductive polymer layer is preferably 10~500nm, more preferably 50~200nm.

[0053] In this invention, the mass percentage of the single-walled carbon nanotubes in the silicon-carbon matrix is ​​preferably 0.02~0.06%, more preferably 0.03~0.05%, and most preferably 0.05%.

[0054] In this invention, the diameter of the single-walled carbon nanotube is preferably 1~2 nm, more preferably 1.2~1.5 nm, and the aspect ratio is preferably 1000~5000, more preferably 2000~3000.

[0055] The present invention also provides a lithium-ion battery, including a negative electrode active material, wherein the negative electrode active material is the low-expansion silicon-carbon negative electrode material described in the above technical solution.

[0056] The following detailed description, in conjunction with embodiments, illustrates the low-expansion silicon-carbon anode material, its preparation method, its application, and lithium-ion batteries provided by this invention. However, these descriptions should not be construed as limiting the scope of protection of this invention.

[0057] Example 1 Ammonia (25% by mass), hydrogen peroxide (30% by mass), and deionized water were mixed in a volume ratio of 1:1:5 and stirred until homogeneous to obtain an oxidizing mixture. 100g of silicon-carbon matrix with a D50 of 9.0μm (vapor-deposited silicon-carbon, particle size distribution: D00≥1.0μm, D10=5.0±2.0μm, D50=9.0±1.5μm, D90<19μm, D... max ≤35μm; tap density is 0.9±0.2g / cm³ 3 ; Specific surface area is 2.45±1.5m² 2 / g; Fe content ≤300ppm, magnetic foreign matter ≤5ppm; the mass percentage of carbon in the vapor-deposited silicon-carbon is 52.0±4.0%; the delithiation specific capacity is 1900±100mA·h / g; the first discharge efficiency ≥89%) is added to 1000mL of the above mixture (solid-liquid ratio 1:10), heated to boiling state (98℃), and stirred continuously for 50 minutes. After that, it is washed repeatedly with deionized water 3 times until the pH of the washing solution is neutral (pH=7.0). The solid product is collected by vacuum filtration, and the solid product is placed in a vacuum drying oven and vacuum dried at 100℃ for 6 hours to obtain the modified silicon-carbon matrix. 0.03 g (0.03% relative to the silicon-carbon matrix) of single-walled carbon nanotubes (diameter 1.2~1.5 nm, aspect ratio 2000~3000) were dispersed in 500 mL of deionized water (pH≈2.0) containing 1.0 g of pyrrole monomer and 0.5 g of sodium benzenesulfonate (dopant), and ultrasonically dispersed for 30 min (frequency 30 kHz) to obtain a mixed dispersion. The modified silicon-carbon matrix was added to the above mixed dispersion, and staged in-situ polymerization was carried out under stirring conditions: the mixture was cooled to 2°C in an ice bath, and a solution containing FeCl3·6H2O (FeCl3 / Py molar ratio of 1.0) was slowly added dropwise under stirring. The reaction was carried out at 2°C for 0.5 h (first stage in-situ polymerization). The temperature of the reaction system was then slowly raised to room temperature (20°C) within 0.5 h, and FeCl3·6H2O was added to make the total molar ratio reach 1.2. The reaction was continued to be stirred for 1.5 h (second stage in-situ polymerization). The reaction system was then heated to 35°C, and FeCl3·6H2O was added again to make the total molar ratio reach 1.5. The reaction was continued to be stirred for 3 h (third stage in-situ polymerization) to obtain the product slurry.

[0058] The resulting slurry was then spray-dried at an inlet temperature of 180°C and an outlet temperature of 90°C to obtain spray-dried powder. The spray-dried powder was vacuum-dried at 100°C for 8 hours under an argon atmosphere to obtain a low-expansion silicon-carbon anode material (including a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer includes cauliflower-shaped polypyrrole aggregates and sheet-like multilayer polypyrrole, single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer, the thickness of the polypyrrole hydrogel conductive polymer layer is 180 nm, and the single-walled carbon nanotubes account for 0.03% of the mass of the silicon-carbon matrix). The silicon-carbon anode material was mixed with a conductive agent (Super P) and a binder (CMC) at a mass ratio of 8:1:1 to form a slurry. The slurry was coated onto copper foil, dried, and rolled to form an anode sheet. Using a lithium metal sheet as the counter electrode and LiPF6 / EC+DEC (EC to DEC volume ratio of 1:1) as the electrolyte, CR2032 coin cells were assembled in an argon glove box. Constant current charge-discharge tests were performed at a current density of 0.5C (voltage range 0.005~1.5V), and the electrode sheet thickness change after 100 cycles was measured to calculate the expansion rate (rebound rate). Figure 3 Here is a SEM image of the low-expansion silicon-carbon anode material, from... Figure 3It is evident that the silicon-carbon matrix surface is completely coated with a continuous and uniform polypyrrole hydrogel conductive polymer layer. Closer to the inner side of the silicon-carbon matrix are cauliflower-shaped polypyrrole aggregates with a smooth, dense surface and tightly packed chain segments, providing strong interfacial anchoring and efficient electron transport. The outer side consists of sheet-like porous polypyrrole structures with abundant nanoscale pores distributed between the layers, providing a physical buffer space for the volume expansion of silicon through mesoporous compression. Simultaneously, long-chain CNT structures are interwoven and entangled within the coating layer, particularly prominent in the outer porous region, overlapping to form a continuous three-dimensional conductive network. This not only compensates for the insufficient intrinsic conductivity of polypyrrole but also inhibits crack propagation and enhances the mechanical strength of the coating layer through a bridging effect. The presence of large-area aggregates or free polypyrrole particles indicates that the gradient polymerization process effectively achieved uniform heterogeneous growth of polypyrrole on the silicon-carbon surface.

[0059] Example 2 Referring to Example 1, the difference is that the amount of SWCNT added is 0.05g (five ten-thousandths); a low-expansion silicon-carbon anode material is obtained (including a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer includes cauliflower-shaped polypyrrole aggregates and sheet-like multilayer polypyrrole, single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer, the thickness of the polypyrrole hydrogel conductive polymer layer is 185nm, and the single-walled carbon nanotubes account for 0.05% of the mass of the silicon-carbon matrix). A button cell was fabricated and tested according to the method in Example 1; Figure 3 Here is a SEM image of the low-expansion silicon-carbon anode material, from... Figure 3 It can be seen that there is no significant difference in the coating effect of 0.05% SWCNT.

[0060] Example 3 Referring to Example 1, the difference is that sodium benzenesulfonate is replaced with sodium 2-p-toluenesulfonate to obtain a low-expansion silicon-carbon anode material (including a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer includes cauliflower-shaped polypyrrole aggregates and sheet-like multilayer polypyrrole, single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer, the thickness of the polypyrrole hydrogel conductive polymer layer is 175 nm, and the single-walled carbon nanotubes account for 0.03% of the mass of the silicon-carbon matrix). The button cell was fabricated and tested according to the method in Example 1.

[0061] Example 4 Referring to Example 1, the difference is that sodium benzenesulfonate is replaced with sodium β-naphthalenesulfonate to obtain a low-expansion silicon-carbon anode material (including a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer includes cauliflower-shaped polypyrrole aggregates and sheet-like multilayer polypyrrole, single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer, the thickness of the polypyrrole hydrogel conductive polymer layer is 185 nm, and the single-walled carbon nanotubes account for 0.03% of the mass of the silicon-carbon matrix). The button cell was fabricated and tested according to the method in Example 1.

[0062] Example 5 Referring to Example 1, the difference lies in modifying the temperature of the third-stage in-situ polymerization to 40°C, resulting in a low-expansion silicon-carbon anode material (including a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer includes cauliflower-shaped polypyrrole aggregates and sheet-like multilayer polypyrrole, single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer, the thickness of the polypyrrole hydrogel conductive polymer layer is 200 nm, and the single-walled carbon nanotubes account for 0.03% of the mass of the silicon-carbon matrix). The button cell was fabricated and tested according to the method in Example 1.

[0063] Example 6 Referring to Example 1, the difference is that the FeCl3·6H2O solution is replaced with an ammonium persulfate solution (ammonium persulfate / Py molar ratio is 1.0), resulting in a low-expansion silicon-carbon anode material (including a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer includes cauliflower-shaped polypyrrole aggregates and sheet-like multilayer polypyrrole, single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer, the thickness of the polypyrrole hydrogel conductive polymer layer is 170 nm, and the single-walled carbon nanotubes account for 0.03% of the mass of the silicon-carbon matrix). The button cell was fabricated and tested according to the method in Example 1.

[0064] Example 7 Referring to Example 1, the difference is that the FeCl3·6H2O solution is replaced with a potassium persulfate solution (potassium persulfate / Py molar ratio of 1.0), resulting in a low-expansion silicon-carbon anode material (comprising a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer comprises cauliflower-shaped polypyrrole aggregates and sheet-like multilayer polypyrrole, wherein single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer, the thickness of the polypyrrole hydrogel conductive polymer layer is 165 nm, and the single-walled carbon nanotubes account for 0.03% of the mass of the silicon-carbon matrix). The button cell was fabricated and tested according to the method in Example 1.

[0065] Comparative Example 1 The difference from Example 1 is that the silicon-carbon material is not coated in any way; The button cell was fabricated and tested according to the method in Example 1.

[0066] Comparative Example 2 Referring to Example 1, the difference lies in modifying the temperature of the third-stage in-situ polymerization to 50°C, resulting in a low-expansion silicon-carbon anode material (including a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the thickness of the polypyrrole hydrogel conductive polymer layer is 150 nm, and the single-walled carbon nanotubes account for 0.03% of the mass percentage of the silicon-carbon matrix; excessively high temperatures lead to severe peroxidation of polypyrrole, and a large amount of conjugated molecular chain structure is destroyed, resulting in a loose structure of the polypyrrole hydrogel conductive polymer layer and a significant decrease in conductivity). The button cell was fabricated and tested according to the method in Example 1.

[0067] Comparative Example 3 Referring to Example 1, the difference lies in replacing the dopant with dodecylbenzenesulfonic acid, resulting in a low-expansion silicon-carbon anode material (comprising a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; the polypyrrole hydrogel conductive polymer layer contains dispersed single-walled carbon nanotubes, the thickness of the polypyrrole hydrogel conductive polymer layer is 190 nm, and the single-walled carbon nanotubes account for 0.03% of the mass percentage of the silicon-carbon matrix; since dodecylbenzenesulfonic acid is a macromolecular organic sulfonic acid dopant, its anion volume is much larger than that of sodium benzenesulfonate. Excessive dopant anion volume leads to increased separation between polypyrrole molecular chains, hindering inter-chain hopping of charge carriers and reducing conductivity. Furthermore, the long alkyl chain of dodecyl also interferes with the orderly stacking of polypyrrole chains). The button cell was fabricated and tested according to the method in Example 1.

[0068] Comparative Example 4 Referring to Example 1, the difference is that the FeCl3·6H2O solution was replaced with a ferrous sulfate heptahydrate solution (ferrous sulfate / Py molar ratio of 1.0), resulting in a low-expansion silicon-carbon anode material (FeSO4·7H2O containing Fe). 2+ The oxidizing power of Fe is much weaker than that of FeCl3. 3+ It cannot effectively oxidize pyrrole monomers to initiate polymerization. Furthermore, SO4... 2- The doping efficiency of the doped anion is lower than that of Cl. - Therefore, this comparative ratio cannot form an effective polypyrrole hydrogel conductive polymer layer. The button cell was fabricated and tested according to the method in Example 1.

[0069] Comparative Example 5 Referring to Example 1, the difference is that the FeCl3·6H2O solution was replaced with hydrogen peroxide (H2O2 / Py molar ratio of 1.0), resulting in a low-expansion silicon-carbon anode material (H2O2 has weak oxidizing power, and its oxidation reaction product is H2O, without the generation of doped anions, thus failing to impart high conductivity to polypyrrole. Therefore, this comparative example cannot form an effectively doped conductive polypyrrole hydrogel conductive polymer layer). The button cell was fabricated and tested according to the method in Example 1.

[0070] Comparative Example 6 Referring to Example 1, the difference is that the gradient control step is omitted, the temperature is maintained at 0°C throughout the process, the FeCl3 / Py molar ratio is 1.0, the total reaction time is 5h, and a silicon-carbon anode material is obtained, in which the coating layer is a dense granular polypyrrole layer without a porous outer layer structure. The button cell was fabricated and tested according to the method in Example 1.

[0071] Comparative Example 7 Referring to Example 1, the difference is that the gradient control step is omitted, the temperature is maintained at 35°C throughout the process, the FeCl3 / Py molar ratio is 1.5, and the total reaction time is 5h, to obtain a silicon-carbon anode material, wherein the coating layer is a polypyrrole agglomerate with severe peroxidation and low conductivity. The button cell was fabricated and tested according to the method in Example 1.

[0072] Test case The electrochemical performance of coin cells assembled with the low-expansion silicon-carbon anode materials described in Examples 1-2, the silicon-carbon anode material described in Comparative Example 1, the product described in Comparative Example 2, and the silicon-carbon matrix described in Comparative Example 3 under different test conditions is shown in Table 1. Table 1. Electrochemical performance of coin cells assembled with the low-expansion silicon-carbon anode materials described in Examples 1-7 and the silicon-carbon anode materials described in Comparative Examples 1-7 under different test conditions.

[0073] Note: Rebound rate refers to the rebound rate of the electrode thickness at full charge relative to the thickness after rolling and settling for 48 hours. As shown in Table 1, the low-expansion silicon-carbon anode material prepared by the method described in this invention exhibits significant advantages in terms of cycle stability, volume expansion suppression, and conductivity. Specific analysis is as follows: Example 1 shows a significant improvement in cycle stability. After 100 cycles at 0.5C, the capacity retention rate reached 85.4%, which is 3.9 percentage points higher than that of full-process low-temperature polymerization, 10.6 percentage points higher than that of full-process high-temperature polymerization, and 4.8 percentage points higher than that of uncoated polymerization. This indicates that the gradient temperature polymerization design effectively maintains the integrity of the electrode structure, avoiding coating layer rupture and repeated SEI film regeneration. Example 1 demonstrates outstanding volume expansion suppression, with a 78.4% electrode rebound rate after 100 cycles, representing a 17 percentage point reduction compared to low-temperature polymerization, a 34.4 percentage point reduction compared to high-temperature polymerization, and a 41.8 percentage point reduction compared to uncoated polymerization. This proves that gradient temperature polymerization effectively absorbs the volume expansion stress of silicon through mesoporous compression and chain segment deformation. The dense inner layer uniformly transmits the expansion stress to the outer layer, gradually attenuating it, thus achieving effective suppression of volume expansion. Example 1 exhibits excellent conductivity, with an electrode conductivity of 2.65 S / cm, the highest among all samples. This represents an improvement of 0.25 S / cm compared to the entire low-temperature polymerization process and 1.08 S / cm compared to the entire high-temperature polymerization process. This indicates that the polypyrrole hydrogel conductive polymer layer and the SWCNT three-dimensional conductive network synergistically construct a highly efficient electron transport channel, compensating for the insufficient intrinsic conductivity of polypyrrole and enhancing the mechanical strength of the coating layer through the bridging effect of SWCNTs. Example 1 outperforms Example 2 in all key performance indicators, including cycle retention rate, electrode rebound rate, and electrode conductivity. This indicates that excessive addition leads to local agglomeration of SWCNT in the polypyrrole matrix, which destroys the uniformity and density of the coating layer and reduces the overall performance. Retention rate: Sodium benzenesulfonate > Sodium β-naphthalenesulfonate > Sodium p-toluenesulfonate > Dodecylbenzenesulfonic acid. This indicates that the type of dopant has a significant impact on performance. Sodium benzenesulfonate has the smallest anion volume, which is most conducive to the close packing of polypyrrole molecular chains, forming a dense inner layer with high crystallinity and high conductivity. The large anion of DBSA causes the molecular chains to separate from each other, hindering the jumping between charge carrier chains, and reducing the conductivity by 0.93 S / cm. Retention rate: FeCl3·6H3O > Ammonium persulfate > Potassium persulfate > FeSO4·7H2O > H2O2. This indicates that the type of oxidant has a significant impact on performance. FeCl3 has the dual function of both oxidant and dopant, with mild and controllable oxidizing properties, which is beneficial for the uniform nucleation of polypyrrole on the silicon-carbon surface. FeSO4 has insufficient oxidizing power, and H2O2 has no doping function, so neither can form an effective coating layer. Example 1 is superior to Example 5 and significantly superior to Comparative Example 2. The high temperature of 40°C caused severe peroxidation of polypyrrole, which destroyed a large amount of the conjugated structure of the molecular chain. The coating layer structure was loose and the conductivity dropped significantly, resulting in the loss of effective volume expansion inhibition ability and a rebound rate as high as 104.6%.

[0074] The overall performance differences can be derived by combining all key indicators (cycle retention rate, rebound rate, conductivity): Example 1> Example 4> Example 3> Example 2> Example 5> Comparative Example 6> Example 6> Example 7> Comparative Example 1> Comparative Example 3> Comparative Example 7> Comparative Example 2> Comparative Example 4> Comparative Example 5.

[0075] In summary, this invention constructs a polypyrrole hydrogel conductive polymer layer in situ on the silicon-carbon surface through gradient control of temperature, time, and oxidant dosage. Combined with the synergistic enhancement of the SWCNT conductive network, it achieves the synergistic effect of "anchoring-buffering-conductivity," significantly suppressing the volume expansion of the silicon-carbon anode and greatly improving cycle stability. This provides a novel technical solution for the silicon-carbon anode interface engineering of next-generation high-energy-density lithium-ion batteries.

[0076] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a low-expansion silicon-carbon anode material, characterized in that, Includes the following steps: A silicon-carbon matrix is ​​surface modified to obtain a modified silicon-carbon matrix; the surface modification includes surface oxidation modification. A mixed dispersion is obtained by mixing single-walled carbon nanotubes with an acidic aqueous solution containing pyrrole monomer and a dopant; the dopant in the acidic aqueous solution is one or more of sodium benzenesulfonate, sodium p-toluenesulfonate, and sodium β-naphthalenesulfonate. The modified silicon-carbon matrix was placed in the mixed dispersion for staged in-situ polymerization to obtain a product slurry; The product slurry was spray-dried to obtain the low-expansion silicon-carbon anode material; The staged in-situ polymerization is carried out under the condition of adding an oxidant, and the staged in-situ polymerization includes a first stage in-situ polymerization, a second stage in-situ polymerization and a third stage in-situ polymerization carried out sequentially; the oxidant includes one or more of anhydrous ferric chloride, ferric chloride hexahydrate, ammonium persulfate and potassium persulfate; The temperature, time, and molar ratio of oxidant to pyrrole monomer all showed an increasing trend in the first-stage in-situ polymerization, the second-stage in-situ polymerization, and the third-stage in-situ polymerization.

2. The preparation method according to claim 1, characterized in that, The temperature of the first stage of in-situ polymerization is 0~5℃, the time is 0.3-1.0, and the molar ratio of oxidant to pyrrole monomer is (0.8~1.2):

1.

3. The preparation method according to claim 1, characterized in that, The second stage of in-situ polymerization is carried out at a temperature of 20~25℃ for 1.0~2.0h, and the molar ratio of oxidant to pyrrole monomer is (1.2~1.5):

1. The time required to raise the temperature from the first stage in-situ polymerization temperature to the second stage in-situ polymerization temperature is 0.5~1.0 h.

4. The preparation method according to claim 1, characterized in that, The third stage of in-situ polymerization is carried out at a temperature of 30~40℃ for 2.0~4.0h, and the molar ratio of oxidant to pyrrole monomer is (1.5~2.0):

1. The time required to raise the temperature from the second stage in-situ polymerization temperature to the third stage in-situ polymerization temperature is 0.8 hours, not exceeding 1 hour.

5. The preparation method according to claim 1, characterized in that, The surface oxidation modification method is a chemical oxidation method; The chemical oxidation process includes: Ammonia, hydrogen peroxide, and water are mixed to obtain a mixture; The silicon-carbon matrix is ​​placed in the mixture for surface hydrophilic modification to obtain the modified silicon-carbon matrix.

6. The preparation method according to claim 5, characterized in that, The volume ratio of ammonia, hydrogen peroxide, and water is 1:1:5; the mass percentage concentration of ammonia is 25%, and the mass percentage concentration of hydrogen peroxide is 30%. The ratio of silicon-carbon matrix to the mixture is 1g:(10~20)mL; The surface hydrophilization modification temperature is 95~100℃, and the time is 40~60min.

7. The preparation method according to claim 1, characterized in that, The inlet temperature of the spray dryer is 150~200℃, and the outlet temperature is 80~100℃.

8. The low-expansion silicon-carbon anode material prepared by the preparation method according to any one of claims 1 to 7, characterized in that, It includes a silicon-carbon matrix and a polypyrrole hydrogel conductive polymer layer coated on the surface of the silicon-carbon matrix; Single-walled carbon nanotubes are dispersed in the polypyrrole hydrogel conductive polymer layer.

9. The low-expansion silicon-carbon anode material as described in claim 8, characterized in that, The mass of the single-walled carbon nanotubes accounts for 0.02 to 0.06% of the mass of the silicon-carbon matrix.

10. A lithium-ion battery, comprising a negative electrode active material, characterized in that, The negative electrode active material is the low-expansion silicon-carbon negative electrode material as described in claim 8 or 9.